Coated cutting tool and cutting tool
By employing a cubic crystal-based coating heat treatment and a stacked structure design in coated cutting tools, the problem of short tool life was solved, and the wear resistance and adhesion resistance at different cutting speeds were improved, thus extending the tool life.
Patent Information
- Application Number
- CN202380030061.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-31
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-03-31
AI Technical Summary
Existing coated cutting tools have a short lifespan in cutting operations, especially in high-speed and low-speed machining where their wear resistance and adhesion resistance are insufficient, making it difficult to meet the requirements for long lifespan.
The coating layer composed of cubic crystals is heat-treated in a non-oxidizing atmosphere to form a hexagonal crystal orientation ratio that satisfies Ih(100)/Ih(002)≤0.9. Combined with a Ta and Mo-containing stacked structure, the bonding between the substrate and the coating layer is improved through an intermediate layer, and the thickness and composition ratio of the stacked structure are controlled.
It extends the life of coated tools in high-speed and low-speed machining, improves wear resistance and adhesion resistance, reduces the risk of coating hardness reduction and peeling, and enhances toughness and strength at high temperatures.
Smart Images

Figure CN118922266B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to coated cutting tools and cutting tools. Background Technology
[0002] As cutting tools used in cutting processes such as turning or milling, coated tools are known to improve wear resistance and other properties by applying a coating layer to the surface of a substrate such as cemented carbide, cermet, or ceramic.
[0003] Existing technical documents
[0004] Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 2002-3284 Summary of the Invention
[0006] A coated cutting tool according to one aspect of the present invention comprises: a substrate; and a coating layer located on the substrate and composed of cubic crystals. The X-ray diffraction spectrum of the coating layer, measured after being held at 1200°C for 0.5 hours in a non-oxidizing atmosphere, satisfies the relationship Ih(100) / Ih(002) ≤ 0.9. Ih(100) is the intensity of the diffraction peak corresponding to the (100) plane of the hexagonal crystal formed in the coating layer. Ih(002) is the intensity of the diffraction peak corresponding to the (002) plane of the hexagonal crystal. Attached Figure Description
[0007] Figure 1 This is a perspective view showing an example of a coated cutting tool according to an embodiment.
[0008] Figure 2 This is a side sectional view illustrating an example of a coated cutting tool according to an embodiment.
[0009] Figure 3 This is a schematic diagram illustrating an example of an X-ray diffraction spectrum measured for a coating layer of an embodiment.
[0010] Figure 4 This is a cross-sectional view illustrating an example of the coating layer in an embodiment.
[0011] Figure 5 This is a cross-sectional view showing an example of a Ta-containing laminated structure and a Mo-containing laminated structure constituting the coating layer of the embodiment.
[0012] Figure 6 This is a cross-sectional view showing an example of a first compound layer and a second compound layer constituting a Ta-containing layered structure.
[0013] Figure 7 This is a cross-sectional view showing an example of the third and fourth compound layers constituting a Mo-containing laminated structure.
[0014] Figure 8 This is a schematic diagram illustrating an example of a film-forming apparatus for forming a coating layer on a substrate.
[0015] Figure 9 This is a front view showing an example of a cutting tool according to an embodiment.
[0016] Figure 10 This is a table showing the manufacturing conditions for the coating layer formed on the substrate.
[0017] Figure 11 This is a table showing the structure of the coating layer formed on the substrate.
[0018] Figure 12A This is a graph showing the X-ray diffraction spectrum of the coated tool for sample No.1 after heat treatment.
[0019] Figure 12B This is a graph showing the X-ray diffraction spectrum of the coated tool for sample No. 2 after heat treatment.
[0020] Figure 12C This is a graph showing the X-ray diffraction spectrum of the coated tool for sample No. 3 after heat treatment.
[0021] Figure 12D This is a graph showing the X-ray diffraction spectrum of the coated tool for sample No. 4 after heat treatment.
[0022] Figure 13 This is a table showing the results of X-ray diffraction spectrum measurements and cutting tests on coated cutting tools for samples No.1 to No.4. Detailed Implementation
[0023] Hereinafter, embodiments (hereinafter referred to as "Embodiments") for implementing the coated cutting tools and cutting tools based on the present invention will be described in detail with reference to the accompanying drawings. The coated cutting tools and cutting tools based on the present invention are not limited by these embodiments. Various embodiments can be appropriately combined without contradicting the intended content. In the following embodiments, the same reference numerals are used to label the same parts, and repeated descriptions are omitted.
[0024] In the embodiments shown below, expressions such as "constant," "orthogonal," "perpendicular," or "parallel" may be used, but these expressions need not be strictly "constant," "orthogonal," "perpendicular," or "parallel." That is, the above expressions, for example, allow for deviations in manufacturing precision or setting precision.
[0025] As cutting tools used in cutting processes such as turning or milling, coated tools are known to improve wear resistance and other properties by applying a coating layer to the surface of a substrate such as cemented carbide, cermet, or ceramic.
[0026] In the aforementioned prior art, there is room for further improvement in extending tool life.
[0027] Therefore, there is a growing expectation for a technology that can overcome the aforementioned problems and extend the life of cutting tools.
[0028] Coated Cutting Tools
[0029] Figure 1 This is a perspective view illustrating an example of a coated cutting tool according to an embodiment. Additionally, Figure 2 This is a side sectional view illustrating an example of the coated cutting tool 1 according to an embodiment. Figure 1 As shown, the coated cutting tool 1 of the embodiment has a blade body 2.
[0030] (Blade Body 2)
[0031] The blade body 2, for example, has an upper surface and a lower surface ( Figure 1 The shape of the surface intersecting the Z-axis shown is a parallelogram-shaped hexahedron.
[0032] One corner of the blade body 2 functions as a cutting edge. The cutting edge has a first surface (e.g., an upper surface) and a second surface (e.g., a side surface) connected to the first surface. In this embodiment, the first surface functions as a "rake face" to scrape away chips generated by cutting, and the second surface functions as a "flank face". At least a portion of the edge where the first and second surfaces intersect is provided with a cutting edge, and the coated tool 1 cuts the workpiece by pressing this cutting edge against it.
[0033] A through hole 5 is provided in the center of the blade body 2, extending vertically through the blade body 2. A screw 75 for mounting the coated tool 1 to the tool holder 70 described later is inserted into the through hole 5 (see reference). Figure 9 ).
[0034] like Figure 2 As shown, the blade body 2 has a substrate 10 and a coating layer 20.
[0035] (Matrix 10)
[0036] The matrix 10 is formed, for example, of a cemented carbide. The cemented carbide contains W (tungsten), specifically WC (tungsten carbide). The cemented carbide may also contain Ni (nickel) or Co (cobalt). Specifically, the matrix 10 is composed of a WC-based cemented carbide in which WC particles are the hard phase component and Co is the main component of the binder phase.
[0037] The matrix 10 can also be formed of cermet. Cermets may contain, for example, Ti (titanium), specifically TiC (titanium carbide) or TiN (titanium nitride). Cermets may also contain Ni or Co.
[0038] The matrix 10 may also be formed from a cubic boron nitride sintered body containing cubic boron nitride (cBN) particles. The matrix 10 is not limited to cubic boron nitride (cBN) particles, and may also contain hexagonal boron nitride (hBN), rhombohedral boron nitride (rBN), or wurtzite boron nitride (wBN) particles.
[0039] The matrix 10 can also be formed of ceramic. The ceramic may contain, for example, Al₂O₃ (aluminum oxide), such as K-Al₂O₃ and α-Al₂O₃. The ceramic may also contain elements other than aluminum oxide. For example, in addition to aluminum oxide, the ceramic may also contain at least one of magnesium (Mg), calcium (Ca), strontium (Sr), silicon (Si), and a Group 3 element of the periodic table.
[0040] (Coating layer 20)
[0041] The coating layer 20 is applied to the substrate 10 for purposes such as improving its wear resistance and heat resistance. Figure 2 In this example, the coating layer 20 completely covers the substrate 10. The coating layer 20 may be located at least on the substrate 10. When the coating layer 20 is located on the first surface (here, the upper surface) of the substrate 10, the first surface has higher wear resistance and heat resistance. When the coating layer 20 is located on the second surface (here, the side surface) of the substrate 10, the second surface has higher wear resistance and heat resistance.
[0042] Here, refer to Figure 3 The specific characteristics of the coating layer 20 are described. Figure 3 This diagram schematically illustrates an example of an X-ray diffraction spectrum measured for the coating layer 20 of the embodiment. The coating layer 20 of the embodiment is composed of cubic crystals at a temperature of room temperature to 1000°C. The coated cutting tool 1 of the embodiment is subjected to heat treatment at a temperature of 1200°C for 0.5 hours in a non-oxidizing atmosphere. In the heat treatment, for example, a closed-type heating furnace (atmosphere furnace) can be used. As a non-oxidizing atmosphere, for example, neutral gases such as nitrogen or hydrogen, or inactive gases such as helium or argon can be used.
[0043] Such heat treatment causes a phase transformation from cubic to hexagonal crystals in the coating layer 20 constituting the embodiment. That is, the heat-treated coating layer 20 contains not only cubic crystals but also hexagonal crystals.
[0044] Next, the X-ray diffraction spectrum of the heat-treated coating 20 was measured using an X-ray diffractometer (XRD). Figure 3 As shown, the X-ray diffraction spectrum measured after heat treatment exhibits various diffraction peaks, including those corresponding to the (iii) plane of the cubic crystal, the (200) plane of the cubic crystal, the (100) plane of the hexagonal crystal, and the (002) plane of the hexagonal crystal. Figure 3 In the figure, c(111), c(200), h(100) and h(002) are used to show the diffraction peak corresponding to the (iii) plane of the cubic crystal, the diffraction peak corresponding to the (200) plane of the cubic crystal, the diffraction peak corresponding to the (100) plane of the hexagonal crystal and the diffraction peak corresponding to the (002) plane of the hexagonal crystal, respectively.
[0045] Regarding the coating layer 20 of the embodiment, the X-ray diffraction spectrum measured on the heat-treated coating layer 20 satisfies the relationship Ih(100) / Ih(002)≤0.9. Here, Ih(100) is the intensity of the diffraction peak corresponding to the (100) plane of the hexagonal crystal formed in the coating layer 20, and Ih(002) is the intensity of the diffraction peak corresponding to the (002) plane of the hexagonal crystal.
[0046] When the X-ray diffraction spectrum of the heat-treated coating layer 20 satisfies the relationship Ih(100) / Ih(002)≤0.9, the proportion of hexagonal crystals formed in the coating layer 20 that are oriented with the (002) face of the hexagonal crystal parallel to the surface of the substrate 10 on which the coating layer 20 is disposed (the direction of the c-axis of the hexagonal crystal is perpendicular to the surface of the substrate 10) (hereinafter referred to as "first-oriented hexagonal crystals") is greater than the proportion of hexagonal crystals that are oriented with the (100) face of the hexagonal crystal parallel to the surface of the substrate 10 (the direction of the c-axis of the hexagonal crystal is parallel to the surface of the substrate 10) (hereinafter referred to as "second-oriented hexagonal crystals").
[0047] The hexagonal crystals with the first orientation tend to slide on the (002) plane, while those with the second orientation tend to slide on the (100) plane. Here, the (002) plane of the hexagonal crystal is more prone to sliding against the (100) plane than the (100) plane. Therefore, it is believed that when the proportion of hexagonal crystals with the first orientation is greater than that with the second orientation, sliding on the (002) plane is more likely to occur. As a result, it is believed that damage caused by adhesion to the workpiece (such as film peeling and chipping caused by the detachment of the bonded portion) can be minimized, thereby improving the adhesion resistance and chipping resistance of the coating layer 20.
[0048] It is believed that when the workpiece is cut using the coated tool 1 of the embodiment, the strain of the hexagonal crystal with the first orientation is smaller than that of the hexagonal crystal with the second orientation. Therefore, it is believed that when the proportion of the hexagonal crystal with the first orientation is larger than that of the hexagonal crystal with the second orientation, the decrease in hardness of the coating layer 20 can be reduced. As a result, it is believed that the wear resistance of the coating layer 20 can be improved.
[0049] Thus, when the X-ray diffraction spectrum of the heat-treated coating 20 satisfies the relationship Ih(100) / Ih(002)≤0.9, the life of the coated tool 1 can be extended.
[0050] In high-speed machining, the temperature of the coated tool 1 is around 1200°C. Therefore, it is considered that heat treatment of holding the coating layer 20 at 1200°C for 0.5 hours in a non-oxidizing atmosphere corresponds to high-speed machining (machining at a cutting speed of ~200 m / min) performed by the coated tool 1. In high-speed machining, when the temperature of the coating layer 20, which is composed of cubic crystals, rises to around 1200°C, hexagonal crystals are generated in the coating layer 20. Generally, there is a tendency for the hardness and wear resistance of the coating layer to decrease as the proportion of hexagonal crystals increases. As a result, there is a tendency for the life of the coated tool to become shorter in high-speed machining. However, in the coated tool 1 of the embodiment, the X-ray diffraction spectrum measured on the heat-treated coating layer 20 satisfies the relationship Ih(100) / Ih(002)≤0.9, thereby reducing the decrease in wear resistance of the coating layer 20 in high-speed machining and improving the coating layer 20's resistance to adhesion and chipping relative to the workpiece.
[0051] On the other hand, during low-speed machining, the temperature of the coated tool 1 is between room temperature and 1000°C. In this case, the coating layer 20 is composed of cubic crystals, thus maintaining the hardness and wear resistance of the coating layer 20. Furthermore, by using the structure of the coating layer 20, where the X-ray diffraction spectrum measured after heat treatment satisfies the relationship Ih(100) / Ih(002)≤0.9 (described later), the hardness and toughness of the coating layer 20 can be improved. As a result, the wear resistance of the coating layer 20 can be improved during low-speed machining.
[0052] Thus, when the X-ray diffraction spectrum measured on the heat-treated coating 20 satisfies the relationship Ih(100) / Ih(002)≤0.9, the life of the coated tool 1 can be extended in both low-speed and high-speed machining.
[0053] The X-ray diffraction spectrum measured on the heat-treated coating 20 sometimes satisfies the relationship Ih(100) / Ih(002)≤0.3. In this case, the proportion of hexagonal crystals with the first orientation can be further increased. As a result, the life of the coated tool 1 can be further extended.
[0054] Here, refer to Figure 4 , Figure 5 , Figure 6 as well as Figure 7 To illustrate the specific structure of the coating 20, the X-ray diffraction spectrum of the heat-treated coating 20 is measured to satisfy the relationship Ih(100) / Ih(002)≤0.9. Figure 4 This is a cross-sectional view showing an example of the coating layer 20 of the embodiment. Figure 5 This is a cross-sectional view showing an example of a Ta-containing laminated structure and a Mo-containing laminated structure constituting the coating layer 20 of the embodiment. Figure 6 This is a cross-sectional view showing an example of a first compound layer and a second compound layer constituting a Ta-containing layered structure. Figure 7 This is a cross-sectional view showing an example of the third and fourth compound layers constituting a Mo-containing laminated structure.
[0055] like Figure 4 As shown, the coating layer 20 includes a plurality of Ta-containing stacked structures 22 and a plurality of Mo-containing stacked structures 23 located above the intermediate layer 21. Each of the plurality of Ta-containing stacked structures 22 is a stacked structure containing at least Ta. Each of the plurality of Mo-containing stacked structures 23 is a stacked structure containing at least Mo.
[0056] like Figure 4 As shown, multiple Ta-containing stacked structures 22 and multiple Mo-containing stacked structures 23 are sometimes alternately stacked within the coating layer 20.
[0057] In this case, the residual stress between the Ta-containing laminated structure 22 and the Mo-containing laminated structure 23 can be reduced. This reduces peeling or cracking between the Ta-containing laminated structure 22 and the Mo-containing laminated structure 23. Furthermore, the effects of the Ta-containing laminated structure 22 and the Mo-containing laminated structure 23, as described later, can be improved. As a result, the lifespan of the coated tool 1 can be extended.
[0058] The average thickness of each of the multiple Ta-containing stacked structures 22 and the multiple Mo-containing stacked structures 23 is sometimes greater than 300 nm and less than 500 nm.
[0059] In this case, the residual stress between the Ta-containing laminated structure 22 and the Mo-containing laminated structure 23 can be reduced. This reduces peeling or cracking between the Ta-containing laminated structure 22 and the Mo-containing laminated structure 23. Furthermore, the effects of the Ta-containing laminated structure 22 and the Mo-containing laminated structure 23, as described later, can be improved. As a result, the lifespan of the coated tool 1 can be extended.
[0060] (Middle layer 21)
[0061] An intermediate layer 21 may also be disposed between the substrate 10 and the coating layer 20. Specifically, the intermediate layer 21 contacts the upper surface of the substrate 10 on one side (the lower surface in this case) and contacts the lower surface of the coating layer 20 (e.g., the Ta-containing laminate structure 22) on the other side (the upper surface in this case).
[0062] Compared to the coating layer 20, the intermediate layer 21 has a higher bonding strength with the substrate 10. Examples of metallic elements possessing this property include Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Si, Y, and Ti. The intermediate layer 21 contains at least one of the aforementioned metallic elements. For example, the intermediate layer 21 may also contain Ti. Si is a half-metal element, but in this specification, it is assumed that half-metal elements are also included among metallic elements.
[0063] When the intermediate layer 21 contains Ti, the Ti content in the intermediate layer 21 can be 1.5 atomic% or more. For example, the Ti content in the intermediate layer 21 can be 2.0 atomic% or more.
[0064] The intermediate layer 21 may also contain components other than the aforementioned metallic elements (Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Si, Y, and Ti). However, from the viewpoint of bonding with the substrate 10, the intermediate layer 21 may also contain at least 95 atomic percent of the aforementioned metallic elements in total. The intermediate layer 21 may also contain at least 98 atomic percent of the aforementioned metallic elements in total. The proportion of metallic components in the intermediate layer 21 can be determined, for example, by analysis using an EDS (energy-dispersive X-ray spectrometer) attached to a STEM (scanning transmission electron microscope).
[0065] In this way, by placing an intermediate layer 21, which has a higher wettability to the substrate 10 than the coating layer 20, between the substrate 10 and the coating layer 20, the adhesion between the substrate 10 and the coating layer 20 can be improved. The adhesion between the intermediate layer 21 and the coating layer 20 is also high, so it is difficult for the coating layer 20 to peel off from the intermediate layer 21.
[0066] The thickness of the intermediate layer 21 can be, for example, greater than 0.1 nm and less than 20 nm.
[0067] (Including Ta-layered structures 22)
[0068] like Figure 5 As shown, each of the multiple Ta-containing layered structures 22 includes a first compound layer 22a and a second compound layer 22b. The first compound layer 22a contains Ta in a first composition ratio. The second compound layer 22b contains Ta in a second composition ratio different from the first composition ratio. It should be noted that either the first composition ratio or the second composition ratio may sometimes be 0.
[0069] In this way, by having multiple Ta-containing laminated structures 22 each comprising a first compound layer 22a containing Ta in a first composition ratio and a second compound layer 22b containing Ta in a second composition ratio different from the first composition ratio, the thermal shock resistance, oxidation resistance, and high-temperature hardness of the coating layer 20 can be improved. As a result, the life of the coated tool 1 can be extended.
[0070] The first compound layer 22a and the second compound layer 22b may each contain Al, Ti, and Ta. In this case, the contents of Al in the first compound layer 22a (Al(1), Ti in the first compound layer 22a (Ti(1), Ta in the first compound layer 22a (Ta(1), Al in the second compound layer 22b (Al(2), Ti in the second compound layer 22b (Ti(2), Ta(1), Ta(2))) sometimes have the relationship Al(1) < Al(2), Ti(1) < Ti(2), and Ta(1) > Ta(2). Ta(2) is sometimes 0.
[0071] When Al(1), Ti(1), Ta(1), Al(2), Ti(2), and Ta(2) have the relationships Al(1) < Al(2), Ti(1) < Ti(2), and Ta(1) > Ta(2), the residual stress between the first compound layer 22a and the second compound layer 22b can be reduced, while maintaining the hardness and adhesion of the first compound layer 22a and the second compound layer 22b. This reduces peeling or cracking between the first compound layer 22a and the second compound layer 22b and increases the strength of the coating layer 20. As a result, the lifespan of the coated tool 1 can be extended.
[0072] The first compound layer 22a and the second compound layer 22b may each contain compounds derived from the formula...
[0073] (Al a Ti b Ta c )N (1)
[0074] (In the formula, a, b, and c satisfy the relationships 0.35≤a≤0.65, 0.3≤b≤0.5, 0.02≤c≤0.2, and a+b+c=1)
[0075] This indicates a Ta-containing compound.
[0076] When a satisfies the relationship 0.35≤a≤0.65, the hardness and wear resistance of the coating layer 20 can be maintained. When b and c satisfy the relationships 0.3≤b≤0.5 and 0.02≤c≤0.2, the oxidation resistance of the coating layer 20 can be maintained and the strength of the coating layer 20 at high temperatures can be improved. As a result, the life of the coated tool 1 can be extended.
[0077] like Figure 6 As shown, the value of c for the Ta-containing compound contained in the first compound layer 22a can also vary continuously in the thickness direction of the first compound layer 22a. Similarly, the value of c for the Ta-containing compound contained in the second compound layer 22b can also vary continuously in the thickness direction of the second compound layer 22b. For example, as... Figure 6 As shown, the value of c for the Ta-containing compound contained in the first compound layer 22a can be extremely large near the center of the distance in the thickness direction of the first compound layer 22a. Similarly, the value of c for the Ta-containing compound contained in the second compound layer 22b can be extremely small near the center of the distance in the thickness direction of the second compound layer 22b.
[0078] In this case, the residual stress between the first compound layer 22a and the second compound layer 22b can be further reduced. This reduces peeling or cracking between the first compound layer 22a and the second compound layer 22b. As a result, the lifespan of the coated tool 1 can be extended.
[0079] (Including Mo-layered structures 23)
[0080] like Figure 5 As shown, each of the multiple Mo-containing layered structures 23 includes a third compound layer 23a and a fourth compound layer 23b. The third compound layer 23a contains Mo in a third composition ratio. The fourth compound layer 23b contains Mo in a fourth composition ratio different from the third composition ratio. Sometimes, either the third composition ratio or the fourth composition ratio is 0.
[0081] In this way, by having multiple Mo-containing laminated structures 23 each comprising a third compound layer 23a containing Mo in a third composition ratio and a fourth compound layer 23b containing Mo in a fourth composition ratio different from the third composition ratio, the toughness and strength of the coating layer 20 can be improved. Furthermore, the lubricity of the coating layer 20 can be maintained even at high temperatures. As a result, the lifespan of the coated tool 1 can be extended.
[0082] The third compound layer 23a and the fourth compound layer 23b may each contain Al, Cr, and Mo. In this case, the contents of Al (Al3) in the third compound layer 23a, the contents of Cr (Cr3) in the third compound layer 23a, the contents of Mo (Mo3) in the third compound layer 23a, the contents of Al (Al4) in the fourth compound layer 23b, the contents of Cr (Cr4) in the fourth compound layer 23b, and the contents of Mo (Mo4) in the fourth compound layer 23b sometimes have the relationships Al (3) < Al (4), Cr (3) > Cr (4), and Mo (3) > Mo (4). Mo (4) is sometimes 0.
[0083] When Al(3), Cr(3), Mo(3), Al(4), Cr(4), and Mo(4) have the relationships Al(3) < Al(4), Cr(3) > Cr(4), and Mo(3) > Mo(4), the residual stress between the third compound layer 23a and the fourth compound layer 23b can be reduced. This reduces peeling or cracking between the third compound layer 23a and the fourth compound layer 23b. Furthermore, the lubricity of the coating layer 20 can be maintained even at high temperatures, and the thermal shock resistance, strength, oxidation resistance, and high-temperature hardness of the coating layer 20 are further improved. As a result, the life of the coated tool 1 can be extended.
[0084] The third compound layer 23a and the fourth compound layer 23b may each contain compounds derived from the formula...
[0085] (Al d Cr e Si f Mo g )N (2)
[0086] (In the formula, d, e, f, and g satisfy the relationships 0.35≤d≤0.65, 0.2≤e≤0.45, 0.03≤f≤0.15, 0.02≤g≤0.2, and d+e+f+g=1)
[0087] The indicated compound contains Mo.
[0088] When d satisfies the relationship 0.35≤d≤0.65, the hardness and wear resistance of the coating layer 20 can be maintained. When e, f, and g satisfy the relationships 0.2≤e≤0.45, 0.03≤f≤0.15, and 0.02≤g≤0.2, the lubricity of the coating layer 20 at high temperatures can be maintained, and the thermal shock resistance, strength, and oxidation resistance of the coating layer 20 can be improved. As a result, the life of the coated tool 1 can be extended.
[0089] like Figure 7 As shown, g for the Mo-containing compound contained in the third compound layer 23a can also vary continuously in the thickness direction of the third compound layer 23a. Similarly, g for the Mo-containing compound contained in the fourth compound layer 23b can also vary continuously in the thickness direction of the fourth compound layer 23b. For example, as... Figure 7 As shown, g for the Mo-containing compound contained in the third compound layer 23a can be extremely large near the center of the distance in the thickness direction of the third compound layer 23a. g for the Mo-containing compound contained in the fourth compound layer 23b can be extremely small near the center of the distance in the thickness direction of the fourth compound layer 23b.
[0090] In this case, the residual stress between the third compound layer 23a and the fourth compound layer 23b can be further reduced. This reduces peeling or cracking between the third compound layer 23a and the fourth compound layer 23b. As a result, the lifespan of the coated tool 1 can be extended.
[0091] The average thickness of the first compound layer 22a, the second compound layer 22b, the third compound layer 23a, and the fourth compound layer 23b is sometimes greater than 3 nm and less than 15 nm.
[0092] In this case, the Ta-containing laminated structure 22, including the first compound layer 22a and the second compound layer 22b, is a laminated structure of multiple layers with a thickness on the nanometer scale. The Mo-containing laminated structure 23, including the third compound layer 23a and the fourth compound layer 23b, is a laminated structure of multiple layers with a thickness on the nanometer scale. This improves the strength of the coating layer 20 against external forces. Furthermore, it enhances the oxidation resistance and high-temperature hardness of the coating layer 20. As a result, it extends the lifespan of the coated tool 1.
[0093] <Manufacturing Method of Coated Cutting Tools>
[0094] Next, refer to Figure 8 An example of a method for manufacturing the coated cutting tool 1 according to the embodiment will be described. Figure 8This figure schematically illustrates an example of a film-forming apparatus for forming a coating layer on a substrate. It should be noted that the method for manufacturing the coated tool 1 is not limited to the method shown below.
[0095] First, a substrate 10 having the shape of the coated tool 1 is fabricated using conventionally known methods. Next, a coating layer 20 is formed on the surface of the substrate 10. As a method for forming the coating layer 20, physical vapor deposition (PVD) methods such as ion plating or sputtering can be used, for example. As an example, when fabricating the coating layer 20 using ion plating, for example, a method can be used... Figure 8 An arc ion plating apparatus (hereinafter referred to as an AIP apparatus) 1000 as shown.
[0096] Figure 8 The AIP device 1000 shown introduces a gas such as N2 or Ar into the vacuum chamber 101 through the gas inlet 102. A high voltage is applied between the cathode electrode 103 and the anode electrode 104 disposed in the AIP device 1000 to generate a gas plasma. Under the action of such plasma, the desired metal or ceramic is evaporated and ionized from the target material 105, generating high-energy metal or ceramic ions. The ionized metal or ceramic is then attached to the surface of the substrate 10, which serves as the sample, and a coating layer 20 is applied to the surface of the substrate 10.
[0097] like Figure 8 As shown, multiple substrates 10 can also be mounted on the tower 107 and placed on the sample support platform 106. Multiple sets (two sets in the figure) of sample support platforms 106 can also be placed on a workbench (not shown). Figure 8 As shown, a heater 108 for heating the substrate 10, a gas outlet 109 for discharging gas to the outside of the system, and a bias power supply 110 for applying a bias voltage to the substrate 10 are provided.
[0098] As the target material 105, for example, a metal target material containing tantalum (Ta), molybdenum (Mo), and one or more metals selected from Group V or Group VI elements of the periodic table, Si, Y, and Ce, an alloy target material that combines the above metals, or a mixture target material composed of powders or sintered bodies of carbides, nitrides, or borides of the above metals can be used.
[0099] While using the target material 105 to evaporate the metal source through arc discharge or glow discharge, thereby ionizing the metal source, it reacts with nitrogen (N2) gas from the nitrogen source, methane (CH4) / acetylene (C2H2) gas from the carbon source, or oxygen (O2) gas, thereby depositing a coating layer 20 on the surface of the substrate 10.
[0100] At this time, the sample support stage 106 is controlled such that the distance from the position of the target 105 to the position of the substrate 10 is 160 mm or more, preferably 260 mm or more. Multiple magnetic field lines with high straightness are generated from the center portion of the surface of the target 105 toward the substrate 10, so that the magnetic flux density near the substrate 10 is 0.2 to 0.8 mT (millitales).
[0101] Sometimes nitrogen gas is introduced into the AIP device 1000 as a reaction gas, and the atmosphere pressure is set to 2-10 Pa. The temperature of the substrate 10 is maintained at 300-500°C. A bias voltage of -50 to -200 V is applied to the substrate 10, generating an arc discharge of 80-200 A between the target 105 (cathode electrode 103) and the anode electrode 104. Metal is deposited onto the substrate 10 while it rotates and revolves.
[0102] As a method for controlling the magnetic flux density near the substrate 10, the magnetic field can be controlled by, for example, by setting an electromagnetic coil or permanent magnet as a magnetic field source around the target 105, placing a permanent magnet inside the AIP device 1000, for example, at the center, or adjusting the position of adjacent target 105.
[0103] The magnetic force is calculated by measuring the magnetic flux density at the location of the substrate 10 using a flux density meter. The magnetic flux density is expressed in mT (millitales). Here, the distance from the location of the target 105 to the location of the substrate 10 represents the distance measured at the location of the substrate 10 closest to the target 105 and the distance of the substrate 10 furthest from the target 105.
[0104] During film formation, in the process of... Figure 8 When the period of the orientation of the substrate 10 closest to the target 105 is set as the rotational speed of the sample, the period of the difference in composition between heavy and light metals in the thickness direction of the coating layer 20 can be adjusted by adjusting the rotational speed. Specifically, the rotational speed of the substrate 10 and the sample support stage 106 is sometimes adjusted in a period of 2 to 20 rpm.
[0105] During film formation, the sample support platform 106 carrying the substrate 10 can rotate simultaneously with the rotation of the tower 107, and the worktable can be rotated by the revolution of multiple sample support platforms 106. By adjusting the timing of such revolution, the thickness of each compound layer constituting the Ta-containing multilayer structure 22 and the Mo-containing multilayer structure 23 can be controlled.
[0106] By applying a pulsed bias voltage, the time or distance at which metal ions travel from the target 105 to the substrate 10 can be adjusted. This allows for the formation of a difference in composition between heavy and light metal components during film formation.
[0107] For example, when the substrate 10 is positioned close to and opposite the target 105, the heavy metal components from the target 105 flow straight towards the substrate 10, resulting in a higher accumulation of heavy metals than light metals in the substrate 10. On the other hand, when the substrate 10 is positioned away from and opposite the target 105, it is believed that the light metal components accumulate in a more circuitous manner in the substrate 10, thus reducing the accumulation of heavy metal components. In this case, it is believed that by maintaining a long distance from the target 105 to the substrate 10 and maintaining a certain level of magnetic flux density near the substrate 10, the circuitous movement of the light metal components is promoted, increasing the compositional difference between the heavy and light metal components.
[0108] <Cutting Tools>
[0109] Next, refer to Figure 9 The structure of the cutting tool having the above-described coated tool 1 will be described. Figure 9 This is a front view showing an example of a cutting tool according to an embodiment.
[0110] like Figure 9 As shown, the cutting tool 100 of the embodiment includes a coated tool 1 and a tool holder 70 for fixing the coated tool 1.
[0111] The handle 70 is from the first end ( Figure 9 The upper end of the middle) faces the second end ( Figure 9 A rod-shaped component extending from the lower end of the handle. The handle 70 is made of, for example, steel or cast iron. In particular, steel with higher toughness among these materials is sometimes used.
[0112] The tool holder 70 has a tool groove 73 at its first end. The tool groove 73 is for mounting the coated tool 1 and has a seat surface intersecting the rotation direction of the workpiece and a constraint side inclined relative to the seat surface. A threaded hole is provided on the seat surface for engaging the screw 75, which will be described later.
[0113] The coated cutting tool 1 is located in the tool slot 73 of the tool holder 70 and is mounted to the tool holder 70 by a screw 75. That is, the screw 75 is inserted into the through hole 5 of the coated cutting tool 1, and the front end of the screw 75 is inserted into the threaded hole formed on the seat surface of the tool slot 73 so that the screw parts are screwed together. Thus, the coated cutting tool 1 is mounted to the tool holder 70 in such a way that the cutting edge 3 protrudes outward from the tool holder 70.
[0114] In the embodiment, a cutting tool used in so-called turning is illustrated. Examples of turning include internal diameter machining, external diameter machining, and grooving. The cutting tool is not limited to those used in turning. For example, the coated tool 1 can also be used as a cutting tool in milling. Examples of cutting tools used in milling include end mills such as face mills, front end mills, side end mills, and grooving end mills, as well as end mills such as single-flute end mills, multi-flute end mills, tapered end mills, and ball end mills.
[0115] Example
[0116] The following is for reference Figures 10-13 The embodiments of the present invention will be described in detail below. The present invention is not limited to the embodiments shown below.
[0117] Figure 10 This is a table showing the manufacturing conditions for the coating layer formed on the substrate. Figure 11 This is a table showing the structure of the coating layer formed on the substrate.
[0118] exist Figure 8 In the AIP device shown, according to Figure 10 The manufacturing conditions shown allow for the formation of a coating layer on a substrate made of WC-based cemented carbide, thereby producing coated cutting tools of samples No. 1 to No. 4. That is, under the following manufacturing conditions... Figure 10 Under the conditions of the arc current (mA), target composition, distance between the target and the substrate (mm), magnetic flux density near the substrate (mT), and rotational speed (rpm) of the sample support stage, a coating layer was formed on the surface of the substrate. The distance between the target and the substrate (mm) varies depending on the rotation of the sample support stage. Figure 10 The values shown vary within the range. Correspondingly, the magnetic flux density (mT) near the matrix also varies. Figure 10 The values shown vary within the range.
[0119] For the coated cutting tools of samples No. 1 and No. 2, multiple Ta-containing laminated structures and multiple Mo-containing laminated structures were formed on the surface of the substrate. Here, the multiple Ta-containing laminated structures and multiple Mo-containing laminated structures were alternately stacked. For the coated cutting tool of sample No. 3, only multiple Mo-containing laminated structures were formed on the surface of the substrate. For the coated cutting tool of sample No. 4, only multiple Ta-containing laminated structures were formed on the surface of the substrate.
[0120] Here, on the surface of the substrate, with Figure 10The number of stacking operations shown indicates that groups of structures containing Ta and Mo were formed, groups of structures containing only Ta were formed, and groups of structures containing only Mo were formed. That is, the number of Ta-containing structures and the number of Mo-containing structures are respectively related to... Figure 10 The number of stacking operations shown is the same. Figure 10 During the stacking time (minutes) shown, Ta-containing stacked structures and Mo-containing stacked structures are formed on the surface of the matrix.
[0121] like Figure 11 As shown, for the coated cutting tools of samples No. 1 and No. 2, the Ta-containing laminated structure consists of a first compound layer and a second compound layer, and the Mo-containing laminated structure consists of a third compound layer and a fourth compound layer. For the coated cutting tool of sample No. 3, the Mo-containing laminated structure consists of a third compound layer and a fourth compound layer. For the coated cutting tool of sample No. 4, the Ta-containing laminated structure consists of a first compound layer and a second compound layer.
[0122] The first compound layer and the second compound layer each contain (Al) a Ti b Ta c N represents Ta-containing compounds. Here, a, b, and c are... Figure 11 The value shown. Figure 11 The values of a, b, and c shown are averages for the Ta-containing compounds contained in the multiple first compound layers or multiple second compound layers of a Ta-containing layered structure. The average composition of a Ta-containing layered structure composed of first and second compound layers is... Figure 10 The composition of the target material shown is consistent for manufacturing Ta-containing laminated structures.
[0123] like Figure 11 As shown, for the coated cutting tools of samples No.1 and No.2, the first compound layer a, the first compound layer b, the first compound layer c, the second compound layer a, the second compound layer b, and the second compound layer c have the following relationships: first compound layer a < second compound layer a, first compound layer b < second compound layer b, and first compound layer c > second compound layer c.
[0124] The third and fourth compound layers each contain (Al) d Cr e Si f Mo g ) represents a Mo-containing compound. Here, d, e, f, and g are... Figure 11 The value shown. Figure 11The values of d, e, f, and g shown are the average values for the Mo-containing compounds contained in the plurality of third compound layers or the plurality of fourth compound layers included in the Mo-containing layered structure. The average composition of the Mo-containing layered structure composed of the third compound layer and the fourth compound is the same as Figure 10 the composition of the target material for producing the Mo-containing layered structure as shown.
[0125] As Figure 11 shown, d of the third compound layer, e of the third compound layer, g of the third compound layer, d of the fourth compound layer, e of the fourth compound layer, and g of the fourth compound layer satisfy the relationships: d of the third compound layer < d of the fourth compound layer, e of the third compound layer > e of the fourth compound layer, and g of the third compound layer > g of the fourth compound layer.
[0126] Regarding the coated tools of Sample No. 1 and No. 2, the respective thicknesses of the Ta-containing layered structure and the Mo-containing layered structure are Figure 11 400 nm, which is the value of the thickness (nm) of each layered structure as shown. Regarding the coated tool of Sample No. 3, the thickness of the Mo-containing layered structure is Figure 11 4000 nm as shown. Regarding the coated tool of Sample No. 4, the thickness of the Ta-containing layered structure is Figure 11 4000 nm as shown.
[0127] Regarding the coated tools of Sample No. 1 and No. 2, the average thickness of the first compound layer, the second compound layer, the third compound layer, and the fourth compound layer is Figure 11 8 nm, which is the value of the average thickness (nm) of the compound layers as shown. Regarding the coated tool of Sample No. 3, the average thickness of the third compound layer and the fourth compound layer is Figure 11 8 nm as shown. Regarding the coated tool of Sample No. 4, the average thickness of the first compound layer and the second compound layer is Figure 11 8 nm as shown.
[0128] <X-ray diffraction spectrum>
[0129] The coated tools of Sample No. 1 to No. 4 were subjected to a heat treatment in which the coating layer was held at 1200°C for 0.5 hours in a nitrogen atmosphere. Thereafter, using an X-ray diffractometer "MiniFlex600" (manufactured by Rigaku Corporation), the X-ray diffraction spectrum of the heat-treated coating layer was measured. The optical system of the above X-ray diffractometer is a concentrated method optical system. The X-ray tube of the above X-ray diffractometer is Cu, with an output of 40 kV / 15 mA.
[0130] The conditions for measuring the X-ray diffraction spectrum are as follows.
[0131] Measurement method: 2θ scan
[0132] Measurement range: 30°C to 46°C
[0133] Steps: 0.01 degrees
[0134] Scanning speed: 2 degrees / minute
[0135] Figure 12A This is a graph showing the X-ray diffraction spectrum of the coated tool for sample No.1 after heat treatment. Figure 12B This is a graph showing the X-ray diffraction spectrum of the coated tool for sample No. 2 after heat treatment. Figure 12C This is a graph showing the X-ray diffraction spectrum of the coated tool for sample No. 3 after heat treatment. Figure 12D This is a graph showing the X-ray diffraction spectrum of the coated tool for sample No. 4 after heat treatment.
[0136] exist Figure 12A , Figure 12B , Figure 12C as well as Figure 12D In the diagram, the horizontal axis represents the X-ray diffraction angle of 20 degrees, and the vertical axis represents the X-ray intensity (in arbitrary units). θ is the Bragg angle of the X-rays (in degrees).
[0137] exist Figure 12A , Figure 12B , Figure 12C as well as Figure 12D In the above, the diffraction peaks in the range of 33° to 34° correspond to the (100) plane of the hexagonal crystal of the metal nitride contained in the heat-treated coating. The diffraction peaks in the range of 36.3° to 36.5° correspond to the (002) plane of the hexagonal crystal mentioned above.
[0138] about Figure 12A , Figure 12B , Figure 12C as well as Figure 12D The X-ray diffraction spectra shown yielded the intensities Ih(100) of the diffraction peak corresponding to the (100) plane of the hexagonal crystal and Ih(002) of the diffraction peak corresponding to the (002) plane of the hexagonal crystal. The ratio Ih(100) / Ih(002) was calculated based on the obtained Ih(100) and Ih(002).
[0139] <Cutting Test>
[0140] Cutting tests were conducted on the coated cutting tools of test samples No.1 to No.4. The test conditions for the cutting tests are as follows. Using a milling hard material type (model: PNMU1205ANER-GM) as the substrate, cutting tests were conducted under the following conditions.
[0141] (1) Cutting method: Milling of square bars with dimensions of 80mm×125mm×300mm.
[0142] (2) Workpiece to be cut: FCD450
[0143] (3) Cutting speed Vc: 150 m / min and 200 m / min
[0144] (4) Feed rate fz for each cutting edge: 0.12mm / t
[0145] (5) Axial penetration depth ap: 2mm
[0146] (6) Processing methods: dry and wet
[0147] (7) Evaluation method: Under the above conditions, the 80mm×300mm surface of the workpiece is milled, and the time point when the Vb wear width of the tool back face reaches 0.1mm is judged as the life of the coated tool.
[0148] Figure 13 This is a table showing the results of X-ray diffraction spectrum measurements and cutting tests on coated cutting tools for samples No.1 to No.4.
[0149] like Figure 13 As shown, for the coated cutting tool of sample No. 1, Ih(100) / Ih(002) is 0.29. For the coated cutting tool of sample No. 2, Ih(100) / Ih(002) is 0.9. For the coated cutting tool of sample No. 3, Ih(100) / Ih(002) is 1.57. For the coated cutting tool of sample No. 4, Ih(100) / Ih(002) is 1.75.
[0150] Regarding the coated cutting tools of samples No. 1 and No. 2, the X-ray diffraction spectra of the heat-treated coating layers satisfy the relationship Ih(100) / Ih(002)≤0.9. On the other hand, regarding the coated cutting tools of samples No. 3 and No. 4, the X-ray diffraction spectra of the heat-treated coating layers do not satisfy the relationship Ih(100) / Ih(002)≤0.9. The coated cutting tools of samples No. 1 and No. 2 correspond to embodiments of the present invention. The coated cutting tools of samples No. 3 and No. 4 correspond to comparative examples of the present invention.
[0151] Thus, it can be confirmed that by forming a coating layer in such a manner that the coating layer comprises a plurality of Ta-containing stacked structures and a plurality of Mo-containing stacked structures, each of the plurality of Ta-containing stacked structures comprising a first compound layer containing Ta in a first composition ratio and a second compound layer containing Ta in a second composition ratio different from the first composition ratio, and each of the plurality of Mo-containing stacked structures comprising a third compound layer containing Mo in a third composition ratio and a fourth compound layer containing Mo in a fourth composition ratio different from the third composition ratio, it is possible to obtain a coating layer whose X-ray diffraction spectrum measured after being held at 1200°C for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship Ih(100) / Ih(002)≤0.9.
[0152] like Figure 13 As shown, the tool life of coated samples No. 1 and No. 2 is the same as or longer than that of coated samples No. 3 and No. 4 for both dry and wet machining, and in both low-speed and high-speed machining. Therefore, it can be confirmed that the tool life can be extended when the X-ray diffraction spectrum of the coating layer measured after being held at 1200°C for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship Ih(100) / Ih(002)≤0.9.
[0153] Regarding the coated cutting tools of samples No. 1 and No. 2, the X-ray diffraction spectrum of the coated layer after heat treatment of sample No. 1 satisfies the relationship Ih(100) / Ih(002)≤0.3. On the other hand, the X-ray diffraction spectrum of the coated cutting tool of sample No. 2 does not satisfy the relationship Ih(100) / Ih(002)≤0.3.
[0154] like Figure 13 As shown, the tool life of the coated material No. 1 is longer than that of the coated material No. 2 in both dry and wet machining, and in both low-speed and high-speed machining. Therefore, it can be confirmed that the tool life can be further extended when the X-ray diffraction spectrum of the coating layer measured after being held at 1200°C for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship Ih(100) / Ih(002)≤0.3.
[0155] As described above, the coated tool of the embodiment (for example, coated tool 1) includes a substrate (for example, substrate 10) and a coating layer (for example, coating layer 20) located on the substrate and composed of cubic crystals. The X-ray diffraction spectrum of the coating layer measured after being held at 1200°C for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship Ih(100) / Ih(002)≤0.9. Ih(100) is the intensity of the diffraction peak corresponding to the (100) plane of the hexagonal crystal formed in the coating layer. Ih(002) is the intensity of the diffraction peak corresponding to the (002) plane of the hexagonal crystal.
[0156] Therefore, the coated cutting tool according to the embodiment can extend the tool life.
[0157] Figure 1 The shape of the coated tool 1 shown is merely an example and is not limited to the shape of coated tools based on the present invention. Coated tools based on the present invention may, for example, have: a rod-shaped body having a rotation axis extending from a first end to a second end; a cutting edge located at the first end of the body; and a groove extending spirally from the cutting edge toward the second end of the body.
[0158] Note (1): A coated cutting tool, wherein the coated cutting tool comprises: a substrate; and a coating layer located on the substrate and composed of cubic crystals, wherein the X-ray diffraction spectrum of the coating layer measured after being held at a temperature of 1200°C for 0.5 hours in a non-oxidizing atmosphere satisfies the relationship Ih(100) / Ih(002)≤0.9, where Ih(100) is the intensity of the diffraction peak corresponding to the (9 100) plane of the hexagonal crystal formed in the coating layer, and Ih(002) is the intensity of the diffraction peak corresponding to the (002) plane of the hexagonal crystal.
[0159] Note (2): According to the coated cutting tool described in Note (1), the X-ray diffraction spectrum satisfies the relationship Ih(100) / Ih(002)≤0.3.
[0160] Note (3): A cutting tool comprising: a rod-shaped shank having a groove at its end; and a coated tool as described in Note (1) or (2), located within the groove.
[0161] Further effects and / or variations can be readily derived by those skilled in the art. Therefore, the broader scope of the invention is not limited to the specific detailed and representative embodiments shown and described above. Thus, various modifications can be made without departing from the spirit or scope of the general concept of the invention as defined by the appended technical solutions and their equivalents.
[0162] Explanation of reference numerals in the attached figures
[0163] 1 Coated cutting tool
[0164] 2 Blade Body
[0165] 3 Cutting edge
[0166] 5 through holes
[0167] 10 matrix
[0168] 20 coating layers
[0169] 21 intermediate layers
[0170] 22 Ta-containing layered structures
[0171] 22a First compound layer
[0172] 22b Second compound layer
[0173] 23 Mo-containing layered structures
[0174] 23a Third compound layer
[0175] 23b Fourth compound layer
[0176] 70 knife handle
[0177] 73-groove
[0178] 75 screws
[0179] 100 cutting tools
[0180] 101 Vacuum Chamber
[0181] 102 Gas Inlet
[0182] 103 cathode electrode
[0183] 104 anode electrode
[0184] 105 target material
[0185] 106 Sample Support Platform
[0186] 107 tower
[0187] 108 heater
[0188] 109 Gas Exhaust Port
[0189] 110 bias power supply
[0190] 1000AIP device.
Claims
1. A coated cutting tool, wherein, The coated cutting tool has the following features: Matrix; and A coating layer, located on the substrate and composed of cubic crystals. The X-ray diffraction spectrum of the coating layer, after being held at 1200°C for 0.5 hours in a non-oxidizing atmosphere, satisfies the relationship Ih(100) / Ih(002)≤0.
9. Ih(100) is the intensity of the diffraction peak corresponding to the (100) plane of the hexagonal crystal formed in the coating layer. Ih(002) is the intensity of the diffraction peak corresponding to the (002) plane of the hexagonal crystal.
2. The coated cutting tool according to claim 1, wherein, The X-ray diffraction spectrum satisfies the relationship Ih(100) / Ih(002)≤0.
3.
3. A cutting tool, wherein, The cutting tool includes: A rod-shaped knife handle with a groove at the end; and The coated cutting tool according to claim 1 or 2, which is located within the cutting groove.
Citation Information
Patent Citations
Hard coating ultrahigh temperature high pressure sintered material
JP2002003284A
Coated cutting tool
JP2019181586A
Hard coating, hard-coated tool, and their production methods
US20190177839A1