Spherical yttrium aluminum garnet powder and method for in-situ synthesis of spherical yttrium aluminum garnet powder by spray granulation technique
By employing spray granulation technology and low-temperature calcination, the problems of high cost and high energy consumption in the preparation of spherical YAG powder have been solved, and the efficient synthesis of pure phase YAG powder at low temperatures has been achieved, making it suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202410971271.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Existing methods for preparing spherical YAG powders are costly, energy-intensive, and require excessively high synthesis temperatures, limiting their application in large-scale production. Furthermore, traditional solid-state reaction methods cause the powders to lose their sintering activity.
By employing spray granulation technology, yttrium oxide and alumina powders are mixed with dispersants and binders through mechanical stirring, spray-dried into spherical powders, and then calcined at low temperature to achieve in-situ synthesis of spherical yttrium aluminum garnet powders.
It reduces production costs, improves production efficiency, and enables the synthesis of pure-phase YAG at low temperatures, making it suitable for large-scale industrial production.
Smart Images

Figure CN118908712B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for in-situ synthesis of spherical yttrium aluminum garnet (YAG) powder at low temperature using spray granulation technology, and the synthesized spherical yttrium aluminum garnet powder, which is suitable for plasma spraying and ceramic pressing. Background Technology
[0002] With the rapid development of science and technology, the demand for high-performance ceramics is increasing. Yttrium aluminum garnet (YAG), as an important inorganic non-metallic material, is widely used in ceramics, coatings, electronics, and medical fields due to its excellent optical, thermal, and mechanical properties. In recent years, with the increasing demands for material performance, spherical YAG powder has attracted widespread attention due to its unique physical and chemical properties: Its unique spherical structure results in a relatively narrow particle size distribution, ensuring the uniformity of powder particles during the molding process. This high uniformity can greatly improve the precision and quality of material preparation, allowing the material's physical and chemical properties to be optimally utilized. Furthermore, the regular particle shape of spherical YAG powder prevents particle cross-linking and accumulation, resulting in excellent flowability and making the production process more efficient. Simultaneously, the spherical structure can better fill the voids in the molding die, thereby improving the ceramic density. Finally, due to its compact structure, spherical YAG has high plasticity, making it easier to prepare materials of various complex shapes, and possesses higher physical and chemical properties, such as hardness and etching resistance. Therefore, the preparation technology of spherical YAG powder is of great significance for improving the technological level and market competitiveness of related industries.
[0003] The preparation methods for spherical YAG powder typically include liquid-phase and solid-phase methods. Liquid-phase methods usually require large amounts of solvent and precipitant, and the yield is low, increasing production costs and limiting its application in large-scale production. Traditional solid-phase reaction methods, due to excessively high synthesis temperatures and long processing times, often cause the powder to lose its sintering activity. Solid-phase reaction methods involving Y2O3 powder and Al2O3 powder typically require temperatures above 1400℃ to effectively synthesize the YAG phase, while the pure phase requires even higher calcination temperatures, typically 1600℃.
[0004] Chinese patent CN 111925202B discloses a yttrium aluminum garnet (YAG) powder and ceramics without sintering aids, as well as their preparation method and applications. This method involves sphericalizing coarse YAG powder in a fluidized bed to obtain spherical YAG powder with an average particle size of 10 μm to 300 μm. However, fluidized bed granulation results in relatively large particle sizes, and requires adjustment of multiple parameters during operation, leading to high energy consumption and high cost. Summary of the Invention
[0005] To solve or partially solve the above-mentioned technical problems, the present invention provides a method for in-situ synthesis of spherical yttrium aluminum garnet powder using spray granulation technology, comprising the following steps:
[0006] S1. Yttrium oxide (Y2O3) powder, aluminum oxide (Al2O3) powder, deionized water, dispersant, and binder are mechanically stirred to obtain a mixed slurry;
[0007] S2. Spray granulation of the mixed slurry to obtain spherical mixed powder;
[0008] S3. Place the above spherical mixed powder in a muffle furnace and calcine it under no-pressure air atmosphere.
[0009] Optionally, the preparation of the mixed slurry includes the following steps:
[0010] S11, according to Y3Al5O 12 According to the stoichiometric ratio, yttrium oxide (Y2O3) powder, aluminum oxide (Al2O3) powder and deionized water were mechanically mixed by stirring.
[0011] S12. After stirring for a period of time, add the dispersant and continue stirring.
[0012] S13. Add a binder before granulation to obtain a mixed slurry.
[0013] Optionally, in step S11, the solid content of the mixed slurry is 30–60 wt.%.
[0014] Optionally, in step S12, the dispersant is selected from one of ammonium citrate, sodium hexametaphosphate, polyvinyl butyral, and polyvinylpyrrolidone, and the amount added is 0.1 to 2 wt.% of the powder mass;
[0015] The binder is selected from polyvinyl alcohol and polyvinyl butyral, and the amount added is 0.1 to 1 wt.% of the powder mass.
[0016] Optionally, in step S2, the mixed slurry is granulated by a spray dryer, the inlet temperature of which is 150-300℃ and the outlet temperature is 50-200℃; the atomizer speed of the spray dryer is 30-50Hz.
[0017] Optionally, in step S2, the particle size of the spherical mixed powder obtained by granulation is 10–100 μm.
[0018] Optionally, in step S2, the standard deviation of the sphericity of the spherical mixed powder obtained by granulation is 0 to 0.3.
[0019] Optionally, in step S2, the flowability index of the spherical mixed powder obtained by granulation is 70-90.
[0020] Optionally, in step S3, the calcination conditions are: heating rate of 1-10℃ / min; calcination temperature range of 1000-1600℃; and high-temperature holding time of 2-10h.
[0021] The present invention also provides a spherical yttrium aluminum garnet (YAG) powder, optionally synthesized by any of the methods described above.
[0022] This invention uses micron-sized Y2O3 powder as raw material. The refined Y2O3 powder is mixed with Al2O3 powder in the manner of Y3Al5O 12 The stoichiometric ratio of Y to Al is used to prepare a mixed slurry by adding dispersant and binder. The resulting slurry is pumped into the spray dryer by peristaltic pump to contact with hot air to achieve spray granulation. The closer the molar ratio of Y to Al is to the stoichiometric ratio of 0.60 by EDS scanning, the better the dispersion uniformity and the lower the cost.
[0023] Specifically, this method employs an Al2O3 / Y2O3 mixed slurry system, including a dispersant and a binder, and uses spray drying to prepare composite granular particles in situ. Guided by the stability of the slurry, the amount of dispersant added is adjusted to change the bonding state of Al2O3 and Y2O3, improving mixing uniformity and lowering the synthesis temperature of the YAG single phase. When the SHMP content is 1 wt.%, the mixed slurry with a solid content of 45 wt.% exhibits the best stability after 24 hours of sedimentation. Under these conditions, the spray-dried particles are monodisperse, dense, and uniformly spherical, which are then calcined at 1100℃ in air to obtain YAG single-phase particles. This method is simple, low in cost and energy consumption, high in yield, and environmentally friendly, making it suitable for large-scale industrial production. Attached Figure Description
[0024] Figure 1 The image shows a scanning electron microscope image and particle size distribution of the mixed spherical powder obtained in Example 1.
[0025] Figure 2 The image shows a scanning electron microscope image and particle size distribution of the mixed spherical powder obtained in Example 2.
[0026] Figure 3 The image shows a scanning electron microscope image and particle size distribution of the mixed spherical powder obtained in Example 3.
[0027] Figure 4 The image shows a scanning electron microscope image and particle size distribution of the mixed spherical powder obtained in Example 4.
[0028] Figure 5 The image shows a scanning electron microscope (SEM) image and particle size distribution of the mixed spherical powder obtained in Example 5.
[0029] Figure 6 The image shows a scanning electron microscope (SEM) image and particle size distribution of the mixed spherical powder obtained in Comparative Example 1.
[0030] Figure 7 The images show the XRD patterns of the mixed spherical powder obtained in Example 3 after calcination at different temperatures. Detailed Implementation
[0031] The technical solution of the present invention will be further described in detail below with reference to specific embodiments. It should be understood that the following embodiments are merely illustrative and explanatory of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are covered within the scope of protection intended by the present invention.
[0032] To address the technical problems of existing technologies, the present invention provides a method for in-situ low-temperature synthesis of spherical YAG powder using spray granulation technology, which can be carried out according to the following steps:
[0033] The fine powder of Y2O3, powder of Al2O3, deionized water, dispersant and binder are mechanically stirred to obtain a mixed slurry;
[0034] Y2O3 fine powder according to Y3Al5O 12 The stoichiometric ratio of the mixture is used to mechanically stir Al2O3 powder and deionized water. After stirring for a certain period of time, a dispersant is added, and a binder is added before granulation to obtain a mixed slurry.
[0035] The solid content of the mixed slurry can be 30–60 wt.%.
[0036] The dispersant can be selected from one of ammonium citrate, sodium hexametaphosphate, polyvinyl butyral, and polyvinylpyrrolidone, and the addition amount is 0.1 to 2 wt.% of the powder mass;
[0037] The binder can be selected from polyvinyl alcohol and polyvinyl butyral, and the amount added is 0.1 to 1 wt.% of the powder mass.
[0038] The above-mentioned mixed slurry was spray-granulated to obtain spherical mixed powder.
[0039] Spray granulation can be carried out using a spray dryer, with the inlet temperature set to 150–300℃ and the outlet temperature set to 50–200℃; the atomizer speed can be set to 30–50Hz.
[0040] D of the spherical mixed powder obtained by granulation 10 It can be 10–30 μm;
[0041] D of the spherical mixed powder obtained by granulation 50 It can be 10–100 μm;
[0042] D of the spherical mixed powder obtained by granulation 90 It can be 50–200 μm;
[0043] The flowability index of the spherical mixed powder obtained by granulation is calculated using the Carr index method according to Chinese National Standard 31057.3-2018. It is a weighted sum of the indices of angle of repose, compressibility, angle of plate, and uniformity, and the value can be 70 to 90.
[0044] The angle of repose of the spherical mixed powder obtained by granulation is an acute angle between the powder accumulation slope and the bottom horizontal plane under static equilibrium conditions, which can be 20 to 40°.
[0045] The compressibility of the spherical mixed powder obtained by granulation is the ratio of the difference between the tapped density and the loose density to the tapped density, and the ratio can be 10% to 30%.
[0046] The plate angle of the spherical mixed powder obtained by granulation is the angle θ between the free surface (inclined surface) of the powder on the plate and the horizontal plane when the plate is lifted vertically upward from the naturally packed powder. S1 The angle θ after being subjected to a certain impact S2 The average value can be between 30° and 50°.
[0047] The uniformity of the spherical mixed powder obtained by granulation is D 60 With D 10 The ratio can be 1 to 10.
[0048] The above-mentioned spherical mixed granulated powder was placed in a muffle furnace and calcined without pressure in an air atmosphere.
[0049] The air calcination conditions can be a heating rate of 1–10 °C / min;
[0050] The calcination temperature range can be 1000–1600℃;
[0051] The high-temperature insulation time can be 2 to 10 hours.
[0052] Compared with the prior art, the advantages of the present invention include:
[0053] The provided Y2O3 micron powder can replace expensive Y2O3 fine powder, resulting in lower production costs;
[0054] The provided spray granulation method ensures uniform dispersion of the two powders, and is simple to operate with high production efficiency;
[0055] The provided in-situ synthesis of spherical YAG has a calcination temperature that is 300℃~500℃ lower than the synthesis temperature of pure phase YAG by the traditional solid-phase reaction method.
[0056] Next, using several specific parameters as examples, the specific implementation process of the present invention will be exemplified, and comparative examples will be given below:
[0057] Example 1
[0058] (1) According to Y3Al5O 12 According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed respectively to prepare a slurry with a solid content of 60wt.%. Based on the total amount of all raw materials, 0.1wt.% of dispersant sodium hexametaphosphate, 1wt.% of binder polyvinyl alcohol, and deionized water were added and mechanically mixed to obtain the precursor slurry for spray granulation.
[0059] (2) The slurry obtained in step (1) is spray-granulated at an inlet temperature of 260℃, an outlet temperature of 110℃, and an atomizer speed of 46Hz to obtain 266g of spherical mixed powder with a median particle size of 91.74μm (e.g. Figure 1 As shown), the powder has an angle of repose of 37°, a flatness angle of 45°, a compressibility of 23.8%, a uniformity of 2.12, a flowability index of 74.5, and a Y to Al ratio of 0.44.
[0060] (3) The spherical mixed powder obtained in step (2) was calcined in air at 1400℃ for 4 hours to obtain pure YAG phase and spherical YAG powder was synthesized in situ.
[0061] Example 2
[0062] (1) According to Y3Al5O 12 According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed to prepare a slurry with a solid content of 30wt.%. Based on the total amount of all raw materials, 2wt.% of dispersant sodium hexametaphosphate, 0.1wt.% of binder polyvinyl alcohol, and deionized water were added and mechanically mixed to obtain a precursor slurry for spray granulation. Other processes were the same as in Example 1, resulting in spherical mixed powder 273 with a median particle size of 19.97μm (e.g., ...). Figure 2 As shown), the powder has an angle of repose of 36°, an angle of flatness of 47°, a compressibility of 19.7%, a uniformity of 1.85, a flowability index of 78, and a Y to Al ratio of 0.48.
[0063] (2) The spherical mixed powder obtained in step (1) was calcined in air at 1300℃ for 4 hours to obtain pure YAG phase, and spherical YAG powder was synthesized in situ.
[0064] Example 3
[0065] (1) According to Y3Al5O 12According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed to prepare a slurry with a solid content of 45wt.%. Based on the total amount of all raw materials, 1wt.% of dispersant sodium hexametaphosphate, 0.5wt.% of binder polyvinyl alcohol, and deionized water were added and mechanically mixed to obtain a precursor slurry for spray granulation. Other processes were the same as in Example 1, resulting in 285g of spherical mixed powder with a median particle size of 38.57μm (e.g. Figure 3 As shown), the powder has an angle of repose of 30°, an angle of flatness of 43°, a compressibility of 15.9%, a uniformity of 2.16, a flowability index of 83, and a Y to Al ratio of 0.61.
[0066] (2) The spherical mixed powder obtained in step (1) was calcined in air at 1100℃ for 4 hours to obtain pure YAG phase and spherical YAG powder was synthesized in situ.
[0067] Example 4
[0068] (1) According to Y3Al5O 12 According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed to prepare a slurry with a solid content of 45wt.%. Based on the total amount of all raw materials, 1wt.% of the dispersant polyvinyl butyral, 0.5wt.% of the binder polyvinyl alcohol, and deionized water were added and mechanically mixed to obtain a precursor slurry for spray granulation. Other processes were the same as in Example 1, resulting in 261g of spherical mixed powder with a median particle size of 40.73μm (e.g., ...). Figure 4 As shown), the powder has an angle of repose of 31°, a flatness angle of 44°, a compressibility of 17%, a uniformity of 2.06, a flowability index of 81, and a Y to Al ratio of 0.67.
[0069] (2) The spherical mixed powder obtained in step (1) was calcined in air at 1400℃ for 4 hours to obtain pure YAG phase, and spherical YAG powder was synthesized in situ.
[0070] Example 5
[0071] (1) According to Y3Al5O 12 According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed to prepare a slurry with a solid content of 45wt.%. Based on the total amount of all raw materials, 1wt.% of ammonium citrate dispersant, 0.5wt.% of polyvinyl alcohol binder, and deionized water were added and mechanically mixed to obtain a precursor slurry for spray granulation. Other processes were the same as in Example 1, resulting in 292g of spherical mixed powder with a median particle size of 37.86μm (e.g. Figure 5As shown), the powder has an angle of repose of 30°, a flatness angle of 46°, a compressibility of 16.3%, a uniformity of 2.21, a flowability index of 82, and a Y to Al ratio of 0.52.
[0072] (2) The spherical mixed powder obtained in step (1) was calcined in air at 1500℃ for 4 hours to obtain pure YAG phase, and spherical YAG powder was synthesized in situ.
[0073] Comparative Example 1
[0074] (1) According to Y3Al5O 12 According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed separately to prepare a slurry with a solid content of 45wt.%. Based on the total amount of all raw materials, without adding dispersant, 0.5wt.% of the binder polyvinyl alcohol and deionized water were added and mechanically mixed to obtain the precursor slurry for spray granulation. Other processes were the same as in Example 1, yielding 274g of spherical mixed powder with a median particle size of 42.74μm (e.g. Figure 6 As shown), the powder has an angle of repose of 32°, a flatness angle of 47°, a compressibility of 17.2%, a uniformity of 2.18, a flowability index of 78, and a Y to Al ratio of 0.28.
[0075] (2) The spherical mixed powder obtained in step (1) was calcined in air at 1600℃ for 4 hours to obtain pure YAG phase, and spherical YAG powder was synthesized in situ.
[0076] Comparative Example 2
[0077] (1) According to Y3Al5O 12 According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed respectively to prepare a slurry with a solid content of 45wt.%. Based on the total amount of all raw materials, 1wt.% of dispersant sodium hexametaphosphate was added and mechanically mixed with deionized water to obtain the precursor slurry.
[0078] (2) The slurry obtained in step (1) is dried in an 80°C oven and passed through a 60-mesh sieve to obtain a mixed powder (e.g. Figure 7 As shown), the powder has an angle of repose of 50°, an angle of flatness of 55°, a compressibility of 41.6%, a uniformity of 1.87, a flowability index of 52.5, and a Y to Al ratio of 0.23.
[0079] (3) The mixed powder obtained in step (2) was calcined in air at 1600℃ for 4 hours to obtain pure YAG phase.
[0080] Comparative Example 3
[0081] (1) According to Y3Al5O 12According to the stoichiometric ratio, 150g of Al2O3 and 200g of refined Y2O3 were weighed respectively to prepare a slurry with a solid content of 45wt.%.
[0082] (2) The slurry obtained in step (1) is dried in an 80°C oven and passed through a 60-mesh sieve to obtain a mixed powder (e.g. Figure 7 As shown), the powder has an angle of repose of 65°, an angle of flatness of 66°, a compressibility of 41.3%, a uniformity of 1.62, a flowability index of 42, and a Y to Al ratio of 0.11.
[0083] (3) The mixed powder obtained in step (2) was calcined in air at 1600℃ for 4 hours to obtain pure YAG phase.
[0084] Table 1
[0085]
[0086]
[0087] Table 2
[0088]
[0089] The Y₂O₃ / Al₂O₃ composite spherical powder prepared by spray granulation has a uniform particle size distribution. The particle size can be controlled by changing the solid content and slurry viscosity, exhibiting high sphericity and high flowability. The addition of a dispersant can adjust the bonding state of Al₂O₃ and Y₂O₃, improving their mixing uniformity. During the high-temperature reaction of Al₂O₃ and Y₂O₃ powders to form the YAG phase, the increased uniformity of the two powders enhances the contact area between the components, facilitating effective contact between reactants and promoting diffusion and migration between Al₂O₃ and Y₂O₃. This promotes the reaction and lowers the synthesis temperature of the YAG phase. When SHMP is used as a dispersant, the molar ratio of Y to Al in the granulated powder is 0.61, closest to the theoretical value, allowing for the synthesis of the YAG single phase at a minimum temperature of 1100℃, which is 300–500℃ lower than the traditional YAG single-phase synthesis temperature. Furthermore, spray granulation offers high production efficiency, enabling large-scale production to meet industrial needs.
Claims
1. A method for in-situ synthesis of spherical yttrium aluminum garnet powder via spray granulation technology, characterized in that, Includes the following steps: S11, according to Y3Al5O 12 According to the stoichiometric ratio, yttrium oxide (Y₂O₃) powder, aluminum oxide (Al₂O₃) powder and deionized water were mechanically mixed by stirring. S12. After stirring for a period of time, add the dispersant and continue stirring. The dispersant is sodium hexametaphosphate, and the amount of dispersant added is 1 wt.% of the powder mass. S13. A binder is added before granulation to obtain a mixed slurry, wherein the solid content of the mixed slurry is 45 wt.%. S2. Spray granulation of the mixed slurry to obtain spherical mixed powder; S3. The above-mentioned spherical mixed powder is placed in a muffle furnace and calcined without pressure in an air atmosphere at a calcination temperature of 1100°C.
2. The method according to claim 1, characterized in that, The binder is selected from polyvinyl alcohol and polyvinyl butyral, and the amount added is 0.1~1 wt.% of the powder mass.
3. The method according to claim 1, characterized in that, In step S2, the mixed slurry is granulated by a spray dryer. The inlet temperature of the spray dryer is 150~300 ℃ and the outlet temperature is 50~200 ℃. The atomizer speed of the spray dryer is 30~50 Hz.
4. The method according to claim 1, characterized in that, In step S2, the particle size of the spherical mixed powder obtained by granulation is 10~100 μm.
5. The method according to claim 1, characterized in that, In step S2, the standard deviation of the sphericity of the spherical mixed powder obtained by granulation is 0~0.
3.
6. The method according to claim 1, characterized in that, In step S2, the flowability index of the spherical mixed powder obtained by granulation is 70~90.
7. The method according to claim 1, characterized in that, In step S3, the calcination process is carried out under the following conditions: the heating rate is 1~10 ℃ / min; the high-temperature holding time is 2~10 h.
8. A spherical yttrium aluminum garnet (YAG) powder, characterized in that, The method described in any one of claims 1-7 is used for synthesis.
Citation Information
Patent Citations
A yttrium aluminum garnet powder without sintering aids, yttrium aluminum garnet ceramics, their preparation method and applications
CN111925202B
Method for preparing special-shaped YAG transparent ceramic through laser additive manufacturing technology
CN116675535A