Waterproof leak-repairing coating as well as preparation method and application thereof

By using two-component polyurethane, talc powder and drying agent, a viscous waterproof and leak-repair coating was prepared, which solved the problem of slow curing speed of water-based waterproof coating and the paint falling off during construction, achieving rapid curing and weather resistance Sex improvement.

CN118909534APending Publication Date: 2024-11-08HUBEI ZHONGRONG LIQING CONSTR ENG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411163367.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing water-based waterproof coatings have slow curing speed, long construction cycle, insufficient wear and weather resistance, and are prone to paint falling off and wasting during construction.

Method used

Using a combination of two-component polyurethane, talc, drying agent and aromatic hydrocarbons, a viscous waterproof leakage repair coating is prepared through a stirring and heating process, which increases the adhesion and weather resistance of the coating and reduces construction. Waste of time and raw materials.

Benefits of technology

It realizes rapid curing of waterproof leakage repair coatings, shortens construction cycles, improves wear resistance and weather resistance, and reduces the shedding and waste of paint during construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of waterproof and leak-repairing coatings, and discloses a waterproof and leak-repairing coating and a preparation method and application thereof.The waterproof and leak-repairing coating is prepared from, by weight, selected resin materials: bi-component polyurethane, acrylic ester, butadiene styrene rubber and modified asphalt, and the comprehensive proportion of the two-component polyurethane, the acrylic ester, the butadiene styrene rubber and the modified asphalt is 0.3 of distribution of a waterproof and leak-proof material assembly; the sum of the inorganic pigment, the fiber material, the talcum powder, the argil and the silica sand accounts for 0.3-0.4 of the distribution of the waterproof leakproof material assembly; according to the invention, the viscous waterproof leak-repairing coating is placed in an environment in which the viscosity is easy to maintain all the time; wherein when too much talcum powder is added, the weather resistance and the aging resistance are easily reduced at the moment; when the added talcum powder is too little, the hardness, ductility and waterproof performance of the material are easily caused, meanwhile, due to the adhesive, the adsorbability is higher when the waterproof leak-repairing coating is used again, and the situation that raw materials are wasted due to falling of the waterproof leak-repairing coating can be avoided to a certain extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waterproof leak-proof coatings, and in particular relates to a waterproof leak-proof coating and a preparation method and application thereof. Background Art

[0002] With the rapid development of China's real estate industry, more and more residential houses are being built, resulting in a large number of serious water leakage problems caused by improper waterproofing, especially in renovated houses, where water leakage is more difficult to deal with.

[0003] At present, the domestic market mainly uses water-based waterproof coatings. However, this coating mainly relies on water evaporation to dry and form a film, so it dries slowly, has a low cross-linking density, and is greatly affected by geographical location and seasons, resulting in a long construction period. At the same time, the film layer is also relatively lacking in wear resistance and weather resistance, and cannot solve the pain points of the domestic waterproof market. Therefore, it is very necessary to develop a waterproof product that has a faster curing speed, a shorter construction period, is not restricted by geographical environment and seasons, and has good wear resistance and weather resistance compared to traditional water-based waterproof coatings;

[0004] However, when the existing waterproof leak-proof coating is used, the coating is often applied to the building materials that need to be repaired during the construction process. At this time, it is easy to fall off, which makes it easy to waste the coating during the bonding process.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:

[0007] A waterproof leak-proof coating comprises the following raw materials in parts by weight:

[0008] Select resin materials: The combined proportion of two-component polyurethane, acrylate, styrene-butadiene rubber and modified asphalt is 0.3 of the total distribution of waterproof and leakproof materials;

[0009] Select filler materials: The total proportion of inorganic pigments, fiber materials, talcum powder, clay, and silica sand is 0.3-0.4 of the total distribution of waterproof and leak-proof materials;

[0010] Selection of additives: The sum of plasticizers, defoamers, dispersants and drying agents accounts for 0.25 of the total distribution of the waterproof and leak-proof material, and the adhesive accounts for 0.25 of the waterproof and leak-proof material;

[0011] Select solvents: The total proportion of solvents such as water alcohols, ketones, ethers and aromatic hydrocarbons is 0.25-0.35 of the total distribution of waterproof materials;

[0012] The total proportion of the selected resin material, filler material, additive and solvent is 100, the proportion of the selected resin material is 30 parts, the proportion of the selected filler material is 30-40 parts, the proportion of the selected additive is 5 parts, and the proportion of the selected solvent is 25-35 parts;

[0013] The specific preparation method of the two-component polyurethane selected from the resin material comprises the following steps:

[0014] Step 1: Select the main materials of two-component polyurethane, polyether polyol, polyester polyol, isocyanate, crosslinking agent and catalyst, and mix them in a certain proportion. The polyether polyol, polyester polyol, isocyanate, crosslinking agent and catalyst are weighed in a proportion so that the total proportion is 0.3 of the waterproof leak-proof coating and the proportion is 30 parts;

[0015] Step 2: Put the prepared polyether polyol, polyester polyol, isocyanate, cross-linking agent and catalyst into the reactor and stir and mix them so that the polyether polyol, polyester polyol, isocyanate, cross-linking agent and catalyst can be mixed evenly and avoid the entry of air to affect the reaction;

[0016] Step 3: After the reaction is completed, take out the prepared two-component polyurethane and wait for curing.

[0017] As a preferred embodiment of the present invention, the operation steps after curing the two-component polyurethane in the above selected resin material are:

[0018] Step 1: When the two-component polyurethane is cured, place it in the grinding equipment;

[0019] Step 2: The staff starts the grinding equipment so that the grinding equipment can grind the solidified two-component polyurethane until the two-component polyurethane becomes powder;

[0020] Step 3: Take out the powdered two-component polyurethane from the grinding equipment, collect it and put it aside.

[0021] As a preferred embodiment of the present invention, based on the above-mentioned selected filler material, the selected filler material is talcum powder: the selected talcum powder is weighed so that it can reach 0.3-0.4 of the distribution of the waterproof leak-proof coating assembly and the proportion is 30-40 parts.

[0022] As a preferred embodiment of the present invention, based on the above-mentioned selection of auxiliary agents, the selected auxiliary agent is a drying agent: the selected drying agent is weighed so that it can reach 0.05 of the total distribution of the waterproof leak-proof coating and the proportion is 5 parts.

[0023] As a preferred embodiment of the present invention, based on the above-mentioned selection of solvents, the selected solvent is an aromatic hydrocarbon: the selected aromatic hydrocarbon is weighed so that it can reach 0.25-0.35 of the total distribution of the waterproof leak-proof coating and the proportion is 25-35 parts.

[0024] Another object of the present invention is to provide a waterproof leak-proof coating and a preparation method thereof, comprising the following steps:

[0025] Step 1: Take out the collected powdered two-component polyurethane, talcum powder, drying agent and aromatic hydrocarbon;

[0026] Step 2: placing powdered two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive into the equipment, heating them by a water bath method, and stirring the two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive by a stirring device in the equipment, so that the two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive can be more fully integrated;

[0027] Step 3: Taking out the mixture when it is evenly stirred, so that the polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive form a relatively viscous waterproof leak-proof coating;

[0028] Step 4: Place the viscous waterproof leak-proof paint in an environment where it can easily maintain its viscosity.

[0029] Another object of the present invention is to provide a waterproof leak-proofing coating according to the present invention for use in building decoration for waterproofing and quick leak-proofing.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The invention comprises the following steps: taking out the collected powdered two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive; placing the powdered two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive in a device, heating them by a water bath method, and stirring the placed two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive by a stirring device in the device, so that the placed two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive can be more fully integrated; taking out the powdered two-component polyurethane when stirred evenly, so that the polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive at this time form a relatively viscous waterproof leak-proof coating; placing the viscous waterproof leak-proof coating in an environment where the viscosity is easily maintained; wherein when too much talcum powder is added, the weather resistance and anti-aging ability are easily reduced; when too little talcum powder is added, the hardness, ductility and waterproof performance of the material are easily reduced; and at the same time, because the talcum powder is contained, the adsorption is stronger when reused, so that the situation that the waterproof leak-proof coating falls off and causes the waste of raw materials can be avoided to a certain extent. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments will be clearly and completely described below in combination with the embodiments of the present invention. The following embodiments are used to illustrate the present invention.

[0033] A waterproof leak-proof coating comprises the following raw materials in parts by weight:

[0034] Select resin materials: The combined proportion of two-component polyurethane, acrylate, styrene-butadiene rubber and modified asphalt is 0.3 of the total distribution of waterproof and leakproof materials;

[0035] Select filler materials: The total proportion of inorganic pigments, fiber materials, talcum powder, clay, and silica sand is 0.3-0.4 of the total distribution of waterproof and leak-proof materials;

[0036] Selection of additives: The sum of plasticizers, defoamers, dispersants and drying agents accounts for 0.25 of the total distribution of the waterproof and leak-proof material, and the adhesive accounts for 0.25 of the waterproof and leak-proof material;

[0037] Select solvents: The total proportion of solvents such as water alcohols, ketones, ethers and aromatic hydrocarbons is 0.25-0.35 of the total distribution of waterproof materials;

[0038] The total proportion of the selected resin material, filler material, additive and solvent is 100, the proportion of the selected resin material is 30 parts, the proportion of the selected filler material is 30-40 parts, the proportion of the selected additive is 5 parts, and the proportion of the selected solvent is 25-35 parts;

[0039] The specific preparation method of the two-component polyurethane selected from the resin material comprises the following steps:

[0040] Step 1: Select the main materials of two-component polyurethane, polyether polyol, polyester polyol, isocyanate, crosslinking agent and catalyst, and mix them in a certain proportion. The polyether polyol, polyester polyol, isocyanate, crosslinking agent and catalyst are weighed in a proportion so that the total proportion is 0.3 of the waterproof leak-proof coating and the proportion is 30 parts;

[0041] Step 2: Put the prepared polyether polyol, polyester polyol, isocyanate, cross-linking agent and catalyst into the reactor and stir and mix them so that the polyether polyol, polyester polyol, isocyanate, cross-linking agent and catalyst can be mixed evenly and avoid the entry of air to affect the reaction;

[0042] Step 3: After the reaction is completed, take out the prepared two-component polyurethane and wait for curing.

[0043] In a specific embodiment, the operation steps after curing the two-component polyurethane in the above selected resin material are:

[0044] Step 1: When the two-component polyurethane is cured, place it in the grinding equipment;

[0045] Step 2: The staff starts the grinding equipment so that the grinding equipment can grind the solidified two-component polyurethane until the two-component polyurethane becomes powder;

[0046] Step 3: Take out the powdered two-component polyurethane from the grinding equipment, collect it and put it aside.

[0047] Further, based on the above-mentioned selection of filler materials, the selected filler material is talcum powder: the selected talcum powder is weighed so that it can account for 0.3-0.4 of the total distribution of the waterproof leak-proof coating and the proportion is 30-40 parts.

[0048] Furthermore, based on the above selection of auxiliary agents, the selected auxiliary agent is a drying agent: the selected drying agent is weighed so that it can reach 0.05 of the total distribution of the waterproof leak-proof coating and the proportion is 5 parts.

[0049] Further, based on the above-mentioned selection of solvents, wherein the selected solvent is an aromatic hydrocarbon: the selected aromatic hydrocarbon is weighed so that it can reach 0.25-0.35 of the total distribution of the waterproof leak-proof coating and the proportion is 25-35 parts.

[0050] Another object of the present invention is to provide a waterproof leak-proof coating and a preparation method thereof, comprising the following steps:

[0051] Step 1: Take out the collected powdered two-component polyurethane, talcum powder, drying agent and aromatic hydrocarbon;

[0052] Step 2: placing powdered two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive into the equipment, heating them by a water bath method, and stirring the two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive by a stirring device in the equipment, so that the two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive can be more fully integrated;

[0053] Step 3: Taking out the mixture when it is evenly stirred, so that the polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive form a relatively viscous waterproof leak-proof coating;

[0054] Step 4: Place the viscous waterproof leak-proof paint in an environment where it can easily maintain its viscosity.

[0055] Another object of the present invention is to provide a waterproof and leak-proof coating for use in building decoration for waterproofing and quick leak-proofing.

[0056] Based on the proportions of talcum powder selected from the above filler materials and aromatic hydrocarbons selected from the solvent, the selected materials are as follows: Table 1 of the proportions of talcum powder and aromatic hydrocarbons:

[0057]

[0058]

[0059] According to the above example of changes in the proportion of talc and aromatic hydrocarbons, the changes in talc and aromatic hydrocarbons are the changes in filler materials and solvents, and the specific effects of the changes in filler materials and solvents on the waterproof leak-proof coating can be determined.

[0060] Based on the specific proportion of drying agent and adhesive in the above additives, composition table 2:

[0061] Proportion 1:2 1:1 2:1 <![CDATA[Auxiliary agent ( 催干剂 )]]> 0.25< 0.25 >0.25 <![CDATA[Auxiliary agent ( 粘合剂 )]]> >0.25 0.25 0.25< Good or bad influence Poor good Poor

[0062] According to the impact of changes in the drying agent and adhesive in the above-mentioned additives on the waterproof leak-proof coating.

[0063] The implementation principle of a waterproof leak-proof coating and its preparation method and application in this embodiment is as follows:

[0064] The main materials for making two-component polyurethane, polyether polyol, polyester polyol, isocyanate, cross-linking agent and catalyst are selected and mixed in a certain proportion. The polyether polyol, polyester polyol, isocyanate, cross-linking agent and catalyst are weighed in a ratio so that the total proportion is 0.3 of the waterproof leak-proof coating and the proportion is 30 parts; the prepared polyether polyol, polyester polyol, isocyanate, cross-linking agent and catalyst are put into the reactor for stirring and mixing, so that the placed polyether polyol, polyester polyol, isocyanate, cross-linking agent and catalyst can be mixed evenly, and the entry of air can be avoided to affect the reaction; when the reaction is completed, the prepared two-component polyurethane is taken out and waited for curing; when the two-component polyurethane is cured, it is placed in a grinding device; the staff starts the grinding device so that the grinding device can grind the cured two-component polyurethane until the two-component polyurethane is powdered; the powdered two-component polyurethane is taken out from the grinding device and collected and placed aside; the collected powdered The two-component polyurethane, talcum powder, drying agent and aromatic hydrocarbon are taken out; the powdered two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive are placed in the equipment, heated by a water bath method, and the placed two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive are stirred by a stirring device in the equipment, so that the placed two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive can be more fully integrated; when the stirring is uniform, it is taken out, so that the polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive at this time form a relatively viscous waterproof sealing coating; the viscous waterproof sealing coating is placed in an environment where it is easy to always maintain viscosity; when too much talcum powder is added, it is easy to cause a decrease in weather resistance and anti-aging ability; when too little talcum powder is added, it is easy to cause the hardness, ductility and waterproof performance of the material. At the same time, because it contains an adhesive, the adsorption is stronger when it is used again, which can avoid the waste of raw materials caused by the falling of the waterproof sealing coating to a certain extent.

Claims

1. A waterproof leak-proof coating, characterized in that: The preparation comprises the following raw materials in parts by weight: Select resin materials: The combined proportion of two-component polyurethane, acrylate, styrene-butadiene rubber and modified asphalt is 0.3 of the total distribution of waterproof and leakproof materials; Select filler materials: The total proportion of inorganic pigments, fiber materials, talcum powder, clay, and silica sand is 0.3-0.4 of the total distribution of waterproof and leak-proof materials; Selection of additives: The total proportion of plasticizer, defoamer, dispersant and drying agent is 0.25 of the total distribution of waterproof and leakproof materials, and the proportion of adhesive is 0.25 of the waterproof and leakproof materials; Select solvents: The total proportion of solvents such as water alcohols, ketones, ethers and aromatic hydrocarbons is 0.25-0.35 of the total distribution of waterproof materials; The total proportion of the selected resin material, filler material, additive and solvent is 100, the proportion of the selected resin material is 30 parts, the proportion of the selected filler material is 30-40 parts, the proportion of the selected additive is 5 parts, and the proportion of the selected solvent is 25-35 parts; The specific preparation method of the two-component polyurethane selected from the resin material comprises the following steps: Step 1: Select the main materials of two-component polyurethane, polyether polyol, polyester polyol, isocyanate, crosslinking agent and catalyst, and mix them in a certain proportion. The polyether polyol, polyester polyol, isocyanate, crosslinking agent and catalyst are weighed in a proportion so that the total proportion is 0.3 of the waterproof leak-proof coating and the proportion is 30 parts; Step 2: Put the prepared polyether polyol, polyester polyol, isocyanate, cross-linking agent and catalyst into the reactor and stir and mix them so that the polyether polyol, polyester polyol, isocyanate, cross-linking agent and catalyst can be mixed evenly and avoid the entry of air to affect the reaction; Step 3: After the reaction is completed, take out the prepared two-component polyurethane and wait for curing.

2. The method for preparing a waterproof leak-proof coating according to claim 1, characterized in that: Based on the above selection of resin materials, the operation steps after curing of the two-component polyurethane are as follows: Step 1: When the two-component polyurethane is cured, place it in the grinding equipment; Step 2: The staff starts the grinding equipment so that the grinding equipment can grind the solidified two-component polyurethane until the two-component polyurethane becomes powder; Step 3: Take out the powdered two-component polyurethane from the grinding equipment, collect it and put it aside.

3. A waterproof leak-proof coating according to claim 1, characterized in that: Based on the above selection of filler materials, the selected filler material is talcum powder: the selected talcum powder is weighed so that it can account for 0.3-0.4 of the total distribution of the waterproof leak-proof coating and the proportion is 30-40 parts.

4. A waterproof leak-proof coating according to claim 1, characterized in that: Based on the above selection of auxiliary agents, the auxiliary agent selected is a drying agent: the selected drying agent is weighed so that it can reach 0.05 of the total distribution of the waterproof leak-proof coating and the proportion is 5 parts.

5. The waterproof leak-proof coating according to claim 1, characterized in that: Based on the above selection of solvents, the selected solvent is aromatic hydrocarbons: the selected aromatic hydrocarbons are weighed so that they can account for 0.25-0.35 of the total distribution of the waterproof leak-proof coating and the proportion is 25-35 parts.

6. A method for preparing a waterproof leak-proof coating as claimed in any one of claims 2 to 5, characterized in that: The following steps are involved: Step 1: Take out the collected powdered two-component polyurethane, talcum powder, drying agent and aromatic hydrocarbon; Step 2: placing powdered two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive into the equipment, heating them by a water bath method, and stirring the two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive by a stirring device in the equipment, so that the two-component polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive can be more fully integrated; Step 3: Taking out the mixture when it is evenly stirred, so that the polyurethane, talcum powder, drying agent, aromatic hydrocarbon and adhesive form a relatively viscous waterproof leak-proof coating; Step 4: Place the viscous waterproof leak-proof paint in an environment where it can easily maintain its viscosity.

7. The waterproof leak-proofing coating as claimed in any one of claims 1 to 6 is used for waterproofing and quick leak-proofing in building decoration.

Citation Information

Patent Citations

  • Uncured polyurethane waterproofing coating and preparation method thereof

    CN103923565A

  • Modified asphalt, preparation method and application

    CN107163597A

  • Preparation technology of non-cured waterproof rubber-asphalt paint

    CN109575807A

  • High-molecular polymer waterproof coating and preparation method thereof

    CN111548680A