PET (Polyethylene Terephthalate) foam board of chemical fiber recycled particles as well as preparation method and application of PET foam board
By adjusting the additive ratio in chemical fiber particles and adding chain extenders, combined with specific extrusion process and temperature settings, the problems of low melting point and low viscosity in the PET foaming reaction of chemical fiber recovery particles are solved, and the PET foaming plate is improved The mechanical properties meet the requirements of wind power blade core materials.
Patent Information
- Application Number
- CN202411242131.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-08
AI Technical Summary
In the PET foaming reaction, chemical fiber recovery particles have low melting point and low in nature viscosity, resulting in low extruder pressure and reduced polymerization reaction efficiency. The PET foamed plates produced do not meet the requirements of wind power blade core materials.
By adjusting the additive ratio in chemical fiber particles, adding chain extenders and crosslinkers, the molecular chain length and binding strength are improved, the reaction smoothness is improved, and the resistance of PET foamed plates is optimized through specific extrusion processes and temperature settings. The compressive strength, shear strength and tensile strength meet the requirements of wind power blade core materials.
The compressive strength of the PET foamed plate is achieved at 6.73-7.12MPa, the shear strength reaches 2.66-3.01 MPa, and the tensile strength reaches 290.2-301.7MPa, which meets the performance requirements of wind power blade core materials and improves the comprehensiveness of the foamed plate. performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the field of PET foam materials, and in particular to a PET foam board of recycled chemical fiber particles and a preparation method and application thereof. Background Art
[0002] As a renewable energy, wind power generation is a new energy source that is different from traditional energy sources. Compared with other new energy sources such as solar power generation, wind power generation has more scale and economic advantages. Especially with the gradual depletion of coal resources, the rising calls for environmental protection and the concern about climate change, as well as people's deepening understanding of the various disadvantages of traditional energy, developed countries in the world have invested a lot of manpower, material resources and financial resources to develop environmentally friendly new energy sources, which has led to the rapid expansion of the wind power industry.
[0003] The upstream materials of the wind power industry mainly include towers, wind turbines, nacelles, main shafts, cables and blades. Wind turbine blades are one of the core components of wind turbines. Their good design, reliable quality and superior performance are the decisive factors to ensure the normal and stable operation of wind turbines.
[0004] From the perspective of wind turbine blade structure, it is mainly composed of reinforcement materials, sandwich materials, matrix materials, surface coatings and structural adhesives between different parts. In the application of wind turbine blades, the structural core material is the key material of wind turbine blades, which can greatly ensure the stability of the laminate, while improving the strength and rigidity of the blade structure, reducing the weight of the blade, preventing local instability, and further improving the impact resistance and load resistance of the entire blade. The sandwich materials currently used in wind turbine blades mainly include balsa wood, PVC foam, PET foam, etc.
[0005] Among them, the good pore structure of PET foam is conducive to processing and is suitable for all resin systems and process technologies. Through thermoforming, complex shapes can be achieved, and under heating, it has good thermal stability, high production efficiency, and low scrap rate, effectively reducing pollution and production costs. PET foam also has an excellent closed-cell structure, and absorbs less resin during infusion molding, which helps reduce the production cost of blades. Therefore, PET foam materials are widely used in wind turbine blades.
[0006] PET foam is a thermoplastic material that can be recycled. Currently, recycled bottle flakes can be used as raw materials to produce PET foam boards, which can meet the requirements of wind turbine blade core materials. In addition to recycled bottle flakes, chemical fiber recycled materials also account for a large proportion of recycled PET materials, but chemical fiber recycled materials themselves have a low melting point and low intrinsic viscosity. These two indicators will reduce the viscosity in the molten state when participating in the PET foaming reaction, resulting in too low pressure on the extruder, reduced polymerization reaction efficiency, and the produced PET foam boards do not meet the use requirements. Summary of the invention
[0007] In order to use chemical fiber recycled particles as raw materials to prepare PET foam boards that meet the required specifications, the present application provides a PET foam board of chemical fiber recycled particles and a preparation method and application thereof.
[0008] In a first aspect, the present application provides a PET foam board of recycled chemical fiber particles, which adopts the following technical solution.
[0009] A PET foam board of chemical fiber recycled particles comprises the following raw materials in parts by weight: 10-50 parts of PET particles, 20-60 parts of chemical fiber particles, 30-35 parts of secondary materials, 0.5-1.1 parts of crosslinking agent, 1.5-2.0 parts of nucleating agent, 0.8-1.5 parts of chain extender, 0.5-1.0 parts of lubricant and 0.4-1.0 parts of foaming agent.
[0010] By adopting the above technical solution, part of the PET particles are replaced with chemical fiber particles. The chemical fiber particles themselves contain many additives required for chemical fibers, which results in the low characteristic viscosity of the chemical fiber particles. In this application, the adverse effects of the additives in the chemical fiber particles are offset by adjusting the proportion of the additives. The chain extender in the additive can increase the length of the molecular chain and the bonding strength; the cross-linking agent plays a lubricating role in the entire chemical reaction process, thereby improving the smoothness of the reaction. If the lubrication is insufficient, the resistance between the inside of the extruder and the PET increases. Its main function is to reduce the extruder pressure, protect the equipment, and ensure the smooth extrusion of the material. The compressive strength of the obtained extruded PET foam board can reach 6.73-7.12MPa, the shear strength can reach 2.66-3.01 MPa, and the tensile strength can reach 290.2-301.7MPa, which can meet the requirements of the core material of wind turbine blades.
[0011] Furthermore, the following raw materials are included in parts by weight: 20-45 parts of PET particles, 30-50 parts of chemical fiber particles, 31-33 parts of secondary materials, 0.7-0.9 parts of crosslinking agent, 1.6-1.8 parts of nucleating agent, 1.0-1.2 parts of chain extender, 0.6-0.8 parts of lubricant, and 0.5-0.7 parts of foaming agent.
[0012] By adopting the above technical solution, the ratio of each raw material is further optimized and the comprehensive performance of the foam board is further improved.
[0013] Furthermore, the weight ratio of the crosslinking agent to the chain extender is 1:(1.3-1.5).
[0014] Furthermore, the intrinsic viscosity of the chemical fiber particles is 0.595-0.605 dl / g.
[0015] Furthermore, the intrinsic viscosity of the PET particles is 1.215-1.225 dl / g, and the intrinsic viscosity of the secondary material is 1.195-1.205 dl / g.
[0016] Furthermore, the chain extender includes one or more of pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate trimer.
[0017] Furthermore, the chain extender comprises pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate trimer in a weight ratio of 1:(3-5):(0.5-1).
[0018] Due to the presence of rigid benzene rings and short flexible chain segments in the PET molecular chain, its melt strength is poor and the crystallization rate is slow, so many problems arise during the foaming process. Improving the melt strength of PET through chemical modification is a necessary condition for the foaming of recycled waste PET materials, and this can be achieved by adding chain extenders. Chain extenders are additives containing at least two functional groups, which can react with the groups of the macromolecular chain segments to produce new covalent bonds to form high molecular weight and recyclable polymers, thereby improving the feasibility of PET foaming.
[0019] By adopting the above technical solution, pyromellitic anhydride is an acid anhydride chain extender that can react with the terminal hydroxyl group of PET, not only extending the molecular chain of PET, but also causing branching and even cross-linking reactions with PET in excess, thus increasing the viscosity of low molecular weight PET. However, the reaction between pyromellitic anhydride and the terminal hydroxyl group of the PET molecular chain easily leads to an increase in the terminal carboxyl content in the system, and the acidic environment caused by a large number of carboxyl groups easily causes PET to thermally decompose at high temperatures.
[0020] Tetraglycidyl diaminodiphenylmethane is a tetrafunctional epoxy chain extender that can not only increase the melt viscosity of PET, but also has high reactivity of the epoxy group in the tetraglycidyl diaminodiphenylmethane molecule, which can react with both carboxyl and hydroxyl groups, and has high reactivity, and can effectively reduce the terminal carboxyl content of the reaction system, thereby inhibiting the thermal degradation of PET.
[0021] The isocyanate group of the hexamethylene diisocyanate trimer chemically reacts with the terminal hydroxyl group of PET. The two are connected by chemical bonds to make the polymer molecular chain grow, and synergistically act with pyromellitic anhydride to increase the viscosity of low molecular weight PET.
[0022] The present invention uses a specific ratio of pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate trimer to extend the chain, thereby obtaining a PET melt having a molecular structure with a topological structure, and the strength, extrusion swell phenomenon, shear viscosity and storage modulus of the obtained PET melt are all improved, and these properties increase the resistance to cell merging, improve the overall stability of the cell structure, and thus enhance the PET foaming effect, thereby obtaining a foamed sheet with excellent comprehensive performance.
[0023] In a second aspect, the present application provides a method for preparing a PET foam board of recycled chemical fiber particles, using the following technical solution.
[0024] A method for preparing a PET foam board of chemical fiber recycled particles, characterized in that it comprises the following steps: S1. Raw material preheating Dry each raw material at 60-70°C for 3-4 hours, then heat to 160-170°C; S2. Extruder preheating Preheat the extruder at 320℃ for 5-6 hours, discharge the remaining material in the extruder, add the cleaning agent, stabilize for 30 minutes, then add other raw materials except the foaming agent, until the clean material is discharged from the extruder outlet, then add the foaming agent; S3. Set the extruder temperature The temperature settings of each zone of the extruder are: Zone 1 295-300°C, Zone 2 295-300°C, Zone 3 295-300°C, Zone 4 290-295°C, Zone 5 285-295°C, Zone 6 290-295°C, Zone 7 270-275°C, Zone 8 260-265°C, Zone 9 280-285°C, Zone 9A 265-270°C, Zone 10 260-265°C, Zone 11 260-265℃, Zone 12 260-265℃, Zone 13 260-265℃, Zone 14 260-265℃, Zone 15 260-265℃, Oil Zone 1 245-255℃, Oil Zone 2 235-240℃, Oil Zone 3 230-235℃, Oil Zone 4 225-230℃, Oil Zone 5 245-250℃, Ring Network Device 275-285℃, Head 1 275-285℃, die 2 275-285℃, die 3 290-295℃, die 4 290-295℃, die 5 285-290℃, die 6 285-290℃, die 1 245-275℃, die 2 245-275℃, die 3 245-275℃, die 4 245-275℃, mixer 235-240℃; S4. Extrusion As the temperature gradually drops to the set value, the material at the outlet of the extruder gradually presents the normal shape of a foam board, and is pulled from the front puller to the rear puller, and after de-edging and flying sawing, it is cooled in a cooling tower, and then passed through a planer before being stacked; S5. Welding After the plate is cooled for 2 days, it is welded to the corresponding length as required; S6. Cut After the welded plates are cooled for 2 days, they are cut into sheets of different sizes according to needs.
[0025] Furthermore, the screw speed of the extruder is 17.8-18.2RPM.
[0026] The foamed board is prepared by a continuous extrusion foaming process. During the extrusion process, the treated PET is mixed with a foaming agent and then added to a screw extruder. The barrel temperature is set mainly considering the decomposition temperature of the foaming agent and the melting temperature of other components of the foaming system. The screw speed affects the die pressure and the residence time of the melt in the extruder. By adopting the above technical solution, according to the ratio of the additives, the extrusion temperature and screw speed matched therewith are set, and a PET foamed board with excellent comprehensive performance is obtained.
[0027] In a third aspect, the present application provides an application of a PET foam board made of recycled chemical fiber particles, using the following technical solution.
[0028] An application of a PET foamed board made of recycled chemical fiber particles, wherein the foamed board is applied to core materials of wind turbine blades.
[0029] In summary, this application has the following beneficial effects: The chemical fiber particles of the present application replace part of the PET particles, and the adverse effects of the additives in the chemical fiber particles are offset by additives in a specific ratio, and then extrusion foaming is performed through a specific extrusion process to obtain an extruded PET foam board with a compressive strength of 6.73-7.12MPa, a shear strength of 2.66-3.01MPa, and a tensile strength of 290.2-301.7MPa, which can meet the requirements of the core material of wind turbine blades. DETAILED DESCRIPTION
[0030] The present application is further described in detail below with reference to the embodiments.
[0031] raw material The raw materials in the examples of this application can be obtained from the market: PET granules, polyethylene terephthalate 100%; Secondary materials, scraps generated during the production of PET foam boards; Crosslinking agent, antioxidant TH-17901; Nucleating agent, silica; Tetraglycidyldiaminodiphenylmethane, light yellow viscous liquid, molecular weight 422; Pyromellitic anhydride, white crystalline powder, molecular weight 218; Hexamethylene diisocyanate trimer, technical pure; Lubricant, 1,2,4,5-pyromellitic dianhydride; Blowing agent, cyclopentane.
[0032] Example Examples 1-7 A PET foam board of chemical fiber recycled particles, the preparation process of which is as follows: S1. Raw material preheating Each raw material was dried at 65°C for 3.5 hours and then heated to 165°C; S2. Extruder preheating Preheat the extruder at 320°C for 5.5 hours, discharge the remaining material in the extruder, add the cleaning agent, stabilize for 30 minutes, and then add other raw materials except the foaming agent according to the raw material ratio in Table 1 until the clean material is discharged from the extruder outlet, and then add the foaming agent; S3. Extruder cooling The temperature of each zone of the extruder was set according to Table 2; the screw speed of the extruder was 17.8 RPM; S4. Extrusion As the temperature gradually drops to the set value, the material at the outlet of the extruder gradually presents the normal shape of a foam board, and is pulled from the front puller to the rear puller, and after de-edging and flying sawing, it is cooled in a cooling tower, and then passed through a planer before being stacked; S5. Welding After the plate is cooled for 2 days, it is welded to the corresponding length as required; S6. Cut After the welded plates are cooled for 2 days, they are cut into sheets of different sizes according to needs.
[0033] Table 1 Example 1-7 PET foam board raw material ratio table (kg)
[0034] Among them, the intrinsic viscosity of the chemical fiber particles is 0.595 dl / g, the intrinsic viscosity of the PET particles is 1.225 dl / g, and the intrinsic viscosity of the secondary material is 1.195 dl / g; the chain extender includes trimer of pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate in a weight ratio of 1:3:1.
[0035] Table 2 Temperature setting table of extruder in PET foam board preparation process in Examples 1-7
[0036] Example 8 Different from Example 3, in Example 8, the intrinsic viscosity of the chemical fiber particles is 0.600 dl / g, the intrinsic viscosity of the PET particles is 1.220 dl / g, and the intrinsic viscosity of the secondary material is 1.200 dl / g.
[0037] Example 9 Different from Example 3, in Example 8, the intrinsic viscosity of the chemical fiber particles is 0.605 dl / g, the intrinsic viscosity of the PET particles is 1.215 dl / g, and the intrinsic viscosity of the secondary material is 1.205 dl / g.
[0038] Example 10 Different from Example 3, the intrinsic viscosity of the chemical fiber particles in Example 8 is 0.595 dl / g.
[0039] Embodiment 11 Different from Example 8, the chain extender in Example 11 includes pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate trimer in a weight ratio of 1:5:0.5.
[0040] Example 12 Different from Example 8, the chain extender in Example 12 includes pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate trimer in a weight ratio of 2:5:0.5.
[0041] Example 13 Different from Example 8, the chain extender in Example 13 includes pyromellitic anhydride and tetraglycidyl diaminodiphenylmethane in a weight ratio of 1:5.5.
[0042] Examples 14-16 Different from Example 8, the chain extenders in Examples 14-16 are pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane, and hexamethylene diisocyanate trimer, respectively.
[0043] Embodiment 17 Different from Example 8, the extruder temperature setting of the PET foam board preparation process in Example 17 is different, see Table 3 for details.
[0044] Table 3 Example 17 PET foam board preparation process extruder temperature setting table
[0045] Embodiment 18 Different from Example 8, in Example 17, the temperature of oil zone 2 is 245°C, the temperature of oil zone 3 is 235°C, and the temperature of oil zone 4 is 235°C.
[0046] Embodiment 19 Different from Example 8, in Example 17, the temperature of oil zone 2 is 240°C, the temperature of oil zone 3 is 240°C, and the temperature of oil zone 4 is 230°C.
[0047] Embodiment 20 Different from Example 8, the mixer temperature in Example 20 is 230°C.
[0048] Embodiment 21 Different from Example 8, the mixer temperature in Example 21 is 245°C.
[0049] Embodiment 22 Different from Example 8, the extruder screw speed in Example 22 is 18.2 RPM.
[0050] Embodiment 23 Different from Example 8, the extruder screw speed in Example 23 is 17.5 RPM.
[0051] Embodiment 24 Different from Example 8, the extruder screw speed in Example 24 is 18.5 RPM.
[0052] Comparative Example Comparative Example 1 The difference from Example 1 is that the amount of the cross-linking agent in Comparative Example 1 is 0.3 kg and the amount of the chain extender is 1.6 kg.
[0053] Comparative Example 2 The difference from Example 1 is that the crosslinking agent in Comparative Example 2 is 1.3 kg and the chain extender is 0.6 kg.
[0054] Performance Testing The foamed boards obtained in the examples and comparative examples were tested for performance according to the methods in ASTM D1621, ASTM C-273, and ASTM D-1623. The test results are shown in Table 4.
[0055] Table 4 Performance test results
[0056] Combining Examples 1-24 with Comparative Examples 1-2 and Table 4, it can be seen that the compressive strength, shear strength and tensile strength of the foamed boards prepared in Examples 1-24 are better than those in Comparative Examples 1-2, which indicates that the foamed boards prepared in the present application have better comprehensive performance.
[0057] Combining Examples 1-5 and Table 4, it can be seen that the change in the raw material ratio of the foam board will significantly affect the mechanical properties of the foam board, among which the comprehensive mechanical properties of the foam board obtained by combining the raw material formula and the preparation process in Example 3 are better.
[0058] Combining Example 3 with Examples 6-7 and Table 4, it can be seen that the ratio of the crosslinking agent to the chain extender affects the mechanical properties of the foamed board, and the ratio of the crosslinking agent to the chain extender in Example 3 is better. This may be because the chain extender in the additive can increase the molecular chain length and improve the viscosity of the PET molecule; while the crosslinking agent plays a lubricating role in the entire chemical reaction process, and after the viscosity of the PET molecule is increased, it ensures smooth extrusion, thereby obtaining a foamed board with excellent comprehensive mechanics.
[0059] Combining Example 3 with Examples 8-10 and Table 4, it can be seen that the viscosity of the chemical fiber particles and the PET particles is adjusted to adjust the viscosity of the entire PET, and the application of low-viscosity chemical fiber particles is achieved by combining with additives.
[0060] Combining Example 8 with Examples 11-16 and Table 4, it can be seen that in Examples 8 and 11-12, pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate trimer are used as chain extenders, in Example 13, pyromellitic anhydride and tetraglycidyl diaminodiphenylmethane are used as chain extenders, and in Examples 14-16, pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate trimer are used as chain extenders. It is obvious that the comprehensive mechanical properties of the foamed boards in Examples 8 and 11-12 are higher than those in Example 13, and the comprehensive mechanical properties of the foamed board in Example 13 are higher than those in Examples 14-16. The comprehensive mechanical properties of the foamed board in Example 12 are relatively weaker than those in Example 8 and Example 11, which indicates that the mechanical properties of the foamed board can be effectively improved by compounding pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate trimer as a chain extender within the ratio range specified in the present application. This may be because pyromellitic anhydride and hexamethylene diisocyanate trimer react with the terminal hydroxyl groups of PET, so that the polymer molecular chain grows and the melt viscosity of PET is increased. At the same time, the epoxy group in the tetraglycidyl diaminodiphenylmethane molecule has high reactivity, and the epoxy group can react with both the carboxyl group and the hydroxyl group, and has high reactivity, and can effectively reduce the terminal carboxyl content of the reaction system, thereby inhibiting the thermal degradation of PET, and obtaining a foamed board with excellent comprehensive performance.
[0061] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A PET foam board made of recycled chemical fiber particles, characterized in that: The invention comprises the following raw materials in parts by weight: 10-50 parts of PET particles, 20-60 parts of chemical fiber particles, 30-35 parts of secondary materials, 0.5-1.1 parts of crosslinking agent, 1.5-2.0 parts of nucleating agent, 0.8-1.5 parts of chain extender, 0.5-1.0 parts of lubricant and 0.4-1.0 parts of foaming agent.
2. The PET foam board of chemical fiber recycling particles according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 20-45 parts of PET particles, 30-50 parts of chemical fiber particles, 31-33 parts of secondary materials, 0.7-0.9 parts of crosslinking agent, 1.6-1.8 parts of nucleating agent, 1.0-1.2 parts of chain extender, 0.6-0.8 parts of lubricant and 0.5-0.7 parts of foaming agent.
3. The PET foam board of chemical fiber recycling particles according to claim 1, characterized in that: The weight ratio of the crosslinking agent to the chain extender is 1:(1.3-1.5).
4. The PET foam board of chemical fiber recycling particles according to claim 1, characterized in that: The intrinsic viscosity of the chemical fiber particles is 0.595-0.605 dl / g.
5. The PET foam board of chemical fiber recycling particles according to claim 1, characterized in that: The intrinsic viscosity of the PET particles is 1.215-1.225 dl / g, and the intrinsic viscosity of the secondary material is 1.195-1.205 dl / g.
6. The PET foam board of chemical fiber recycling particles according to claim 1, characterized in that: The chain extender includes one or more of pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate trimer.
7. The PET foam board of chemical fiber recycling particles according to claim 5, characterized in that: The chain extender comprises a trimer of pyromellitic anhydride, tetraglycidyl diaminodiphenylmethane and hexamethylene diisocyanate in a weight ratio of 1:(3-5):(0.5-1).
8. A method for preparing a PET foam board of chemical fiber recycled particles according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. Raw material preheating Dry each raw material at 60-70°C for 3-4 hours, then heat to 160-170°C; S2. Extruder preheating Preheat the extruder at 320℃ for 5-6 hours, discharge the remaining material in the extruder, add the cleaning agent, stabilize for 30 minutes, then add other raw materials except the foaming agent, until the clean material is discharged from the extruder outlet, then add the foaming agent; S3. Set the extruder temperature The temperature settings of each zone of the extruder are: Zone 1 295-300°C, Zone 2 295-300°C, Zone 3 295-300°C, Zone 4 290-295°C, Zone 5 285-295°C, Zone 6 290-295°C, Zone 7 270-275°C, Zone 8 260-265°C, Zone 9 280-285°C, Zone 9A 265-270°C, Zone 10 260-265°C, Zone 11 260-265℃, Zone 12 260-265℃, Zone 13 260-265℃, Zone 14 260-265℃, Zone 15 260-265℃, Oil Zone 1 245-255℃, Oil Zone 2 235-240℃, Oil Zone 3 230-235℃, Oil Zone 4 225-230℃, Oil Zone 5 245-250℃, Ring Network Device 275-285℃, Head 1 275-285°C, die 2 275-285°C, die 3 290-295°C, die 4 290-295°C, die 5 285-290°C, die 6 285-290°C, die 1 245-275°C, die 2 245-275°C, die 3 245-275°C, die 4 245-275°C, mixer 235-240°C; S4. Extrusion As the temperature gradually drops to the set value, the material at the outlet of the extruder gradually presents the normal shape of a foam board, and is pulled from the front puller to the rear puller, and after de-edging and flying sawing, it is cooled in a cooling tower, and then passed through a planer before being stacked; S5. Welding After the plate is cooled for 2 days, it is welded to the corresponding length as required; S6. Cut After the welded plates are cooled for 2 days, they are cut into sheets of different sizes according to needs.
9. The method for preparing a PET foam board of chemical fiber recycling particles according to claim 8, characterized in that: The screw speed of the extruder was 17.8-18.2 RPM.
10. An application of a PET foam board made of recycled chemical fiber particles as claimed in any one of claims 1 to 7, characterized in that: The foamed board is applied to the core material of a wind turbine blade.
Citation Information
Patent Citations
Foaming PET sheet material and method for preparing same
CN101544811A
PET foam product and preparation method thereof
CN105131538A
Thermoplastic polyester extrusion foam forming method
CN109605708A
High-scratch-resistance physical foaming extrusion PET and PP composite material and preparation method thereof
CN110527263A
Polyester foam material and preparation method thereof
CN113025007A
Cited By
PET (Polyethylene Terephthalate) foam board prepared from chemical fiber reclaimed materials as well as preparation method and application of PET foam board