Water-based flame-retardant coating and preparation method thereof
By combining the preparation of modified flame retardant and polyurethane acrylate, the problem of poor flame retardant performance of polyurethane acrylate coating is solved, and the efficient flame retardant performance of water-based flame retardant coating is achieved. It is suitable for a variety of fields and reduces environmental pollution. .
Patent Information
- Application Number
- CN202411171742.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-08
AI Technical Summary
The flame retardant properties of existing polyurethane acrylate coatings are poor, which limits their application in the coating field, especially the disadvantages of water-based materials to environmental pollution.
Using a modified flame retardant, the modified flame retardant with a particle size of 50-100μm was prepared by heating and stirring methylpiperazine and ammonium polyphosphate in methanol, and then adding cobalt nitrate and dimethylimidazole. Combined with polyurethane acrylate, aqueous alkyd resin, etc., an aqueous flame retardant coating was prepared.
It significantly improves the flame retardant performance of water-based flame retardant coatings, making them suitable for buildings, coatings, plastics, wires and cables, and shows better flame retardant effect when the particle size of modified flame retardant is 60-90μm. .
Smart Images

Figure BDA0005009474670000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coating materials, and particularly relates to a water-based flame-retardant coating and a preparation method thereof. Background Art
[0002] Paint is applied to the surface of the object to be protected or decorated, and can form a continuous film that is firmly attached to the object. It is usually a viscous liquid made of resin, oil, or emulsion, with or without pigments, fillers, and corresponding additives, and is prepared with organic solvents or water. Paint is often made of chemical mixtures, and has four main functions: protection, decoration, concealing product defects and other special functions to enhance the value of the product. Paints can be divided into: anti-corrosion paint, anti-rust paint, insulation paint, high temperature resistant paint, aging resistant paint, acid and alkali resistant paint, chemical medium resistant paint, etc. according to their performance.
[0003] Polyurethane acrylate contains acrylic functional groups and carbamate bonds. The acrylic functional groups have the high wear resistance, adhesion, flexibility, high peel strength and excellent low-temperature resistance of polyurethane and the excellent optical properties and weather resistance of polyacrylate. It is a radiation-curing material with excellent comprehensive properties and has been widely used in the field of coatings. However, the flame retardant properties of polyurethane acrylate cured products are poor, which limits its application.
[0004] CN101864151A discloses a flame retardant resin composition for high peeling reinforced printed circuit board, a printed circuit board using the same and a manufacturing method thereof, the flame retardant resin composition comprises: a composite epoxy resin, which comprises a bisphenol A type epoxy resin, a cresol novolac epoxy resin, a rubber modified epoxy resin and a phosphorus epoxy resin; a curing agent; a curing accelerator; and a calcium carbonate inorganic filler, which has not only thermal stability and mechanical strength but also high peeling strength. However, the above-mentioned flame retardant coating is not a water-based material and has the disadvantage of environmental pollution.
[0005] Therefore, it is necessary to develop new water-based coatings containing polyurethane acrylates to improve their flame retardant properties. Summary of the invention
[0006] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a water-based flame retardant coating and a preparation method thereof.
[0007] To achieve the purpose of the present invention, the present invention provides a water-based flame retardant coating, which comprises, by weight:
[0008] 15-35 parts of polyurethane acrylate, 20-40 parts of water-based alkyd resin, 1-10 parts of diluent, 1-5 parts of dispersant, 1-5 parts of defoamer, 1-3 parts of titanium dioxide, 1-10 parts of modified flame retardant, 1-3 parts of wetting agent, 25-40 parts of water, wherein the flame retardant is a modified flame retardant prepared by the following preparation method: 1) adding methylpiperazine to methanol, stirring evenly, then adding ammonium polyphosphate, heating and stirring overnight, and obtaining product 1 after post-treatment; 2) adding product 1 to methanol, adding cobalt nitrate, stirring evenly, adding dimethylimidazole, and obtaining modified flame retardant after post-treatment.
[0009] In some preferred embodiments, the polyurethane acrylate of the present invention has a functionality of 5 and a relative molecular mass between 2000-3000.
[0010] In some preferred embodiments, the diluent described in the present invention is dipropylene glycol methyl ether.
[0011] In some preferred embodiments, the dispersant described in the present invention is hydroxypropyl methylcellulose.
[0012] In some preferred embodiments, the defoamer described in the present invention is DF-89 water-based coating defoamer.
[0013] In some preferred embodiments, the particle size of the modified flame retardant is 50-100 μm, and more preferably, the particle size of the modified flame retardant is 60-90 μm.
[0014] In some preferred embodiments, in step 1) of the method for preparing the modified flame retardant, the weight ratio of anhydrous piperazine to ammonium polyphosphate particles is (50-100):(80-150), preferably (70-80):(100-110).
[0015] In some preferred embodiments, in step 1) of the method for preparing the modified flame retardant, the post-treatment method is cooling to room temperature, filtering, washing, drying, grinding, and sieving.
[0016] In some preferred embodiments, in step 2) of the method for preparing the modified flame retardant, the post-treatment method is filtering, washing, drying, grinding, and screening.
[0017] In some preferred embodiments, in step 2) of the method for preparing the modified flame retardant, the modified flame retardant is sieved with 170-230 mesh.
[0018] In some preferred embodiments, the present invention provides a water-based flame retardant coating, characterized in that, in parts by weight, it includes: 20-30 parts of polyurethane acrylate, 25-35 parts of water-based alkyd resin, 3-6 parts of diluent, 2-4 parts of dispersant, 2-4 parts of defoaming agent, 2-3 parts of titanium dioxide, 3-7 parts of modified flame retardant, 2-3 parts of wetting agent, and 30-35 parts of water.
[0019] In some preferred embodiments, the present invention provides a water-based flame retardant coating, characterized in that, in parts by weight, it includes: 25 parts of polyurethane acrylate, 30 parts of water-based alkyd resin, 4-5 parts of diluent, 3 parts of dispersant, 3 parts of defoaming agent, 2 parts of titanium dioxide, 4-6 parts of modified flame retardant, 2 parts of wetting agent, and 30-35 parts of water.
[0020] In some preferred embodiments, the present invention provides a water-based flame retardant coating, characterized in that, in parts by weight, it includes: 25 parts of polyurethane acrylate, 30 parts of water-based alkyd resin, 4 parts of diluent, 3 parts of dispersant, 3 parts of defoaming agent, 2 parts of titanium dioxide, 5 parts of modified flame retardant, 2 parts of wetting agent, and 35 parts of water.
[0021] The present invention also provides a method for preparing a modified flame retardant, comprising:
[0022] 1) adding methylpiperazine to methanol, stirring evenly, then adding ammonium polyphosphate, heating and stirring overnight, and obtaining product 1 after post-treatment;
[0023] 2) Add product 1 to methanol, add cobalt nitrate, stir evenly, add dimethylimidazole, and obtain a modified flame retardant after post-treatment.
[0024] In some preferred embodiments, the present invention provides a method for preparing a modified flame retardant, comprising:
[0025] 1) adding methylpiperazine to methanol, stirring evenly, then adding ammonium polyphosphate, heating and stirring overnight, and obtaining product 1 after post-treatment, wherein the post-treatment method comprises cooling to room temperature, suction filtration, washing, drying, grinding, and sieving;
[0026] 2) adding the product 1 to methanol, adding cobalt nitrate, stirring evenly, adding dimethylimidazole, and obtaining a modified flame retardant after post-treatment, wherein the post-treatment method comprises filtering, washing, drying, grinding, and sieving.
[0027] In some preferred embodiments, the present invention provides a method for preparing a modified flame retardant, comprising:
[0028] 1) adding methylpiperazine to methanol, stirring evenly, then adding ammonium polyphosphate, heating and stirring overnight, and obtaining product 1 after post-treatment, wherein the post-treatment method comprises cooling to room temperature, suction filtration, washing, drying, grinding, and sieving;
[0029] 2) adding product 1 to methanol, adding cobalt nitrate, stirring evenly, adding dimethylimidazole, and obtaining a modified flame retardant after post-treatment, wherein the post-treatment method comprises filtering, washing, drying, grinding, and sieving, wherein 170-230 mesh is used for sieving.
[0030] The present invention also provides a method for preparing a water-based flame retardant coating, comprising:
[0031] 1) Weighing polyurethane acrylate, water-based alkyd resin, diluent, dispersant, defoamer, titanium dioxide, modified flame retardant, wetting agent, and water respectively according to the above weight percentages;
[0032] 2) adding polyurethane acrylate, water-based alkyd resin, defoamer, modified flame retardant and diluent into a mixer for mixing and stirring at a speed of 600-700 r / min for 30-40 min;
[0033] 3) Add dispersant, titanium dioxide, wetting agent and water, stir at a speed of 400-500 r / min, stir for 15-20 min, and obtain a water-based flame retardant coating after stirring.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The inventors of the present invention have found that a water-based flame-retardant coating of the present invention has stronger flame-retardant properties by modifying the flame retardant, and can be applied to the fields of construction, coatings, plastics, wires and cables, wood, etc.; and when the particle size of the modified flame retardant is 60-90μm, its flame retardant effect is better. DETAILED DESCRIPTION
[0036] The following representative examples are intended to better illustrate the present invention, but are not intended to limit the scope of the present invention. Unless otherwise specified, the materials used in the following examples were commercially available.
[0037] Sources of some raw materials:
[0038] The polyurethane acrylate uses the flame-retardant aliphatic polyurethane acrylate of Guangzhou Sanwang Chemical Materials Co., Ltd., with the brand name SW3675;
[0039] Waterborne alkyd resin was purchased from Hebei Deda New Materials Co., Ltd.;
[0040] Polyphosphoramide was purchased from Sichuan Haiwang Technology Co., Ltd.
[0041] The above raw material manufacturer models are only specifically selected to support the raw materials in the embodiments and are adopted in the experiments. In the actual production and preparation process, the sources of raw materials are not limited to the above manufacturer models.
[0042] Preparation of modified flame retardant
[0043] 1) adding 75 parts by weight of methylpiperazine to methanol, stirring evenly, then adding 100 parts by weight of ammonium polyphosphate, heating to 80° C. and stirring overnight, cooling to room temperature, filtering, washing, drying, grinding, and sieving to obtain an intermediate;
[0044] 2) The intermediate is added to methanol, cobalt nitrate is added, and after stirring evenly, dimethylimidazole is added, and stirring evenly, and then filtered, washed, dried, and ground. The obtained product is sieved with 170-230 mesh to obtain a modified flame retardant.
[0045] Example 1
[0046] A water-based flame retardant coating, characterized in that, in parts by weight, it comprises: 25 parts of polyurethane acrylate, 30 parts of water-based alkyd resin, 4 parts of diluent, 3 parts of dispersant, 3 parts of defoamer, 2 parts of titanium dioxide, 5 parts of modified flame retardant (particle size is 70 μm), 2 parts of wetting agent, and 35 parts of water;
[0047] The preparation method thereof comprises:
[0048] 1) Weighing polyurethane acrylate, water-based alkyd resin, diluent, dispersant, defoamer, titanium dioxide, modified flame retardant, wetting agent, and water respectively according to the above weight percentages;
[0049] 2) adding polyurethane acrylate, water-based alkyd resin, defoamer, modified flame retardant and diluent into a mixer for mixing and stirring at a speed of 600-700 r / min for 30-40 min;
[0050] 3) Add dispersant, titanium dioxide, wetting agent and water, stir at a speed of 400-500 r / min, stir for 15-20 min, and obtain a water-based flame retardant coating after stirring.
[0051] Example 2
[0052] A water-based flame retardant coating, characterized in that, in parts by weight, it comprises: 20 parts of polyurethane acrylate, 25 parts of water-based alkyd resin, 3 parts of diluent, 2 parts of dispersant, 2 parts of defoamer, 2 parts of titanium dioxide, 3 parts of modified flame retardant (particle size is 70 μm), 2 parts of wetting agent, and 30 parts of water;
[0053] The preparation method thereof comprises:
[0054] 1) Weighing polyurethane acrylate, water-based alkyd resin, diluent, dispersant, defoamer, titanium dioxide, modified flame retardant, wetting agent, and water respectively according to the above weight percentages;
[0055] 2) adding polyurethane acrylate, water-based alkyd resin, defoamer, modified flame retardant and diluent into a mixer for mixing and stirring at a speed of 600-700 r / min for 30-40 min;
[0056] 3) Add dispersant, titanium dioxide, wetting agent and water, stir at a speed of 400-500 r / min, stir for 15-20 min, and obtain a water-based flame retardant coating after stirring.
[0057] Example 3
[0058] A water-based flame retardant coating, characterized in that, in parts by weight, it comprises: 30 parts of polyurethane acrylate, 35 parts of water-based alkyd resin, 6 parts of diluent, 4 parts of dispersant, 4 parts of defoamer, 3 parts of titanium dioxide, 7 parts of modified flame retardant (particle size is 80 μm), 3 parts of wetting agent, and 40 parts of water;
[0059] The preparation method thereof comprises:
[0060] 1) Weighing polyurethane acrylate, water-based alkyd resin, diluent, dispersant, defoamer, titanium dioxide, modified flame retardant, wetting agent, and water respectively according to the above weight percentages;
[0061] 2) adding polyurethane acrylate, water-based alkyd resin, defoamer, modified flame retardant and diluent into a mixer for mixing and stirring at a speed of 600-700 r / min for 30-40 min;
[0062] 3) Add dispersant, titanium dioxide, wetting agent and water, stir at a speed of 400-500 r / min, stir for 15-20 min, and obtain a water-based flame retardant coating after stirring.
[0063] Example 4
[0064] A water-based flame retardant coating, characterized in that, in parts by weight, it comprises: 35 parts of polyurethane acrylate, 40 parts of water-based alkyd resin, 4 parts of diluent, 4 parts of dispersant, 4 parts of defoamer, 3 parts of titanium dioxide, 6 parts of modified flame retardant (particle size is 90 μm), 2 parts of wetting agent, and 40 parts of water;
[0065] The preparation method thereof comprises:
[0066] 1) Weighing polyurethane acrylate, water-based alkyd resin, diluent, dispersant, defoamer, titanium dioxide, modified flame retardant, wetting agent, and water respectively according to the above weight percentages;
[0067] 2) adding polyurethane acrylate, water-based alkyd resin, defoamer, modified flame retardant and diluent into a mixer for mixing and stirring at a speed of 600-700 r / min for 30-40 min;
[0068] 3) Add dispersant, titanium dioxide, wetting agent and water, stir at a speed of 400-500 r / min, stir for 15-20 min, and obtain a water-based flame retardant coating after stirring.
[0069] Comparative Example 1
[0070] A water-based flame retardant coating, characterized in that, in parts by weight, it comprises: 35 parts of polyurethane acrylate, 35 parts of water-based alkyd resin, 3 parts of diluent, 3 parts of dispersant, 4 parts of defoamer, 3 parts of titanium dioxide, 3 parts of modified flame retardant (particle size is 110 μm), 2 parts of wetting agent, and 30 parts of water;
[0071] The preparation method thereof comprises:
[0072] 1) Weighing polyurethane acrylate, water-based alkyd resin, diluent, dispersant, defoamer, titanium dioxide, modified flame retardant, wetting agent, and water respectively according to the above weight percentages;
[0073] 2) adding polyurethane acrylate, water-based alkyd resin, defoamer, modified flame retardant and diluent into a mixer for mixing and stirring at a speed of 600-700 r / min for 30-40 min;
[0074] 3) Add dispersant, titanium dioxide, wetting agent and water, stir at a speed of 400-500 r / min, stir for 15-20 min, and obtain a water-based flame retardant coating after stirring.
[0075] Comparative Example 2
[0076] A water-based flame retardant coating, characterized in that, in parts by weight, it comprises: 30 parts of polyurethane acrylate, 35 parts of water-based alkyd resin, 4 parts of diluent, 3 parts of dispersant, 4 parts of defoamer, 3 parts of titanium dioxide, 4 parts of polyphosphoramide, 2 parts of wetting agent, and 30 parts of water;
[0077] The preparation method thereof comprises:
[0078] 1) Weighing polyurethane acrylate, water-based alkyd resin, diluent, dispersant, defoamer, titanium dioxide, polyphosphoramide, wetting agent, and water respectively according to the above weight percentages;
[0079] 2) adding polyurethane acrylate, water-based alkyd resin, defoamer, modified flame retardant and diluent into a mixer for mixing and stirring at a speed of 600-700 r / min for 30-40 min;
[0080] 3) Add dispersant, titanium dioxide, wetting agent and water, stir at a speed of 400-500 r / min, stir for 15-20 min, and obtain a water-based flame retardant coating after stirring.
[0081] Experimental Example Performance Test
[0082] The water-based flame retardant coatings prepared in Examples 1 to 4 and Comparative Examples 1-2 were coated on a plate with a length, width and height of 200*200*10, and the plate was fully dried in an oven at 50°C, and then an ablation test was performed on the prepared plate with a hexane spray gun; the limiting oxygen index (LOI) was measured with an oxygen index tester in accordance with GB / T2406-2009, and the results are shown in Table 1:
[0083] Table 1 Performance test results
[0084]
[0085] Therefore, compared with the comparative example, the flame retardant coating of the present invention has better flame retardancy.
[0086] Although the present invention has been described in detail above, it is understood by those skilled in the art that various modifications and changes can be made to the present invention without departing from the spirit and scope of the present invention. The invention is not restricted by the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement methods and shall be included in the protection scope of the present invention.
Claims
1. A water-based flame retardant coating, characterized in that: The invention comprises, by weight, 15-35 parts of polyurethane acrylate, 20-40 parts of water-based alkyd resin, 1-10 parts of diluent, 1-5 parts of dispersant, 1-5 parts of defoamer, 1-3 parts of titanium dioxide, 1-10 parts of modified flame retardant, 1-3 parts of wetting agent and 25-40 parts of water, wherein the flame retardant is a modified flame retardant prepared by the following preparation method: 1) adding methylpiperazine to methanol, stirring evenly, then adding ammonium polyphosphate, heating and stirring overnight, and obtaining product 1 after post-treatment; 2) adding product 1 to methanol, adding cobalt nitrate, stirring evenly, adding dimethylimidazole, and obtaining the modified flame retardant after post-treatment.
2. A water-based flame retardant coating according to claim 1, characterized in that: The particle size of the modified flame retardant is 50-100 μm.
3. The water-based flame-retardant coating according to claim 1, characterized in that: The particle size of the modified flame retardant is 60-90 μm.
4. The water-based flame-retardant coating according to claim 1, characterized in that: The diluent is dipropylene glycol methyl ether.
5. The water-based flame-retardant coating according to claim 1, characterized in that: The dispersant is hydroxypropyl methylcellulose.
6. The water-based flame-retardant coating according to claim 1, characterized in that: The defoamer is DF-89 water-based paint defoamer.
7. The water-based flame-retardant coating according to claim 1, characterized in that: In parts by weight, it includes: 20-30 parts of polyurethane acrylate, 25-35 parts of water-based alkyd resin, 3-6 parts of diluent, 2-4 parts of dispersant, 2-4 parts of defoamer, 2-3 parts of titanium dioxide, 3-7 parts of modified flame retardant, 2-3 parts of wetting agent, and 30-35 parts of water.
8. The water-based flame-retardant coating according to claim 1, characterized in that: In parts by weight, it includes: 25 parts of polyurethane acrylate, 30 parts of water-based alkyd resin, 4 parts of diluent, 3 parts of dispersant, 3 parts of defoamer, 2 parts of titanium dioxide, 5 parts of modified flame retardant, 2 parts of wetting agent, and 35 parts of water.
9. A method for preparing a water-based flame-retardant coating according to claims 1-8, comprising: 1) Weighing polyurethane acrylate, water-based alkyd resin, diluent, dispersant, defoamer, titanium dioxide, modified flame retardant, wetting agent, and water respectively according to the above weight percentages; 2) adding polyurethane acrylate, water-based alkyd resin, defoamer, modified flame retardant and diluent into a mixer for mixing and stirring at a speed of 600-700 r / min for 30-40 min; 3) Add dispersant, titanium dioxide, wetting agent and water, stir at a speed of 400-500 r / min, stir for 15-20 min, and obtain a water-based flame retardant coating after stirring.
Citation Information
Patent Citations
Water-based polyurethane flame-retardant coating used on circuit board and preparation method of water-based polyurethane flame-retardant coating
CN106118445A
Flame-retardant coating containing urethane acrylate and preparation method of flame-retardant coating
CN115820100A
Core-shell structure flame retardant modified large shaving board, preparation method and application
CN118404667A
Cited By
Water-based paint with flame retardance and preparation method thereof
CN119708995A
A flame-retardant water-based coating and preparation method thereof
CN119708995B
Water-based intumescent fireproof coating as well as preparation method and application thereof
CN119823621A
Water-based intumescent fireproof coating as well as preparation method and application thereof
CN122127841A