Method for preparing autoclaved sand-lime bricks from dry residues obtained after oil-based rock debris treatment
Through anaerobic thermal desorption and autoclave processes, the oil bedrock cuttings were processed to prepare high-strength and low-cost autoclave ash sand bricks, which solved the problems of oil bedrock cuttings and achieved efficient utilization of building materials.
Patent Information
- Application Number
- CN202411241973.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The amount of oil bedrock cuttings generated in the shale gas exploration and development process increases, and contains harmful substances that are difficult to naturally degrade. The existing treatment methods have not effectively improved their utilization rate and reduced costs.
After the oil bedrock chips are treated by anaerobic thermal desorption process, the ash slag is prepared through refrigeration, crushing, screening and stirring, and a specific proportion of stirring is combined with cement and water, and high-temperature and high-pressure treatment is carried out through an autoclave to form steaming. Pressed ash sand bricks.
The utilization rate of oil bedrock chips is improved, and the prepared autoclaved ash sand bricks reach the strength of the best product, while reducing production costs and meeting the performance indicators of national standards.
Smart Images

Figure CN118908667A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmental protection, and in particular to a method for preparing autoclaved lime sand bricks from dry residues after oil-based rock cuttings are processed. Background Art
[0002] Oil-based cuttings are a type of oil-containing solid waste produced when oil-based drilling fluid is used to open up oil and gas "channels". In the exploration and development of resources such as shale gas, due to the complex mineral composition of shale, in order to ensure the stability of the well wall and reduce well control risks, oil-based mud with a certain proportion of proppant must be used as drilling fluid. In this way, the amount of oil-based cuttings produced increases accordingly. Its main components include oil, water, drill cuttings, polymer compounds and other impurities, including a variety of harmful substances that are difficult to degrade in the natural environment.
[0003] Existing methods for processing oil-based rock cuttings include pyrolysis, solvent extraction technology, incineration technology, physicochemical separation technology, solidification technology, thermal desorption treatment technology and biodegradation. The oil-based rock cuttings after pyrolysis, physicochemical separation and thermal desorption treatment technology can be recycled. These treatment methods have laid the foundation for the environmentally friendly utilization of oil-based rock cuttings.
[0004] Autoclaved sand-lime brick is an ordinary sand-lime brick made of sand and lime as the main raw materials, which is prepared by blank preparation, pressed into shape, and cured by high-pressure steam. Autoclaved sand-lime brick is a new type of building material with mature technology, excellent performance and energy saving. It is suitable for load-bearing walls of multi-story mixed structure buildings. Summary of the invention
[0005] In view of the above technical problems, the present invention proposes the following technical solutions for utilizing oil-based rock cuttings in building materials: A method for preparing autoclaved lime sand bricks from dry residue after oil-based rock cuttings treatment, characterized by comprising the following steps: Step 1: Treat the oil-based rock cuttings with an anaerobic thermal desorption process to produce ash, which is cooled by a refrigeration auger, and then crushed by a two-stage crusher. The crushed ash is screened by a vibrating screen with a mesh size of 0.8 cm. The screened ash is one of the raw materials.
[0006] Step 2: Prepare auxiliary cement, the cement grade is PO42.5R.
[0007] Step 3, weigh the ash, cement and water using the meter in the meter; Step 4: Put ash and cement into a wheel mixer, let the wheel mixer mix the ingredients, and at the same time transport them to the water adder equipped with the wheel mixer through a water pump, and evenly spray them in the wheel mixer for mixing. The ingredient ratio is 81.3% for ash, 7.32% for cement, and 11.38% for water. The finished product after mixing is a water-containing colloid.
[0008] Step 5: The water-containing colloidal intermediate material after stirring is sent to a drum screening machine through a closed conveyor. When the drum screening machine screens the water-containing colloidal material, the colloidal material or hard stones larger than 5 mm in the material are screened out.
[0009] Step 6: The screened water-containing colloidal material is conveyed to a pulverizer by a closed belt for pulverization. The pulverizer has the functions of breaking up and pulverizing. The pulverizer controls the fineness of the water-containing colloidal material to within 4 mm. The pulverized material is conveyed to the next process by a closed belt.
[0010] Step 7: The crushed material is pressed into shape by a bidirectional simulated static press, and then the autoclaved brick body is taken out from the bidirectional simulated static press.
[0011] Step 8: Before entering the autoclave, the bricks pressed out of the brick machine are placed in a natural environment for one to two hours to reduce excess moisture in the autoclaved bricks.
[0012] Step 8. Use a double-opening autoclave, place the autoclaved brick body into the autoclave and seal it, then pass steam into it. After the steam is passed into the autoclave, the space inside the autoclave is under a pressure of 10 MPa, and the temperature inside the autoclave is maintained at 250 to 300 degrees. Under this state, autoclave and pressure are maintained for three hours, and then the autoclave is opened again. After the autoclaved brick body reaches a certain strength after high-temperature and high-pressure autoclaving in the autoclave, it becomes a finished autoclaved lime sand brick.
[0013] Step nine, take out the finished autoclave lime sand bricks in the autoclave and place them in the finished product yard in the natural environment.
[0014] Compared with the prior art, the present invention has the following advantages: (1) the present invention produces ash slag after treating oil-based rock cuttings by anaerobic thermal desorption process, and then uses the ash slag for making autoclaved lime sand bricks after treatment, which can greatly improve the utilization rate of oil-based rock cuttings; (2) the present invention uses a specific proportion of oil-based rock cuttings to make autoclaved lime sand bricks, which can not only make the autoclaved lime sand bricks reach the strength of superior products, but also further reduce the production cost of autoclaved lime sand bricks. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a schematic diagram of the process flow of the present invention. DETAILED DESCRIPTION
[0016] A method for preparing autoclaved lime sand bricks from dry residue after oil-based rock cuttings processing comprises the following steps: Step 1, oil-based rock cuttings processing: the oil-based rock cuttings produce ash after anaerobic thermal desorption treatment, and then the ash is specially treated so that the dry slag is suitable for raw materials for brick making. The specific process is that the ash after anaerobic thermal desorption treatment is first cooled by a refrigeration auger, and the cold auger cools the ash from about 320°C to about 50°C, and then the ash enters a double-stage hammer crusher, and the ash is crushed by the double-stage hammer crusher. The crushed ash is transported to an ash tank through a screw conveyor and an elevator. In the process of loading the dry slag from the ash tank into an ash tank transport vehicle, it is screened by a vibrating screen. The screen size of the vibrating screen is 0.8 cm. The purpose is to screen out materials such as iron blocks and debris that exceed 0.8 cm in the ash, and the ash that passes the vibrating screen and is less than 0.8 cm is loaded into an ash tank truck and transported to a brick factory, and then driven into the ash tank in the brick factory as the main raw material for autoclaved lime sand bricks.
[0017] Step 2: Raw material preparation: prepare cement, ash and water, where the cement grade is PO42.5R. The raw materials cement and ash are transported to the production workshop by special tank trucks. After connecting the tank trucks to the cement silo and ash silo through pipelines, they are transported to the cement silo and ash silo by air pumps for standby use.
[0018] Step 3: Batching and mixing: according to the ratio of cement 11.38% and ash 81.3%, the raw materials are measured in the metering device and then enter the batching machine. Then the batching machine puts the ash and cement into the wheel mixer, and the wheel mixer mixes the ingredients. At the same time, water is pumped into the water adder equipped with the wheel mixer through the water pump. The water adder will spray the water evenly in the wheel mixer for mixing. The batching ratio is 81.3% of ash, 7.32% of cement, and 11.38% of water. The finished product after mixing is a water-containing colloid. For example, the weight of the raw materials entering the batching machine at one time is: 1500 kg of ash and 135 kg of cement. Then, 210 kg of water is evenly fed into the mixer through the water adder. The uniform mixing in the mixer is completed after 360 seconds.
[0019] Step 4, screening: the water-containing colloidal intermediate material after stirring is sent to a drum screening machine through a closed conveyor. When the drum screening machine screens the water-containing colloidal material, the colloidal material or hard stones larger than 5 mm in the material are screened out.
[0020] Step 5, crushing: the screened water-containing colloidal material is conveyed to the crusher by a closed belt for crushing. The crusher has the functions of breaking up and crushing. The crusher can control the fineness of the material within 4mm. The crushed material is conveyed to the brick machine receiving hopper by a closed belt.
[0021] Step 6: Compression molding: The crushed materials are pressed into autoclaved brick bodies by a two-way simulated static press. The autoclaved brick bodies are stacked on a steaming trolley by an automatic stacker and enter the static curing area.
[0022] Step 7. Resting: The purpose of resting is to allow some of the excess water in the autoclaved bricks to evaporate, so as to prevent cracks in the autoclaved bricks caused by the thermal expansion of water during the subsequent heating process. Secondly, resting can increase the strength of the autoclaved bricks, thereby improving the strength of the product. Generally, the resting time for autoclaved bricks is 1-2 hours.
[0023] Step 8, autoclave curing: the autoclave is a double-opening type. The assembled autoclaved bricks enter the autoclave along the track and are sealed. Then steam is introduced into the autoclave. The autoclaved bricks are autoclaved at high temperature and high pressure in the autoclave before the furnace is opened for production. During this process, the steam in the autoclave should be kept at a pressure of 10 MPa and a temperature of 250-300 degrees Celsius. The autoclave is maintained for 3 hours and then maintained at pressure for another 3 hours. After the autoclaved bricks reach a certain strength, they become finished autoclaved fly ash bricks. The steam used in the specific autoclave process is provided by a natural gas boiler installed in the factory.
[0024] Step 9: Finished product stacking: The lime sand bricks are transported to the finished product yard by crane after leaving the furnace for inspection and sale.
[0025] The autoclaved fly-lime bricks produced by this method using oil-based rock cuttings have an average compressive strength of 26.9MPa, which fully meets the strength index of superior autoclaved fly-lime bricks (>25MPa). At the same time, the other indicators of autoclaved fly-lime bricks, such as radionuclide limit, frost resistance, water absorption rate, linear drying shrinkage rate and softening coefficient, also fully meet the national standard "Autoclaved fly-lime brick" (GB11945-1999).
Claims
1. A method for preparing autoclaved lime sand bricks from dry residue after oil-based rock cuttings treatment, characterized in that The following steps are involved: Step 1: treating the oil-based rock cuttings with an anaerobic thermal desorption process to produce ash residue; Step 2: Prepare auxiliary cement, the cement grade is PO42.5R; Step 3, weigh the ash, cement and water using the meter in the meter; Step 4: Put ash and cement into a wheel mixer, let the wheel mixer stir the ingredients, and at the same time, transport them to the water adder equipped with the wheel mixer through a water pump, and evenly spray them in the wheel mixer for stirring, wherein the ingredient ratio is 81.3% of ash, 7.32% of cement, and 11.38% of water, and the finished product after stirring is a water-containing colloid; Step 5: The water-containing colloidal intermediate material after stirring is sent to a drum screening machine through a closed conveyor to further screen the material; Step 6: The screened water-containing colloidal material is conveyed to the pulverizer by a closed belt for pulverization, and the pulverized material is conveyed to the next process by a closed belt; Step 7: The crushed material is pressed into shape by a bidirectional simulated static press, and then the autoclaved brick body is taken out from the bidirectional simulated static press; Step 8: Place the autoclaved brick body in a natural environment for one to two hours to reduce excess moisture in the autoclaved brick body; Step 8: Use a double-opening autoclave to place the autoclaved brick body into the autoclave, seal it, and then introduce steam. After the autoclaved brick body reaches a certain strength after being autoclaved at high temperature and high pressure in the autoclave, it becomes an autoclaved sand-lime brick product. Step 9: Take out the autoclaved sand-lime brick product from the autoclave and place it in a finished product yard in a natural environment.
2. The method for preparing autoclaved lime sand bricks from dry residue after oil-based rock cuttings treatment according to claim 1, characterized in that: In step one, the ash produced after the oil-based rock cuttings are treated by an anaerobic thermal desorption process is pretreated, the ash is cooled by a refrigeration auger, and then the cooled ash is crushed by a two-stage crusher. The crushed ash is screened by a vibrating screen with a mesh size of 0.8 cm. The screened ash is one of the raw materials.
3. The method for preparing autoclaved lime sand bricks from dry residue after oil-based rock cuttings treatment according to claim 1, characterized in that: When the drum screening machine in step 5 screens the water-containing colloid, the colloid or hard stones larger than 5 mm in the material are screened out.
4. The method for preparing autoclaved lime sand bricks from dry residue after oil-based rock cuttings treatment according to claim 1, characterized in that: The pulverizer in step six has the functions of breaking up and crushing, and the pulverizer controls the fineness of the water-containing colloidal material to within 4 mm.
5. The method for preparing autoclaved sand-lime bricks from dry residue after oil-based rock cuttings treatment according to claim 1, characterized in that: After steam is introduced into the autoclave in step eight, a pressure of ten MPa is created in the space inside the autoclave, and the temperature inside the autoclave is maintained at two hundred and fifty to three hundred degrees. In this state, the autoclave is autoclaved and pressure maintained for three hours, and then the autoclave is opened.
Citation Information
Patent Citations
Application of well drilling detritus in baking-free brick material
CN101085702A
Autoclaved sand-lime brick made from cured slag and preparation method of same
CN104761217A
Baking-free brick prepared by oil-based drill cutting residues
CN105967595A
Baking-free brick prepared from waste slurry and preparation method thereof
CN107840623A
Aggregate-free unfired building block brick and production method thereof
CN108046681A