Micro part electroforming method and micro part

By using choline chloride-type ionic liquid and metal source for electrodeposition, the defects of traditional water-based electroforming liquid in electroforming of micro-parts are solved, and high-precision and high-performance micro-part preparation is achieved, reducing costs And avoid environmental pollution.

CN118910680APending Publication Date: 2024-11-08XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411306911.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Traditional water-based electroforming liquid has hydrogen evolution reactions during the electroforming of micro parts, resulting in reduced current efficiency, defects such as pinholes and pitting, and the alloy element ratio is difficult to accurately control, affecting the performance of the parts.

Method used

Choline chloride ionic liquid is used as electroforming liquid, combined with ethylene glycol or urea, and electrodeposition is performed using metal sources such as nickel, iron, and copper. Micro parts are formed through electroforming core molds, and post-treatment such as low-temperature heat treatment. and surface polishing.

Benefits of technology

It improves the forming accuracy and performance of micro-parts, avoids defects caused by hydrogen evolution reaction, and achieves low-cost, safe and non-toxic and efficient preparation of high-quality metal micro-parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910680A_ABST
    Figure CN118910680A_ABST
Patent Text Reader

Abstract

The invention provides a micro-part electroforming method and a micro-part, and relates to the technical field of micro-manufacturing forming. The micro part electroforming method comprises the steps that a metal source is added into ionic liquid to obtain electroforming liquid; wherein the ionic liquid comprises choline chloride; the electroforming core mold etched with the microstructure serves as a cathode, a metal sheet serves as an anode, the cathode and the anode are immersed in the electroforming solution, and electroforming is conducted in an electrodeposition mode; and taking out the electroformed cathode component to obtain the micro part. The electroforming effect of the micro part can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of micro-manufacturing forming technology, and in particular to a micro-part electroforming forming method and a micro-part. Background Art

[0002] Metal micro parts have great application prospects in the fields of aviation, aerospace, biomedicine, micro-electromechanical systems (MEMS), etc. due to their excellent mechanical properties and various functional characteristics. Among many micro-forming technologies, micro-electroforming technology has become one of the key technologies for manufacturing metal micro parts due to its advantages of high replication accuracy and repeatability, low cost, ability to prepare nanocrystalline materials and ability to form complex microstructures.

[0003] However, the presence of hydrogen evolution side reactions during the electroplating process of conventional water-based electroforming liquids not only reduces the current efficiency, but also produces defects such as pinholes and pitting in the micro-parts, resulting in low dimensional replication accuracy of the formed metal micro-parts. At the same time, due to the differences in the electronegativity of various metal ions in conventional water-based electroforming liquids, the proportion and type of alloying elements in the micro-electroforming of metal micro-parts are difficult to accurately control, thus affecting and limiting the performance of the micro-parts.

[0004] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention

[0005] The purpose of the present disclosure is to provide a micro-part electroforming method and a micro-part, thereby overcoming the problem of poor electroforming effect of micro-parts at least to a certain extent.

[0006] According to a first aspect of the present disclosure, a method for electroforming a micro-part is provided, comprising: adding a metal source into an ionic liquid to obtain an electroforming liquid; wherein the ionic liquid contains choline chloride; using an electroforming core mold etched with a microstructure as a cathode and a metal sheet as an anode, immersing them in the electroforming liquid, and performing electroforming by electrodeposition; and taking out the cathode component after electroforming to obtain a micro-part.

[0007] Optionally, the ionic liquid further comprises ethylene glycol, and the molar ratio of choline chloride to ethylene glycol is 1:1 to 1:5; or the ionic liquid further comprises urea, and the molar ratio of choline chloride to urea is 1:2 to 1:4.

[0008] Optionally, the ionic liquid further comprises an organic solvent; wherein the organic solvent is any one of malic acid, oxalic acid and myristic acid.

[0009] Optionally, the metal source is one or more metal sources selected from nickel, iron and copper.

[0010] Optionally, adding a metal source into the ionic liquid to obtain an electroforming liquid comprises: adding the metal source into the ionic liquid and stirring the mixture uniformly at a temperature of 80° C. to 100° C. to obtain the electroforming liquid.

[0011] Optionally, the material of the electroforming core mold is any one of metal, ceramic, and organic matter.

[0012] Optionally, the electroforming includes direct current electroforming or pulse electroforming, and the current density of the electroforming is 0.5 mA / cm 2 Up to 10mA / cm 2 , the potential range of electroforming is -0.1V to -10V.

[0013] Optionally, taking out the cathode component after electroforming to obtain a micro-part includes: taking out the cathode component after electroforming, placing the cathode component in deionized water for ultrasonic cleaning and drying; and demolding the cathode component to obtain a micro-part.

[0014] Optionally, demolding the cathode component to obtain a micro-part includes: demolding the cathode component to obtain an intermediate part; post-processing the intermediate part to obtain the micro-part; wherein the post-processing includes a low-temperature heat treatment process and a surface polishing process.

[0015] According to a second aspect of the present disclosure, a micro-part is provided. The micro-part is manufactured by any of the above-mentioned micro-part electroforming methods.

[0016] In the scheme of the exemplary embodiment of the present disclosure, choline chloride type ionic liquid is used as the electroforming liquid, which overcomes the high preparation cost of the traditional water-based electroforming liquid, the product is harmful to the environment, the process is complicated, and the structural defects caused by the hydrogen evolution reaction, and has the advantages of being simple and efficient, safe and non-toxic, and low cost. In addition, the electroforming forming scheme of the present disclosure can improve the forming accuracy and performance of metal micro parts, and can realize the short process and low cost preparation of metal micro parts with high surface quality.

[0017] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0019] Figure 1The flowchart of the micro-part electroforming method according to the exemplary embodiment of the present disclosure is schematically shown.

[0020] Figure 2 A schematic diagram of the size and morphology of the copper gear prepared in Example 1 of the present disclosure is shown.

[0021] Figure 3 A schematic diagram of the tooth shape of the nickel micro-gear prepared in Example 2 of the present disclosure is shown.

[0022] Figure 4 A schematic diagram of the microscopic morphology of the nickel-iron alloy microfluidic channel prepared in Example 3 of the present disclosure is shown. DETAILED DESCRIPTION

[0023] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, processes, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.

[0024] In addition, the accompanying drawings are only schematic illustrations of the present disclosure and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated descriptions will be omitted. The flowcharts shown in the accompanying drawings are only exemplary illustrations and do not necessarily include all the steps. For example, some steps can also be decomposed, while some steps can be combined or partially combined, so the actual execution order may change according to the actual situation.

[0025] Ionic liquid (also known as room temperature molten salt) refers to an organic liquid substance composed entirely of ions at room temperature and adjacent temperatures. Due to the excellent properties of ionic liquids such as wide electrochemical window, low melting point, non-volatility, non-flammability, good thermal stability, and wide liquid range, it can not only deposit alkali metals, alkaline earth metals, refractory metals, etc. that are difficult to deposit in traditional aqueous solutions, but also avoid defects such as pinholes and pitting caused by hydrogen evolution reactions during water-based electrodeposition. Therefore, ionic liquids are considered to be ideal solvents for electrodeposited alloys. However, ionic liquids are sensitive to air and water, and must be operated under vacuum and inert gas protection. The synthesis process is complicated and the production cost is high, so they are subject to certain restrictions in actual production. In addition, since the viscosity of ionic liquids is greater than that of water-based electroforming liquids, the liquid phase mass transfer efficiency in the microcavity of the core mold during electrodeposition is limited, and the growth rate of the casting layer is low.

[0026] Choline chloride ionic liquid, as a new type of ionic liquid, not only has the advantages of traditional ionic liquids, but also has a simple preparation process, low-cost raw materials, is green and non-toxic, and can exist stably in the air environment.

[0027] In view of this, an embodiment of the present disclosure provides a micro-part electroforming solution based on choline chloride-based ionic liquid.

[0028] It should be noted that the micro parts mentioned in the embodiments of the present disclosure are parts corresponding to the micro electroforming technology, which may refer to parts with a scale below the millimeter level. The present disclosure does not limit the specific size of the micro parts involved.

[0029] Figure 1 The flowchart of the method for electroforming a micro-part according to an exemplary embodiment of the present disclosure is schematically shown. Figure 1 The micro-part electroforming method of the embodiment of the present disclosure comprises the following steps:

[0030] S12. Adding a metal source into an ionic liquid to obtain an electroforming solution; wherein the ionic liquid comprises choline chloride.

[0031] In an exemplary embodiment of the present disclosure, the ionic liquid further comprises ethylene glycol, and the molar ratio of choline chloride to ethylene glycol is 1:1 to 1:5; or the ionic liquid further comprises urea, and the molar ratio of choline chloride to urea is 1:2 to 1:4.

[0032] According to some embodiments of the present disclosure, the ionic liquid may further include an organic solvent, and the organic solvent may be any one of malic acid, oxalic acid, and myristic acid.

[0033] The ionic liquid mentioned in the present disclosure can be pre-configured or specially configured when executing the micro-part electroforming method of the present disclosure, and the present disclosure does not impose any limitation on this.

[0034] The metal source may be one or more of nickel, iron, and copper. In the embodiment of the present disclosure, the metal source may be added to the ionic liquid in the form of a metal salt, such as one or more of nickel chloride, cupric chloride, and ferrous chloride.

[0035] The present disclosure does not limit the concentration of the metal source. For example, the concentration range may be 0.1 mol / L to 0.5 mol / L.

[0036] Specifically, a metal source is added into the ionic liquid, and stirred evenly at a temperature of 80° C. to 100° C. until dissolved, so as to obtain an electroforming solution for electrodepositing metal.

[0037] S14. The electroforming core mold etched with a microstructure is used as a cathode and the metal sheet is used as an anode, immersed in the electroforming liquid, and electroforming is performed by electrodeposition.

[0038] In the exemplary embodiments of the present disclosure, the microstructure may include various regular and irregular structures such as tooth-shaped structures and microchannel structures, which are not limited in the present disclosure. The material of the electroforming core mold may be any one of metal, ceramic, and organic matter.

[0039] It is understandable that, in the electroforming process, the electroforming mandrel is usually inserted into (or bound to) a metal wire and fixed as a cathode, and the present disclosure does not limit the association between the electroforming mandrel and the metal wire.

[0040] In addition, the embodiments of the present disclosure do not limit the type of metal sheet, which can be a combination of one or more of copper sheets, nickel sheets, and iron sheets. It can be understood that this combination of metal sheets can include configurations such as series connection and parallel connection.

[0041] According to some embodiments of the present disclosure, electroforming may include direct current electroforming or pulse electroforming, and the current density of electroforming is 0.5 mA / cm 2 Up to 10mA / cm 2 , the potential range of electroforming is -0.1V to -10V.

[0042] S16. Take out the cathode component after electroforming to obtain a micro part.

[0043] According to some embodiments of the present disclosure, first, the cathode component after electroforming can be taken out, and the cathode component can be placed in deionized water for ultrasonic cleaning and drying.

[0044] Next, the cathode component is demolded to obtain a micro-part. Specifically, the dried electroformed component can be taken out by manual demolding, and the demolded component is recorded as an intermediate component. The intermediate component is then post-processed to obtain a finished micro-part. The present disclosure does not limit the post-processing process, for example, it can include a low-temperature heat treatment process and a surface polishing process.

[0045] The present invention places an electroforming core mold etched with a microstructure into a choline chloride type ionic liquid electroforming solution for electroforming. Compared with the traditional water-based electroforming solution, the choline chloride type ionic liquid has the advantages of simple process, no need for additives, long-term stability and reusability of the electroforming solution, no harmful intermediates in the electrodeposition process, and environmental friendliness. In the preparation process of the present invention, by replacing the traditional water-based electroforming solution with a choline chloride type ionic liquid electroforming solution, the surface defects caused by hydrogen embrittlement caused by hydrogen evolution can be effectively avoided, thereby further improving the forming accuracy and performance of metal micro parts.

[0046] The micro-part electroforming method disclosed in the present invention is described below through specific embodiments.

[0047] Example 1

[0048] First, 0.5 mol / L copper chloride was added to the ionic liquid prepared by choline chloride and urea, and the choline chloride and urea were mixed in a molar ratio of 1:3, and stirred for 3 hours at a temperature of 80°C until the solution was uniform and transparent, thereby obtaining a choline chloride-type ionic liquid electroplating solution for electrodepositing metallic copper.

[0049] Next, the titanium alloy electroforming core mold etched with a gear structure was fixed as the cathode, and then immersed in the copper chloride choline type ionic liquid electroforming solution, and a copper sheet with a mass purity greater than 99% was selected as the anode, and micro-electroforming was performed using an electrochemical workstation. The temperature for micro-electroforming using direct current was 80°C and the voltage was -0.45V.

[0050] Then, after the micro-electroforming is completed, the cathode component after micro-electroforming is taken out and ultrasonically cleaned in deionized water and dried in an oven. Finally, the blown-dried electrodeposited component, i.e., the metal copper micro-part, is taken out by manual demoulding. The required metal copper gear product is obtained after annealing at 300°C and surface polishing.

[0051] Figure 2 The metal copper gear diagram prepared in Example 1 is Figure 2 It can be seen that the metal copper gear with a diameter of about 5 mm prepared in Example 1 has a smooth surface morphology and an obvious metallic luster, which proves that the method disclosed in the present invention is controllable, has high forming accuracy and good forming quality.

[0052] Example 2

[0053] First, 0.1 mol / L nickel chloride was added to the ionic liquid prepared by choline chloride and ethylene glycol, and the mixture was mixed at a molar ratio of 1:2 with choline chloride and ethylene glycol, and stirred for 3 hours at a temperature of 100°C until the solution was uniform and transparent, thereby obtaining a choline chloride-type ionic liquid electroplating solution for electrodepositing metallic nickel.

[0054] Next, the surface-plated gold-plated ceramic core mold with micro-tooth profile structure etched on it was fixed as the cathode, and then immersed in the nickel chloride choline type ionic liquid electroforming solution. A nickel sheet with a purity greater than 99% was selected as the anode, and micro-electroforming was performed using an electrochemical workstation. The temperature for micro-electroforming with direct current was 100°C and the current density was 2 mA / cm 2 .

[0055] Then, after the micro-electroforming is completed, the cathode component after micro-electroforming is taken out and ultrasonically cleaned in deionized water and dried in an oven. Finally, the dried electrodeposited component, i.e., the metal nickel micro-part, is taken out by manual demoulding. Annealing treatment is performed at 200°C for 60 minutes in a muffle furnace to eliminate the residual stress in the metal nickel micro-part, and then the surface is polished to obtain the desired metal nickel micro-gear product.

[0056] Figure 3 This is a structural diagram of a nickel micro-gear with a tooth width of about 100 μm prepared in Example 2. It can be seen from the figure that the nickel gear structure is complete and has no defects, and has good replication forming accuracy.

[0057] Example 3

[0058] First, 0.3 mol / L nickel chloride and 0.1 mol / L ferrous chloride were added to the ionic liquid prepared by choline chloride and ethylene glycol, and the molar ratio of choline chloride and ethylene glycol was 1:2. The mixture was stirred at 100 °C for 3 h until the solution was uniform and transparent, and the electrodeposited Ni 75 Fe 25 Choline chloride type ionic liquid electroforming solution for alloys.

[0059] Next, the conductive organic electroforming core mold etched with a microchannel structure is fixed as the cathode, and then immersed in a nickel-iron alloy choline chloride type ionic liquid electroforming solution. A nickel sheet and an iron sheet with a mass purity greater than 99% are selected with an area of ​​3:1 as the anode, and micro-electroforming is performed using an electrochemical workstation. It is understandable that at this time, the nickel sheet and the iron sheet can be connected in parallel through wires. The temperature for micro-electroforming using direct current is 100°C and the current density is 10mA / cm 2 .

[0060] Then, after the micro-electroforming is completed, the cathode component after micro-electroforming is taken out and placed in deionized water for ultrasonic cleaning and placed in an oven for drying. Finally, the dried electrodeposited component, i.e., Ni 75 Fe 25 The alloy microchannel was taken out and annealed in a muffle furnace at 300°C for 60 min to eliminate Ni 75 Fe 25 The residual stress in the alloy microchannel is then polished to obtain the required Ni 75 Fe 25 Finished alloy microfluidic channel.

[0061] Figure 4 The Ni with line width ranging from 200 μm to 100 μm prepared in Example 3 75 Fe 25 Alloy microfluidic parts, as can be seen from the figure Ni 75 Fe 25 The alloy microfluidic parts have a complete structure without defects and have good replication forming accuracy.

[0062] Furthermore, the disclosed embodiment also provides a micro-part, which is prepared by the above-mentioned micro-part electroforming method.

[0063] It should be noted that although the steps of the method in the present disclosure are described in a specific order in the drawings, this does not require or imply that the steps must be performed in this specific order, or that all the steps shown must be performed to achieve the desired results. Additionally or alternatively, some steps may be omitted, multiple steps may be combined into one step, and / or one step may be decomposed into multiple steps, etc.

[0064] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.

[0065] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing what is disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary technical means in the art that are not disclosed in the present disclosure. The specification and embodiments are to be considered merely as exemplary, and the true scope and spirit of the present disclosure are indicated by the claims.

[0066] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.

Claims

1. A method for electroforming micro parts, It is characterized in that include: Adding a metal source into an ionic liquid to obtain an electroforming solution; wherein the ionic liquid comprises choline chloride; The electroforming core mold etched with microstructures is used as a cathode and the metal sheet is used as an anode, and the two are immersed in the electroforming liquid to perform electroforming by electrodeposition; The cathode member after electroforming is taken out to obtain a micro-part.

2. The micro-part electroforming method according to claim 1, It is characterized in that The ionic liquid further comprises ethylene glycol, and the molar ratio of choline chloride to ethylene glycol is 1:1 to 1:5; or The ionic liquid further comprises urea, and the molar ratio of choline chloride to urea is 1:2 to 1:

4.

3. The micro-part electroforming method according to claim 1, It is characterized in that The ionic liquid further comprises an organic solvent; Wherein, the organic solvent is any one of malic acid, oxalic acid and myristic acid.

4. The micro-part electroforming method according to claim 1, It is characterized in that The metal source is one or more metal sources selected from nickel, iron and copper.

5. The micro-part electroforming method according to any one of claims 1 to 4, It is characterized in that Adding a metal source to an ionic liquid to obtain an electroforming solution includes: The metal source is added into the ionic liquid and stirred uniformly at a temperature of 80° C. to 100° C. to obtain an electroforming solution.

6. The micro-part electroforming method according to claim 1, It is characterized in that The material of the electroforming core mold is any one of metal, ceramic and organic matter.

7. The micro-part electroforming method according to claim 1, It is characterized in that The electroforming includes direct current electroforming or pulse electroforming, and the current density of the electroforming is 0.5 mA / cm 2 Up to 10mA / cm 2 , the potential range of electroforming is -0.1V to -10V.

8. The micro-part electroforming method according to claim 1, It is characterized in that The cathode component after electroforming is taken out to obtain micro parts, including: Taking out the electroformed cathode component, placing the cathode component in deionized water for ultrasonic cleaning and drying; The cathode member is demolded to obtain a micro-part.

9. The micro-part electroforming method according to claim 8, It is characterized in that Demolding the cathode component to obtain a micro-part comprises: demoulding the cathode component to obtain an intermediate part; Post-processing the intermediate part to obtain a micro-part; Wherein, the post-processing includes a low-temperature heat treatment process and a surface polishing process.

10. A micro part, It is characterized in that The micro-part is prepared by the micro-part electroforming method as described in any one of claims 1 to 9.