A filling cement and a method for producing the same

By preparing filling cementitious materials, using phosphate rock flotation tailings, phosphogypsum, and alkali slag as the main raw materials, and combining water glass and acrylic ester copolymer emulsion as curing accelerators, the stability problem of solid wastes such as phosphogypsum was solved, realizing its effective application in road infrastructure materials and building materials, improving the strength and stability of the materials, and reducing environmental pollution.

CN118908684BActive Publication Date: 2026-11-20KUNMING UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411007503.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2026-11-20
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

In existing technologies, solid wastes such as phosphogypsum, phosphate rock flotation tailings, and alkali slag have long-term stability problems during resource utilization, leading to large-scale accumulation and environmental pollution. It is difficult to effectively solve the long-term stability problem of these materials as fillers for road infrastructure and building materials.

Method used

Using phosphate rock flotation tailings, phosphogypsum, and alkali residue as the main raw materials, combined with water glass and acrylic ester copolymer emulsion as curing accelerators, a filling cementitious material is prepared through mixing, molding, and curing to form substances such as hydrated sodium silicate, hydrated calcium aluminosilicate, and calcium phosphate compounds, thereby enhancing the strength and stability of the material.

Benefits of technology

It has achieved the stabilization and resource utilization of three types of solid waste, improved the mechanical strength, toughness and impact resistance of filling cementitious materials, solved the problem of solid waste accumulation, reduced environmental pollution, and improved the density and mechanical properties of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908684B_ABST
    Figure CN118908684B_ABST
Patent Text Reader

Abstract

The application discloses a kind of filling cementitious materials and preparation method thereof, belong to the technical field of resource utilization of solid waste.The cement, phosphorus tailing powder, flotation phosphogypsum and alkali residue are uniformly mixed to obtain dry mixture in the application;Then dry mixture, water and curing accelerator are uniformly mixed to obtain wet mixture;Finally, wet mixture is placed into prefabricated film, and compression molding, demolding and curing obtain filling cementitious material.Through the filling cementitious material after processing, PO4 3‑ The curing effect is remarkable, and F- and the measured heavy metals in the leaching solution are also within the range specified in the "Integrated Wastewater Discharge Standard" (GB8978-1996). The filling cementitious material has good mechanical properties and can be used as building materials and pavement infrastructure. It has the characteristics of simple process flow, energy saving and environmental protection, safety and reliability, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solid waste resource utilization technology, specifically relating to a filling cementitious material and its preparation method. Background Technology

[0002] Phosphogypsum is a byproduct of wet-process phosphoric acid production. Its main component is CaSO4·2H2O. Producing one ton of phosphoric acid generates approximately five tons of phosphogypsum. It is estimated that over 200 to 300 million tons of phosphogypsum are produced globally each year, with China producing over 60 million tons. Currently, the main method for disposing of phosphogypsum in China is stockpiling. The large-scale stockpiling of phosphogypsum not only occupies vast amounts of land but also pollutes groundwater, soil, and the atmosphere over long periods, damaging the surrounding ecosystem. The indiscriminate dumping of phosphogypsum hinders the sustainable development of the wet-process phosphoric acid and phosphate fertilizer industries. Therefore, promoting the reduction and resource utilization of phosphogypsum has become an urgent problem to be solved.

[0003] Phosphate rock flotation tailings are generated during the phosphate rock flotation process. They are mainly composed of dolomite (CaMg(CO3)2), fluorapatite (Ca5(PO4)3F), CaSO4·2H2O, SiO2, and other impurities. Typically, the weight percentage of P2O5 in phosphate rock flotation tailings is less than 10%, and the weight percentage of MgO is greater than 15%. Globally, only 7% of phosphate rock flotation tailings are recycled for use as building materials, agricultural fertilizers, ceramsite, and magnesium ferric sulfate. 93% of phosphate rock flotation tailings are directly discarded in tailings ponds without any treatment, occupying large amounts of farmland and causing serious ecological pollution.

[0004] Alkali residue is an alkaline waste residue discharged during the alkali production and treatment processes in industrial production. It includes waste residue discharged from the ammonium alkali process and other alkaline waste residues discharged from industrial production processes. The main components of alkali residue are calcium salts such as calcium carbonate, calcium sulfate, and calcium chloride, with small amounts of sulfur dioxide and other components. Alkali residue is a byproduct obtained from the refining and alkali washing of gasoline, diesel, and liquefied petroleum gas products from oil refineries. It mainly contains free alkali, sodium phenolate, sodium naphthenate, neutral oil, water, and various sulfides. The treatment of alkali residue has always been a bottleneck restricting the development of the soda ash industry both domestically and internationally. Most alkali plants have long adopted the method of mixed discharge, causing certain environmental pollution. The treatment of alkali residue generated by the soda ash industry is also urgently needed.

[0005] Significant progress has been made in the research on the resource utilization of the three types of solid waste both domestically and internationally. However, when these three types of solid waste are used as road infrastructure and building materials, the long-term stability of the filler material is a common problem, and the overall utilization rate of these three types of solid waste is not high, failing to fundamentally solve the problem of large-scale accumulation and storage of these three types of solid waste. Therefore, developing a solidification accelerator to simultaneously solidify and stabilize these three types of solid waste remains of great significance. Summary of the Invention

[0006] To address the shortcomings of the prior art, this invention provides a filling cementitious material and its preparation method.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing a filling cementitious material includes the following steps:

[0009] (1) The phosphate tailings are crushed and sieved to obtain phosphate tailings powder; then the phosphogypsum is flotated and dried to obtain flotation phosphogypsum.

[0010] (2) Mix cement, phosphorus tailings powder, flotation phosphogypsum and alkali residue to obtain dry mixture;

[0011] (3) Mix the dry mixture, water and curing accelerator to obtain a wet mixture;

[0012] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material.

[0013] In a preferred embodiment of the present invention, the flotation process is foam flotation.

[0014] In a preferred embodiment of the present invention, the curing accelerator comprises a water glass and an acrylate copolymer emulsion, wherein the mass ratio of the water glass and the acrylate copolymer emulsion is 6:5 to 12.

[0015] In a preferred embodiment of the present invention, the mass ratio of cement, phosphorus tailings powder, flotation phosphogypsum and alkali slag is (1-2):(2-3):(2-3):(1-2).

[0016] More preferably, the mass ratio of the cement, phosphate tailings powder, flotation phosphogypsum and alkali slag is 2:3:3:2. Under this ratio, the pH of the filling cementitious material is 7.0 to 9.0, at which point the mechanical properties and density are optimal.

[0017] In this invention, the proportions of phosphate rock flotation tailings and phosphogypsum added are made as close as possible, while the amount of alkaline residue added is reduced. This ensures that the density and mechanical properties of the filling cementitious material are maintained while minimizing the use of cement. The use of flotation-processed phosphogypsum in this invention reduces PO4 levels. 3- The leaching of the gel improves the unconfined compressive strength of the gel material.

[0018] In a preferred embodiment of the present invention, the mass ratio of the dry mix to water is 5:(1-3); the mass of the curing accelerator is 1% to 3% of the total mass of the dry mix and water.

[0019] More preferably, when the mass ratio of the dry mix to water is 5:2 and the mass of the curing accelerator is 2% of the total mass of the dry mix and water, the compressive and flexural strength of the filling cementitious material is optimal.

[0020] In a preferred embodiment of the present invention, the pressure of the molding die is 40-60 MPa and the time is 15-25 h.

[0021] In a preferred embodiment of the present invention, the curing temperature is 10-30℃, the time is 20-40 days, and the relative humidity is 80-90%.

[0022] More preferably, the compressive and flexural strength of the filling cementitious material is optimal when the curing temperature is 20°C, the curing time is 30 days, and the relative humidity is 85%.

[0023] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0024] (1) This invention utilizes the synergistic effect of phosphate rock flotation tailings, phosphogypsum, and alkaline residue, combined with a solidification accelerator to increase the doping content of these materials, thereby enhancing the mechanical strength, toughness, impact resistance, and water resistance of the filling cementitious material. Furthermore, the synergistic effect of water glass and acrylic copolymer emulsion increases the doping content of phosphate rock flotation tailings, phosphogypsum, and alkaline residue on one hand, and on the other hand, increases the PO4 content in phosphogypsum and phosphate rock flotation tailings. 3- and F - The curing process.

[0025] (2) This invention simultaneously solidifies and stabilizes three solid wastes: phosphate rock flotation tailings, phosphogypsum, and alkali slag, effectively solving the current problem of their accumulation. Simultaneously, the phosphate rock flotation tailings, phosphogypsum, and alkali slag interact in a water and cement medium to generate substances such as hydrated sodium silicate (CSH), hydrated calcium aluminosilicate (CASH), and calcium phosphate compounds, enhancing the strength, stability, density, and other mechanical properties of the filling cementitious material. Furthermore, the alkali-activated effect of phosphogypsum and phosphate tailings powder under the action of alkali slag promotes the dissolution of phosphogypsum and accelerates the reaction process. Unreacted phosphate tailings powder can also fill the pores of the solidified body, increasing its density. Water glass can regulate the crystal growth mode of the cement gel material, forming finer and more uniform crystals, improving the density and mechanical properties of the solidified body. Attached Figure Description

[0026] Figure 1 A flowchart illustrating the preparation process of filling cementitious materials. Detailed Implementation

[0027] To better illustrate the purpose, technical solution, and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0028] Example 1

[0029] A method for preparing a filling cementitious material includes the following steps:

[0030] (1) The phosphate tailings were crushed and passed through a 100-mesh sieve to obtain phosphate tailings powder; then the phosphogypsum was subjected to flotation treatment and dried to obtain flotation phosphogypsum.

[0031] (2) Mix cement, phosphorus tailings powder, flotation phosphogypsum and alkali residue in a mass ratio of 1:2:3:1 to obtain dry mixture.

[0032] (3) Mix the dry mixture with water at a mass ratio of 5:1 and the curing accelerator at a mass ratio of 1% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylate copolymer emulsion, and the mass ratio of water glass and acrylate copolymer emulsion is 6:10.

[0033] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material; the pressing pressure is 50MPa and the time is 20h; the curing temperature is 20℃ and the time is 30 days, and the relative humidity is 85%.

[0034] The obtained filling cementitious material was subjected to leaching tests to detect PO4. 3- It is 6.8 mg / L, F - Both the tested heavy metals and the measured heavy metals were within the range specified in GB8978-1996.

[0035] Unconfined compressive strength of filling cementitious materials: 7d: 6.5MPa; 28d: 8.3MPa; 90d: 12.8MPa.

[0036] Example 2

[0037] A method for preparing a filling cementitious material includes the following steps:

[0038] (1) The phosphate tailings were crushed and passed through a 100-mesh sieve to obtain phosphate tailings powder; then the phosphogypsum was subjected to flotation treatment and dried to obtain flotation phosphogypsum.

[0039] (2) Mix cement, phosphorus tailings powder, flotation phosphogypsum and alkali residue in a mass ratio of 2:3:3:1 to obtain dry mixture.

[0040] (3) Mix the dry mixture with water at a mass ratio of 5:3 and the curing accelerator at a mass ratio of 1% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylate copolymer emulsion, and the mass ratio of water glass and acrylate copolymer emulsion is 6:5.

[0041] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material; the pressing pressure is 40MPa and the time is 15h; the curing temperature is 10℃ and the time is 10 days, and the relative humidity is 90%.

[0042] The obtained filling cementitious material was subjected to leaching tests to detect PO4. 3- It is 7.2 mg / L, F - Both the tested heavy metals and the measured heavy metals were within the range specified in GB8978-1996.

[0043] Unconfined compressive strength of filling cementitious materials: 7d: 6.2MPa; 28d: 8.2MPa; 90d: 12.5MPa.

[0044] Example 3

[0045] A method for preparing a filling cementitious material includes the following steps:

[0046] (1) The phosphate tailings were crushed and passed through a 100-mesh sieve to obtain phosphate tailings powder; then the phosphogypsum was subjected to flotation treatment and dried to obtain flotation phosphogypsum.

[0047] (2) Mix cement, phosphorus tailings powder, flotation phosphogypsum and alkali residue in a mass ratio of 2:3:3:2 to obtain dry mixture.

[0048] (3) Mix the dry mixture with water at a mass ratio of 5:2 and the curing accelerator at a mass ratio of 2% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylate copolymer emulsion, and the mass ratio of water glass and acrylate copolymer emulsion is 6:12.

[0049] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material; the pressing pressure is 60MPa and the time is 25h; the curing temperature is 30℃ and the time is 40 days, and the relative humidity is 80%.

[0050] The obtained filling cementitious material was subjected to leaching tests to detect PO4. 3- It is 4.1 mg / L, F - Both the tested heavy metals and the measured heavy metals were within the range specified in GB8978-1996.

[0051] Unconfined compressive strength of filling cementitious materials: 7d: 6.9MPa; 28d: 9.1MPa; 90d: 13.9MPa.

[0052] Example 4

[0053] A method for preparing a filling cementitious material includes the following steps:

[0054] (1) The phosphate tailings were crushed and passed through a 100-mesh sieve to obtain phosphate tailings powder; then the phosphogypsum was subjected to flotation treatment and dried to obtain flotation phosphogypsum.

[0055] (2) Mix cement, phosphorus tailings powder, flotation phosphogypsum and alkali residue in a mass ratio of 2:3:2:2 to obtain dry mixture.

[0056] (3) Mix the dry mixture with water at a mass ratio of 5:3 and the curing accelerator at a mass ratio of 3% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylate copolymer emulsion, and the mass ratio of water glass and acrylate copolymer emulsion is 6:10.

[0057] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material; the pressing pressure is 40-60MPa and the time is 15h; the curing temperature is 10℃ and the time is 10 days, and the relative humidity is 90%.

[0058] The obtained filling cementitious material was subjected to leaching tests to detect PO4. 3- It is 4.9 mg / L, F - Both the tested heavy metals and the measured heavy metals were within the range specified in GB8978-1996.

[0059] Unconfined compressive strength of filling cementitious materials: 7d: 6.8MPa; 28d: 8.8MPa; 90d: 13.3MPa.

[0060] Example 5

[0061] A method for preparing a filling cementitious material includes the following steps:

[0062] (1) The phosphate tailings were crushed and passed through a 100-mesh sieve to obtain phosphate tailings powder; then the phosphogypsum was subjected to flotation treatment and dried to obtain flotation phosphogypsum.

[0063] (2) Mix cement, phosphorus tailings powder, flotation phosphogypsum and alkali residue in a mass ratio of 1:2:2:1 to obtain dry mixture.

[0064] (3) Mix the dry mixture with water at a mass ratio of 5:2 and the curing accelerator at a mass ratio of 2% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylate copolymer emulsion, and the mass ratio of water glass and acrylate copolymer emulsion is 6:10.

[0065] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material; the pressing pressure is 40-60MPa and the time is 15h; the curing temperature is 10℃ and the time is 10 days, and the relative humidity is 90%.

[0066] The obtained filling cementitious material was subjected to leaching tests to detect PO4. 3- It is 4.8 mg / L, F - Both the tested heavy metals and the measured heavy metals were within the range specified in GB8978-1996.

[0067] Unconfined compressive strength of filling cementitious materials: 7d: 6.6MPa; 28d: 9.0MPa; 90d: 13.2MPa.

[0068] Comparative Example 1

[0069] A method for preparing a filling cementitious material includes the following steps:

[0070] (1) The phosphate tailings were crushed and passed through a 100-mesh sieve to obtain phosphate tailings powder; then the phosphogypsum was subjected to flotation treatment and dried to obtain flotation phosphogypsum.

[0071] (2) Mix cement, phosphorus tailings powder, flotation phosphogypsum and alkali residue in a mass ratio of 1:2:3:1 to obtain dry mixture;

[0072] (3) Mix the dry mixture with water at a mass ratio of 5:1 to obtain the wet mixture;

[0073] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material; the pressing pressure is 50MPa and the time is 20h; the curing temperature is 20℃ and the time is 30 days, and the relative humidity is 85%.

[0074] The obtained filling cementitious material was subjected to leaching tests to detect PO4. 3- The concentration was 13.8 mg / L, and the measured heavy metal concentration was within the range specified in GB8978-1996. - It is not within the scope specified in GB8978-1996.

[0075] Unconfined compressive strength of filling cementitious materials: 7d: 5.2MPa; 28d: 7.1MPa; 90d: 10.3MPa.

[0076] Comparative Example 2

[0077] A method for preparing a filling cementitious material includes the following steps:

[0078] (1) The phosphate tailings were crushed and passed through a 100-mesh sieve to obtain phosphate tailings powder; then the phosphogypsum was subjected to flotation treatment and dried to obtain flotation phosphogypsum.

[0079] (2) Mix cement, phosphorus tailings powder, flotation phosphogypsum and alkali residue in a mass ratio of 1:2:3:1 to obtain dry mixture.

[0080] (3) Mix the dry mixture with water at a mass ratio of 5:3, and the acrylic copolymer emulsion at a mass of 1% of the total mass of the dry mixture and water to obtain a wet mixture.

[0081] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material; the pressing pressure is 50MPa and the time is 20h; the curing temperature is 20℃ and the time is 30 days, and the relative humidity is 85%.

[0082] The obtained filling cementitious material was subjected to leaching tests to detect PO4. 3- The concentration was 12.5 mg / L, and all tested heavy metals were within the range specified in GB8978-1996. - It is not within the scope specified in GB8978-1996.

[0083] Unconfined compressive strength of filling cementitious materials: 7d: 5.6MPa; 28d: 7.5MPa; 90d: 11.2MPa.

[0084] Comparative Example 3

[0085] A method for preparing a filling cementitious material includes the following steps:

[0086] (1) The phosphate tailings were crushed and passed through a 100-mesh sieve to obtain phosphate tailings powder; then the phosphogypsum was subjected to flotation treatment and dried to obtain flotation phosphogypsum.

[0087] (2) Mix cement, phosphorus tailings powder, flotation phosphogypsum and alkali residue in a mass ratio of 1:2:3:1 to obtain dry mixture.

[0088] (3) Mix the dry mixture with water at a mass ratio of 5:3 and add water glass at a mass of 1% of the total mass of the dry mixture and water to obtain a wet mixture.

[0089] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material; the pressing pressure is 50MPa and the time is 20h; the curing temperature is 20℃ and the time is 30 days, and the relative humidity is 85%.

[0090] The obtained filling cementitious material was subjected to leaching tests to detect PO4. 3- The concentration was 9.3 mg / L, and both F- and the measured heavy metals were within the range specified in GB8978-1996.

[0091] Unconfined compressive strength of filling cementitious materials: 7d: 6.1MPa; 28d: 7.6MPa; 90d: 11.6MPa.

[0092] Comparative Examples 1-3 show that the synergistic effect of water glass and acrylate copolymer emulsion can increase the dosage of flotation phosphogypsum, phosphate tailings powder, and alkaline residue, and can effectively fix PO4 in phosphate tailings powder and phosphogypsum. 3- And F-. A lack of water glass will reduce the hydrolysis and hydration efficiency of the curing components and delay PO4. 3- The curing process of F- increases its leaching risk. The lack of acrylate copolymer emulsion affects the adhesive strength of the components in this filling gel material, reducing overall mechanical properties. Acrylate copolymer emulsion can also form a hydrophobic film on the surface and inside the cured body, improving its water resistance.

[0093] Comparative Example 4

[0094] A method for preparing a filling cementitious material includes the following steps:

[0095] (1) The phosphate tailings were crushed and passed through a 100-mesh sieve to obtain phosphate tailings powder; then the phosphogypsum was subjected to flotation treatment and dried to obtain flotation phosphogypsum.

[0096] (2) Mix cement, phosphorus tailings powder and flotation phosphogypsum in a mass ratio of 1:2:3 to obtain dry mixture.

[0097] (3) Mix the dry mixture with water at a mass ratio of 5:1 and the curing accelerator at a mass ratio of 1% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylate copolymer emulsion, and the mass ratio of water glass and acrylate copolymer emulsion is 6:10.

[0098] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material; the pressing pressure is 50MPa and the time is 20h; the curing temperature is 20℃ and the time is 30 days, and the relative humidity is 85%.

[0099] The obtained filling cementitious material was subjected to leaching tests to detect PO4. 3- The concentration was 9.9 mg / L, and both F- and the measured heavy metals were within the range specified in GB8978-1996.

[0100] Unconfined compressive strength of filling cementitious materials: 7d: 5.7MPa; 28d: 7.8MPa; 90d: 11.9MPa.

[0101] Comparative Example 5

[0102] A method for preparing a filling cementitious material includes the following steps:

[0103] (1) Flotation phosphogypsum is obtained by flotation treatment and drying.

[0104] (2) Mix cement, flotation phosphogypsum and alkali residue in a mass ratio of 1:3:1 to obtain dry mixture.

[0105] (3) Mix the dry mixture with water at a mass ratio of 5:1 and the curing accelerator at a mass ratio of 1% of the total mass of the dry mixture and water to obtain a wet mixture; the curing accelerator includes water glass and acrylate copolymer emulsion, and the mass ratio of water glass and acrylate copolymer emulsion is 6:10.

[0106] (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material; the pressing pressure is 50MPa and the time is 20h; the curing temperature is 20℃ and the time is 30 days, and the relative humidity is 85%.

[0107] The obtained filling cementitious material was subjected to leaching tests to detect PO4. 3- The concentration was 10.2 mg / L, and both F- and the measured heavy metals were within the range specified in GB8978-1996.

[0108] Unconfined compressive strength of filling cementitious materials: 7d: 6.1MPa; 28d: 7.7MPa; 90d: 11.8MPa.

[0109] As can be seen from the comparison between Example 1 and Comparative Examples 4-5, the absence of alkaline residue or phosphorus tailings powder results in PO4... 3- and F - The curing effect and the mechanical strength of the filling gel material will both decrease. Mixing alkaline slag with cement and water will generate hydrated calcium aluminosilicate (CASH), which improves the mechanical properties of the filling gel material. The phosphate components in phosphate tailings can also react with calcium to generate various calcium phosphate compounds with certain cementing properties, such as hydroxyapatite, further improving the strength and stability of the solidified body. Furthermore, the alkaline slag provides an alkaline environment to the curing system; phosphogypsum and phosphate tailings powder can generate an alkaline activation effect in this environment, thereby promoting the dissolution of phosphogypsum and accelerating the reaction process.

[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the essence and scope of the technical solutions of the present invention.

Claims

1. A method for preparing a filling cementitious material, characterized in that, Includes the following steps: (1) The phosphate tailings are crushed and sieved to obtain phosphate tailings powder; then the phosphogypsum is subjected to flotation treatment and dried to obtain flotation phosphogypsum. (2) Mix cement, phosphorus tailings powder, flotation phosphogypsum and alkali residue in a mass ratio of (1~2):(2~3):(2~3):(1~2) to obtain dry mixture; (3) Mix the dry mixture, water and curing accelerator to obtain a wet mixture; wherein the curing accelerator includes water glass and acrylate copolymer emulsion, and the mass ratio of water glass and acrylate copolymer emulsion is 6:5~12; the mass ratio of the dry mixture and water is 5:(1-3); the mass of the curing accelerator is 1%~3% of the total mass of the dry mixture and water; (4) Place the wet mixture into the precast mold, press, demold, and cure to obtain the filling cementitious material.

2. The method for preparing the filling cementitious material as described in claim 1, characterized in that, The flotation process is foam flotation.

3. The method for preparing the filling cementitious material as described in claim 1, characterized in that, The mass ratio of cement, phosphorus tailings powder, flotation phosphogypsum, and alkali residue is 2:3:3:

2.

4. The method for preparing the filling cementitious material as described in claim 1, characterized in that, The pressure of the mold is 40-60 MPa, and the time is 15-25 h.

5. The method for preparing the filling cementitious material as described in claim 1, characterized in that, The curing temperature is 10-30℃, the time is 20-40 days, and the relative humidity is 80-90%.

6. The method for preparing the filling cementitious material as described in claim 5, characterized in that, The curing temperature is 20℃, the time is 30 days, and the relative humidity is 85%.

7. The filling cementitious material prepared by the method of any one of claims 1-6.

Citation Information

Patent Citations

  • Construction method for preventing loess embankment settlement by using phosphogypsum

    AU2020100913A4

  • Method for preparing mine filler by cementing solid wastes in iron and steel industry with heavy metal tailings

    CN112279565A