GIS-type zeolite, zeolite molded body, adsorption device, and method for producing purified gas

By optimizing the structure and composition of GIS type zeolite, the problem of embrittlement and adsorption-desorption hysteresis during carbon dioxide adsorption is solved, and the embrittlement resistance and adsorption-desorption efficiency of zeolite are improved.

CN118922381APending Publication Date: 2024-11-08ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202380029598.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing GIS type zeolites are prone to brittle during carbon dioxide adsorption, resulting in the device being blocked, and there is an adsorption-desorption hysteresis, affecting the adsorption-desorption efficiency.

Method used

By controlling the position and intensity of the diffraction peak PCO2, as well as the silica-alumina ratio and cationic species, the structure and composition of the zeolite are optimized, the hysteresis phenomenon in the carbon dioxide adsorption-desorption isotherms are reduced, and the brittleness resistance of the zeolite is improved.

Benefits of technology

It significantly improves the embrittlement resistance and adsorption-desorption efficiency of GIS type zeolites, reduces the hysteresis during the carbon dioxide adsorption-desorption process, and extends the service life of the zeolite molded body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922381A_ABST
    Figure CN118922381A_ABST
Patent Text Reader

Abstract

Provided is a GIS-type zeolite in which, among diffraction peaks observed at a diffraction angle 2 [theta] = 25.81-34.57 DEG in a spectrum obtained by X-ray diffraction in a dehydrated state and under carbon dioxide adsorption conditions, the diffraction angle (2 [theta]) of the diffraction peak PCO2 having the strongest intensity is 28.60-29.54 DEG.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a GIS type zeolite, a zeolite molded body, an adsorption device and a method for producing a purified gas. Background Art

[0002] Zeolite can be used as an adsorbent, a desiccant, a separating agent, a catalyst, a catalyst carrier, a detergent builder, an ion exchanger, a wastewater treatment agent, a fertilizer, a food additive, a cosmetic additive, and the like, and is particularly useful for gas separation.

[0003] Among zeolites, substances represented by the GIS structure, which is a code for defining zeolite structures established by IZA (International Zeolite Association), are called GIS-type zeolites. GIS-type zeolites are zeolites with fine pores composed of 8-membered oxygen rings. Regarding this GIS-type zeolite, for example, in Patent Document 1, a GIS-type zeolite having an adsorption capacity for carbon dioxide was synthesized, and it was shown that when the GIS-type zeolite is used as an adsorbent, it can be used for separation, recovery, and purification of carbon dioxide.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. WO2019 / 202933 Summary of the invention

[0007] Problems to be solved by the invention

[0008] When using adsorbent materials to separate, recover, and purify carbon dioxide, pressure swing adsorption separation, temperature swing adsorption separation, or pressure swing-temperature swing adsorption separation are used. In these methods, zeolite is filled in a column or the like for use. In order to prevent the fine powder zeolite from accumulating in the flow path in the device and blocking the flow path, the zeolite is shaped and used in the form of a granular zeolite molded body. As the performance of the zeolite molded body, it is required to have a durability sufficient to correspond to the conditions of use. The following problem has been found: If a large amount of carbon dioxide is adsorbed by a zeolite molded body containing GIS-type zeolite, the zeolite molded body will become brittle. Due to this embrittlement, for example, fine powder will be generated in the adsorption device, which will make the continuous operation of the device difficult due to pressure loss and the like.

[0009] Furthermore, as a performance of the adsorbent material, it is required that there is no adsorption-desorption hysteresis of carbon dioxide. Adsorption-desorption hysteresis refers to the phenomenon of hysteresis in the adsorption and desorption in the adsorption-desorption isotherm of carbon dioxide. When the adsorbent material is used, in the process of heating and vacuuming to carry out the desorption-regeneration of carbon dioxide, it is required that the adsorption amount during adsorption and the desorption amount during regeneration are large. Regarding adsorption-desorption hysteresis, the adsorption amount during adsorption decreases, and along with it, the desorption amount during regeneration decreases, so when used as an adsorbent material, it is difficult to say that it is a desired characteristic. Patent document 1 shows a GIS-type zeolite in which the cations in the zeolite are replaced with Li, Na, K, Rb, and Cs, but adsorption-desorption hysteresis in the adsorption-desorption isotherm of carbon dioxide is observed.

[0010] The object of the present invention is to provide a GIS-type zeolite which has excellent resistance to embrittlement with respect to carbon dioxide adsorption when used as a molded body and can reduce the adsorption-desorption hysteresis in the adsorption-desorption isotherm of carbon dioxide, a molded body comprising the GIS-type zeolite, an adsorbent comprising the molded body, and a method for producing a purified gas using the adsorbent.

[0011] Means for solving problems

[0012] The present inventors have conducted intensive research to solve the above problems and found that the diffraction peak P shown below CO2 When it is within the specified range, or the ratio of the diffraction peaks shown below CO2 / P de When the content is within the prescribed range, the molded article has excellent resistance to embrittlement due to carbon dioxide adsorption when used as the molded article, and can reduce the adsorption-desorption hysteresis in the carbon dioxide adsorption-desorption isotherm, thereby completing the present invention.

[0013] That is, the present invention includes the following embodiments.

[0014] <1>

[0015] A GIS type zeolite, wherein in a spectrum obtained by X-ray diffraction under a dehydrated state and carbon dioxide adsorption condition, among the diffraction peaks observed at diffraction angles of 2θ=25.81 to 34.57°, a diffraction peak P having the strongest intensity is CO2 The diffraction angle (2θ) is 28.60~29.54°.

[0016] <2>

[0017] A GIS type zeolite, wherein in a spectrum obtained by X-ray diffraction in a dehydrated state and under nitrogen adsorption conditions, a diffraction peak having the strongest intensity observed between diffraction angles 2θ=25.81 and 34.57° is defined as P de When PCO2 / P de ≧0.969.

[0018] <3>

[0019] like <1> The GIS type zeolite, wherein in the spectrum obtained by X-ray diffraction in a dehydrated state and under nitrogen adsorption conditions, the diffraction peak with the strongest intensity observed between the diffraction angle 2θ=25.81 and 34.57° is defined as P de When P CO2 / P de ≧0.969.

[0020] <4>

[0021] like <1> ~ <3> The GIS-type zeolite according to any one of the preceding claims, wherein the silica-alumina ratio of the GIS-type zeolite is 3.40 or more.

[0022] <5>

[0023] like <1> ~ <4> The GIS-type zeolite described in any one of the above aspects contains potassium or lithium as a cationic species in the GIS-type zeolite.

[0024] <6>

[0025] like <5> The GIS type zeolite described above has a ratio (Z / T) of the total amount of potassium and lithium (Z) to the total amount of alkali metals (T) in the GIS type zeolite of 0.05 or more.

[0026] <7>

[0027] like <1> ~ <6> The GIS type zeolite described in any one of the preceding claims, wherein 29 The peak area intensities attributed to Q4(3Al), Q4(2Al), Q4(1Al) and Q4(0Al) observed in the Si-MAS-NMR spectrum are set to a, b, c and d, respectively, satisfying (a+d) / (b+c)≧0.192.

[0028] <8>

[0029] A zeolite shaped body comprising <1> ~ <7> The GIS-type zeolite described above.

[0030] <9>

[0031] like <8> The zeolite shaped body comprises a carrier.

[0032] <10>

[0033] like <8> or <9> The zeolite shaped body, wherein the carrier comprises an inorganic binder and an organic binder.

[0034] <11>

[0035] like <8> ~ <10> In any one of the zeolite molded bodies, a total content of the carriers is 1 to 99% by mass based on 100% by mass of the total amount of the zeolite molded body.

[0036] <12>

[0037] like <8> ~ <11> The zeolite molded body described in any one of the above aspects has a cylindrical shape.

[0038] <13>

[0039] like <12> The zeolite molded body has a length of 3 mm to 30 mm, and a diameter of 1 mm to 30 mm.

[0040] <14>

[0041] An adsorption device comprising <8> ~ <13> The zeolite shaped body described in any one of the above.

[0042] <15>

[0043] A method for producing a purified gas, comprising:

[0044] Separation process, using <14> The adsorption device separates one or more gases selected from the group consisting of CO2, H2O, He, Ne, Cl2, NH3 and HCl from a mixture containing two or more gases selected from the group consisting of H2, N2, O2, Ar, CO and hydrocarbons.

[0045] <16>

[0046] like <15> The production method, wherein, in the separation step, the gas is separated by a pressure swing adsorption separation method, a temperature swing adsorption separation method, or a pressure swing-temperature swing adsorption separation method.

[0047] Effects of the Invention

[0048] According to the present invention, there can be provided a GIS-type zeolite which has excellent resistance to embrittlement with respect to carbon dioxide adsorption when used as a molded body and can reduce the adsorption-desorption hysteresis in the adsorption-desorption isotherm of carbon dioxide, a molded body comprising the GIS-type zeolite, an adsorbent comprising the molded body, and a method for producing a purified gas using the adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] Figure 1 These are the carbon dioxide adsorption isotherm and desorption isotherm diagrams of the GIS-type zeolite obtained in Comparative Example 1.

[0050] Figure 2 This is a diagram illustrating an adsorbent according to one embodiment of the present invention. DETAILED DESCRIPTION

[0051] The specific implementation mode of the present invention (hereinafter referred to as "the present implementation mode") is described in detail below. The present invention is not limited to the following description, and can be implemented by various modifications within the scope of its main points. It should be noted that in this specification, the expression of a numerical range such as "1 to 100" includes both its lower limit "1" and upper limit "100". In addition, the expression of other numerical ranges is the same.

[0052] [GIS type zeolite]

[0053] In the spectrum obtained by X-ray diffraction under the condition of carbon dioxide adsorption in the dehydrated state of the GIS type zeolite of the present embodiment, among the diffraction peaks observed at diffraction angles of 2θ=25.81 to 34.57°, the diffraction peak P having the strongest intensity is CO2 The diffraction angle (2θ) is 28.60~29.54°.

[0054] In the GIS type zeolite of the present embodiment, in the spectrum obtained by X-ray diffraction in a dehydrated state under nitrogen adsorption conditions, the diffraction peak with the strongest intensity observed between the diffraction angles 2θ=25.81 and 34.57° is defined as P de When P CO2 / P de ≧0.969.

[0055] Any of the above GIS-type zeolites is excellent in resistance to embrittlement due to carbon dioxide adsorption when used as a molded body, and can reduce the adsorption-desorption hysteresis in the carbon dioxide adsorption-desorption isotherm.

[0056] It is believed that a specific X-ray diffraction peak is related to the rigidity of the crystal (which is affected by the bonding mode of Si and Al present in the zeolite framework). If the diffraction peak is controlled in a prescribed manner, the structural change when carbon dioxide is adsorbed to the zeolite can be suppressed. That is, according to the present embodiment, by controlling the bonding mode of Si and Al, the rigidity of the zeolite itself can be controlled, and the energy consumption corresponding to the expansion and contraction can be reduced, thereby reducing the hysteresis, and the maximum stress corresponding to the expansion and contraction when used as an adsorbent material can be reduced. According to these characteristics, the adsorption-desorption hysteresis in the adsorption-desorption isotherm of carbon dioxide can be reduced, and a GIS-type zeolite with resistance to embrittlement of carbon dioxide adsorption when used as a molded body is provided.

[0057] From the perspective of improving the embrittlement resistance to carbon dioxide adsorption when used as a molded body and reducing the adsorption-desorption hysteresis in the carbon dioxide adsorption-desorption isotherm, P CO2 The diffraction angle (2θ) is preferably 28.60 to 29.50°, more preferably 28.60 to 29.10°, and further preferably 28.60 to 28.90°.

[0058] P CO2 / P de It is preferably 0.969 or more, more preferably 0.974 or more, and even more preferably 0.985 or more. CO2 / P de The upper limit of is not particularly limited, and may be 1.33 or less, 1.20 or less, or 1.01 or less.

[0059] About P CO2 and P de The diffraction angle (2θ) can be measured in more detail by the method described in the Examples. CO2 and P de The diffraction angle (2θ) can be obtained, for example, by successively adding a silicon oxide source in an aging step in a method for producing a GIS-type zeolite described later, controlling initial nucleation in zeolite precursor synthesis, and the like.

[0060] There are no particular restrictions on the GIS-type zeolite of the present embodiment. The lower the silica-alumina ratio (indicated by the molar ratio of silica to alumina expressed as SiO2 / Al2O3, hereinafter also referred to as "SAR"), the more hydrophilic it is, and the stronger the adsorption force of polar molecules such as carbon dioxide becomes. Since the adsorption force is too strong if the SAR is low, the energy required for desorption by heating and vacuuming will increase, and thus a high SAR is preferred. The SAR is preferably greater than 3.40, more preferably greater than 4.40, more preferably greater than 4.50, further preferably greater than 4.69, further preferably greater than 4.90, further preferably greater than 5.40, and further preferably greater than 6.01. There is no particular restriction on the upper limit of the SAR, but if the SAR is too high, the interaction with the adsorbate is reduced, and thus the SAR is preferably less than 3000, more preferably less than 500, and further preferably less than 100. The SAR of the zeolite in the zeolite molded body is determined by 29 SAR can be determined by Si-MAS-NMR measurement. SAR can be measured in more detail by the method described in the examples below. SAR can be determined by mixing water and OH in the gel. - The amount ratio etc. can be adjusted.

[0061] From the perspective of the energy required for desorption, a high SAR is preferred. On the other hand, when the SAR in the GIS type zeolite increases, it is confirmed that the adsorption-desorption hysteresis in the adsorption-desorption isotherm of carbon dioxide becomes dominant. In the GIS type zeolite of the present embodiment, the adsorption-desorption hysteresis in the adsorption-desorption isotherm of carbon dioxide can be eliminated by controlling the bonding mode of Si and Al in the zeolite framework. Specifically, 29 The peak area intensities attributable to Q4(3Al), Q4(2Al), Q4(1Al), and Q4(0Al) observed in the Si-MAS-NMR spectrum are set to a, b, c, and d, respectively, preferably satisfying (a+d) / (b+c)≧0.192, more preferably 0.913≧(a+d) / (b+c)≧0.195, and further preferably 0.519≧(a+d) / (b+c)≧0.199. 29 Peaks such as Q4(3Al), Q4(2Al), Q4(1Al), and Q4(0Al) observed in the Si-MAS-NMR spectrum represent the bonding mode of Si and Al in the zeolite framework, and (a+d) and (b+c), which are the sum of the area intensities, represent the sum of the amounts of these bonding modes, and (a+d) / (b+c) represents the abundance ratio. The abundance ratio of the bonding modes of Si and Al affects the structural changes of the zeolite framework itself during adsorption and desorption. Therefore, by making the abundance ratio (a+d) / (b+c) of the bonding modes of Si and Al in the zeolite framework within an appropriate range, the adsorption-desorption hysteresis in the adsorption-desorption isotherm can be eliminated. (a+d) / (b+c) can be measured by the method described in the examples described later. In order to make (a+d) / (b+c) within a specified range, it can be adjusted by the amount ratio of alkali metal / alkaline earth metal and OH- in the mixed gel during synthesis.

[0062] From the perspective of improving the selective adsorption capacity of carbon dioxide, as the cationic species in the GIS type zeolite, potassium or lithium is preferably contained, and potassium is more preferably contained. In addition, the total content of potassium and lithium in the zeolite is calculated in the form of the ratio (Z / T) of the total value of the amount of substance of potassium and lithium in the GIS type zeolite (Z) relative to the total value of the amount of substance of alkali metals (T). Z / T is preferably greater than 0.05, more preferably greater than 0.10, and further preferably greater than 0.15. There is no particular limit to the upper limit of Z / T, and Z / T can be less than 1.00. Regarding Z / T, it can be measured by ICP-emission spectrometry using a liquid that is appropriately diluted after the zeolite is thermally dissolved in an aqueous sodium hydroxide solution or aqua regia. In more detail, Z / T can be measured by the method described in the examples described later. Z / T can be adjusted by changing the ratio of potassium and lithium in the cationic species of the GIS type zeolite.

[0063] The ratio (K / T) of the total amount of potassium (K) in the GIS zeolite to the total amount of each alkali metal (T) is preferably 0.05 or more, more preferably 0.10 or more, and even more preferably 0.15 or more. The upper limit of K / T is not particularly limited, and K / T may be 1.00 or less.

[0064] GIS type zeolite preferably has a diameter of 10 cm 3 / g or more of carbon dioxide adsorption. The carbon dioxide adsorption of zeolite is preferably 20cm 3 / g or more, more preferably 40cm 3 / g or more, more preferably 50cm 3 The upper limit of the carbon dioxide adsorption amount of zeolite is not particularly limited, but is, for example, 100 cm 3 / g or less. The carbon dioxide adsorption capacity is the carbon dioxide adsorption capacity (cm2) per 1g of zeolite at 25°C. 3 ). More specifically, the measurement was performed by the method described in the Examples.

[0065] The methane adsorption capacity of GIS zeolite is preferably less than 10 cm 3 / g. The methane adsorption capacity of zeolite is more preferably 9cm 3 / g or less, more preferably 8cm 3 / g or less. The methane adsorption capacity is the methane adsorption capacity (cm2) per 1g of zeolite at 25°C. 3 ). More specifically, the measurement was performed by the method described in the Examples.

[0066] The selectivity of the GIS type zeolite represented by the carbon dioxide adsorption amount / methane adsorption amount is preferably 10 or more, more preferably 13 or more, and further preferably 15 or more. The upper limit of the adsorption selectivity of the zeolite is not particularly limited, and is, for example, 100 or less.

[0067] The preferred content of zeolite may be 50% by mass or more, 60% by mass or more, 70% by mass or more, or 80% by mass or more relative to the total amount 100% by mass of the zeolite molded body. In addition, the content of GIS-type zeolite may be 98% by mass or less, or 95% by mass or less relative to the total amount 100% by mass of the zeolite molded body.

[0068] (Synthesis method of GIS type zeolite)

[0069] The method for producing the GIS type zeolite of the present embodiment may include, for example, a step of preparing a mixed gel, the mixed gel containing a silicon oxide source containing silicon, an aluminum source containing aluminum, an alkali metal source / alkaline earth metal source containing at least one selected from an alkali metal (M1) and an alkaline earth metal (M2), an alkali source, a phosphorus source containing phosphorus, an organic structure directing agent, and water. The mixed gel and the components contained therein are described below.

[0070] [Mixed gel]

[0071] The hybrid gel in the present embodiment is a mixture containing a silicon oxide source, an aluminum source, an alkali metal source / alkaline earth metal source, and water as components, and optionally containing an alkali source, a phosphorus source, and an organic structure directing agent.

[0072] The silicon oxide source refers to a component in the mixed gel that is a raw material for silicon contained in the zeolite manufactured from the mixed gel, the aluminum source refers to a component in the mixed gel that is a raw material for aluminum contained in the zeolite manufactured from the mixed gel, the alkali metal source / alkaline earth metal source refers to a component in the mixed gel that is a raw material for alkali metal and / or alkaline earth metal contained in the zeolite manufactured from the mixed gel, the alkali source refers to a component used for the purpose of adjusting the alkalinity (pH) in the mixed gel, and the phosphorus source refers to a component in the mixed gel that is a raw material for phosphorus contained in the zeolite manufactured from the mixed gel.

[0073] [Silicon oxide source]

[0074] As a silicon oxide source, there is no particular limitation as long as it is a commonly used silicon oxide source, and examples thereof include crystalline silicon oxide, amorphous silicon oxide, silicic acid, silicates, and organic silicic acid compounds. More specific examples include sodium silicate, potassium silicate, calcium silicate, magnesium silicate, fumed silica, precipitated silica, silica gel, colloidal silica, aluminum silicate, tetraethoxysilane (TEOS), trimethylethoxysilane, and the like. These compounds can be used alone or in combination. Here, aluminum silicate is both a silicon oxide source and an aluminum source.

[0075] Among these, fumed silica, colloidal silica, or precipitated silica is preferred because zeolite with high crystallinity tends to be obtained.

[0076] [Aluminum source]

[0077] The aluminum source is not particularly limited as long as it is a commonly used aluminum source, and specific examples thereof include sodium aluminate, aluminum sulfate, aluminum nitrate, aluminum acetate, aluminum hydroxide, aluminum oxide, aluminum chloride, aluminum alkoxide, metallic aluminum, amorphous aluminum silicate gel, etc. These compounds may be used alone or in combination of a plurality of them.

[0078] Among these, sodium aluminate, aluminum sulfate, aluminum nitrate, aluminum acetate, aluminum hydroxide, aluminum chloride, and aluminum alkoxide are preferred because they tend to produce zeolites with high crystallinity. From the same perspective, sodium aluminate and aluminum hydroxide are more preferred, and sodium aluminate is further preferred.

[0079] [Alkali metal source / alkaline earth metal source]

[0080] The type of the alkali metal / alkaline earth metal in the alkali metal source / alkaline earth metal source is not particularly limited, and any alkali metal compound and / or any alkaline earth metal compound can be used.

[0081] Examples of the alkali metal source / alkaline earth metal source include, but are not limited to, hydroxides, bicarbonates, carbonates, acetates, sulfates, nitrates, etc. of alkali metals or alkaline earth metals. These compounds may be used alone or in combination of plural types.

[0082] As the alkali metal and alkaline earth metal used as the alkali source, Li, Na, K, Rb, Cs, Ca, Mg, Sr, Ba, etc. can be generally used. From the aspect that the crystallization of the GIS type skeleton is easier to form, Na and K are preferably used, and Na is more preferably used. In addition, the alkali metal and alkaline earth metal used as the alkali metal source / alkaline earth metal source can be used alone, or a plurality of them can be used in combination.

[0083] Specifically, the alkali source includes, but is not limited to:

[0084] Sodium sulfate, sodium sulfite, sodium thiosulfate, sodium nitrite, sodium nitrate, sodium carbonate, sodium bicarbonate, sodium phosphate, sodium acetate, sodium formate, sodium citrate, sodium oxalate, sodium fluoride, sodium chloride, sodium bromide, sodium iodide, sodium sulfide, sodium silicate, sodium metasilicate, sodium tetraborate, sodium chlorate, sodium perchlorate, sodium cyanide, sodium metastannate, sodium hexahydroxytin (IV) acid, sodium hexacyanoferrous (II) acid, sodium permanganate, sodium chromate, sodium dichromate,

[0085] Potassium sulfate, potassium sulfite, potassium thiosulfate, potassium nitrite, potassium nitrate, potassium carbonate, potassium bicarbonate, potassium phosphate, potassium acetate, potassium formate, potassium citrate, potassium oxalate, potassium fluoride, potassium chloride, potassium bromide, potassium iodide, potassium sulfide, potassium silicate, potassium metasilicate, potassium tetraborate, potassium chlorate, potassium perchlorate, potassium cyanide, potassium metastannate, potassium hexahydroxytin (IV) acid, potassium hexacyanoferrous (II) acid, potassium permanganate, potassium chromate, potassium dichromate,

[0086] Lithium sulfate, lithium sulfite, lithium thiosulfate, lithium nitrite, lithium nitrate, lithium carbonate, lithium bicarbonate, lithium phosphate, lithium acetate, lithium formate, lithium citrate, lithium oxalate, lithium fluoride, lithium chloride, lithium bromide, lithium iodide, lithium sulfide, lithium silicate, lithium metasilicate, lithium tetraborate, lithium chlorate, lithium perchlorate, lithium cyanide, lithium metastannate, lithium hexahydroxytin (IV) acid, lithium hexacyanoferrous (II) acid, lithium permanganate, lithium chromate, lithium dichromate,

[0087] Rubidium sulfate, rubidium sulfite, rubidium thiosulfate, rubidium nitrite, rubidium nitrate, rubidium carbonate, rubidium bicarbonate, rubidium phosphate, rubidium acetate, rubidium formate, rubidium citrate, rubidium oxalate, rubidium fluoride, rubidium chloride, rubidium bromide, rubidium iodide, rubidium sulfide, rubidium silicate, rubidium metasilicate, rubidium tetraborate, rubidium chlorate, rubidium perchlorate, rubidium cyanide, rubidium metastannate, rubidium hexahydroxytin (IV) acid, rubidium hexacyanoferrous (II) acid, rubidium permanganate, rubidium chromate, rubidium dichromate,

[0088] Cesium sulfate, cesium sulfite, cesium thiosulfate, cesium nitrite, cesium nitrate, cesium carbonate, cesium bicarbonate, cesium phosphate, cesium acetate, cesium formate, cesium citrate, cesium oxalate, cesium fluoride, cesium chloride, cesium bromide, cesium iodide, cesium sulfide, cesium silicate, cesium metasilicate, cesium tetraborate, cesium chlorate, cesium perchlorate, cesium cyanide, cesium metastannate, cesium hexahydroxytin (IV) acid, cesium hexacyanoferrous (II) acid, cesium permanganate, cesium chromate, cesium dichromate,

[0089] Magnesium sulfate, magnesium sulfite, magnesium thiosulfate, magnesium nitrite, magnesium nitrate, magnesium carbonate, magnesium bicarbonate, magnesium phosphate, magnesium acetate, magnesium formate, magnesium citrate, magnesium oxalate, magnesium fluoride, magnesium chloride, magnesium bromide, magnesium iodide, magnesium sulfide, magnesium silicate, magnesium metasilicate, magnesium tetraborate, magnesium chlorate, magnesium perchlorate, magnesium cyanide, magnesium metastannate, magnesium hexahydroxystannate (IV), magnesium hexacyanoferrous (II), magnesium permanganate, magnesium chromate, magnesium dichromate,

[0090] Calcium sulfate, calcium sulfite, calcium thiosulfate, calcium nitrite, calcium nitrate, calcium carbonate, calcium bicarbonate, calcium phosphate, calcium acetate, calcium formate, calcium citrate, calcium oxalate, calcium fluoride, calcium chloride, calcium bromide, calcium iodide, calcium sulfide, calcium silicate, calcium metasilicate, calcium tetraborate, calcium chlorate, calcium perchlorate, calcium cyanide, calcium metastannate, calcium hexahydroxystannate (IV), calcium hexacyanoferrous (II), calcium permanganate, calcium chromate, calcium dichromate,

[0091] Strontium sulfate, strontium sulfite, strontium thiosulfate, strontium nitrite, strontium nitrate, strontium carbonate, strontium bicarbonate, strontium phosphate, strontium acetate, strontium formate, strontium citrate, strontium oxalate, strontium fluoride, strontium chloride, strontium bromide, strontium iodide, strontium sulfide, strontium silicate, strontium metasilicate, strontium tetraborate, strontium chlorate, strontium perchlorate, strontium cyanide, strontium metastannate, strontium hexahydroxytin (IV) acid, strontium hexacyanoferrous (II) acid, strontium permanganate, strontium chromate, strontium dichromate,

[0092] Barium sulfate, barium sulfite, barium thiosulfate, barium nitrite, barium nitrate, barium carbonate, barium bicarbonate, barium phosphate, barium acetate, barium formate, barium citrate, barium oxalate, barium fluoride, barium chloride, barium bromide, barium iodide, barium sulfide, barium silicate, barium metasilicate, barium tetraborate, barium chlorate, barium perchlorate, barium cyanide, barium metastannate, barium hexahydroxytin (IV) acid, barium hexacyanoferrous (II) acid, barium permanganate, barium chromate, barium dichromate, etc.

[0093] [Alkali source]

[0094] Alkali source is used for the purpose of adjusting the alkalinity (pH) in the mixed gel in order to promote crystallization into a zeolite structure when manufacturing zeolite. The alkali used can be any compound showing alkalinity, and both inorganic compounds and organic compounds are acceptable. From the perspective of cost, inorganic compounds are preferred, and alkali metal hydroxides can be more preferably cited. As alkali metal hydroxides, lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, etc. can be cited, and sodium hydroxide and potassium hydroxide can be preferably cited, and sodium hydroxide can be more preferably cited. These compounds can be used alone, or a plurality of them can be used in combination.

[0095] The phosphorus source is not particularly limited as long as it is a commonly used phosphorus source, and specific examples include aqueous phosphoric acid solution, sodium phosphate, aluminum phosphate, potassium phosphate, lithium phosphate, calcium phosphate, barium phosphate, etc. These compounds may be used alone or in combination of plural types.

[0096] Among these, phosphoric acid aqueous solution, sodium phosphate, and aluminum phosphate are preferred because they tend to produce zeolite with high crystallinity. From the same viewpoint, phosphoric acid aqueous solution and sodium phosphate are more preferred, and phosphoric acid aqueous solution is still more preferred.

[0097] [Organic structure directing agent]

[0098] When zeolite is produced by hydrothermal synthesis of a mixed gel, the organic structure-directing agent is a compound that promotes crystallization into a zeolite structure. The organic structure-directing agent may be used as necessary in the crystallization of zeolite.

[0099] The organic structure directing agent may be of any type as long as it can form the desired GIS-type zeolite. The organic structure directing agent may be used alone or in combination of two or more.

[0100] As the organic structure directing agent, for example, amines, quaternary ammonium salts, alcohols, ethers, amides, alkyl ureas, alkyl thioureas, cyanoalkanes, and alicyclic heterocyclic compounds containing nitrogen as a heteroatom can be used, but are not limited thereto. Preferably, alkylamines are used, and more preferably, isopropylamine is used.

[0101] Such salts may be accompanied by anions. Representative examples of such anions include, but are not limited to, Cl - Br - ,I - Halogen ions, hydroxide ions, acetate ions, sulfate ions, nitrate ions, carbonate ions, and bicarbonate ions are preferred. Among these, halogen ions and hydroxide ions are preferred, and halogen ions are more preferred, because crystal formation of the GIS-type skeleton becomes easier.

[0102] [Composition ratio of mixed gel]

[0103] In the present embodiment, in order to synthesize GIS-type zeolite with a suitable structure, the selection of a silicon oxide source is important. The dissolution behavior of the silicon oxide source at the initial stage of the reaction has a great influence on the bonding mode of Al in the zeolite framework, so it is necessary to select a suitable silicon oxide source according to the composition of the mixed gel. In addition, the dissolution behavior of the silicon oxide source at the initial stage of the reaction depends on the amount of alkali metal / alkaline earth metal contained in the silicon oxide source itself. The ratio of the amount of alkali metal / alkaline earth metal contained in the silicon oxide source itself to SiO2 is expressed in the form of the molar ratio of the sum of L12O and L2O to SiO2, i.e. (L12O+L2O) / SiO2. (Here, L1 and L2 respectively represent the alkali metal and alkaline earth metal contained in the silicon oxide source, and they are calculated in the form of oxides.)

[0104] It should be noted that even when using a plurality of silicon oxide sources, the ratio of the total molar amount of the alkali metal / alkaline earth metal contained in the plurality of silicon oxide sources to the total molar amount of SiO2 can be considered. From the perspective of selecting a suitable silicon oxide source and controlling the dissolution behavior of the silicon oxide source in the initial stage of the reaction, the ratio of the alkali metal / alkaline earth metal contained in the silicon oxide source itself to SiO2 (L12O+L2O) / SiO2 is preferably 0.30 or less, more preferably 0.25 or less, and further preferably 0.08 or less.

[0105] In order to synthesize GIS-type zeolites with suitable structures, the amount of alkali metal / alkaline earth metal in the mixed gel is related to the OH - The ratio of alkali metal / alkaline earth metal in the mixed gel is the most important. - OH - The total molar ratio of M12O and M2O, i.e., OH - / (M12O+M2O). (Here, M1 represents an alkali metal and M2 represents an alkaline earth metal. They are calculated in the form of oxides.) In addition, OH - It is OH derived from inorganic hydroxides such as NaOH and Ca(OH)2, and organic hydroxides such as tetraethylammonium hydroxide. -, excluding OH released when substances expressed as oxides such as sodium aluminate and sodium silicate, or their hydrates are dissolved in water. - .

[0106] In the formation of zeolite, the silicon oxide source and aluminum source dissolved in the water solvent react while dissolving, thereby crystallizing. - The ratio of alkali metal / alkaline earth metal to OH is within an appropriate range, the bonding mode of Al in the zeolite framework can be controlled, and a GIS type zeolite having an ideal crystal structure can be synthesized. From the perspective of forming an ideal GIS type framework crystal, the amount of alkali metal / alkaline earth metal and OH - OH - / (M12O+M2O) is preferably 0.20 or less, more preferably 0.16 or less, and further preferably 0.10 or less.

[0107] The ratio of the silica source to the aluminum source in the mixed gel is expressed as the molar ratio of the oxides of each element, i.e., SiO2 / Al2O3 (it should be noted that the ratio in the synthesized zeolite is inconsistent with the silica-alumina ratio of the mixed gel. The silica-alumina ratio of the synthetic zeolite is determined by other compositions and synthesis conditions). The SiO2 / Al2O3 in the mixed gel is not particularly limited as long as it is a ratio that can form zeolite. For the reason that it tends to be able to inhibit the formation of zeolites having a framework different from the GIS-type framework, the ratio is preferably 3.0 to 70.0, more preferably 3.5 to 65.0, and even more preferably 4.0 to 60.0.

[0108] In addition, if the ratio of water to alumina (H2O / Al2O3) is high, the components in the mixed gel are more easily dispersed uniformly, but if it is too high, the crystallization rate will be significantly reduced. Therefore, in order to synthesize GIS-type zeolite with an optimal crystal structure, it is necessary to control H2O / Al2O3 to the optimum because it affects the balance between crystallization and redissolution.

[0109] From the above aspects, H2O / Al2O3 is preferably 210≦H2O / Al2O3≦780, more preferably 220≦H2O / Al2O3≦778, and further preferably 230≦H2O / Al2O3≦775.

[0110] The ratio of the phosphorus source to the aluminum source in the mixed gel is expressed as the molar ratio of the oxides of each element, i.e., P2O5 / Al2O3. The P2O5 / Al2O3 ratio is not particularly limited as long as it is a ratio capable of forming zeolite, but is preferably less than 1.0, more preferably 0.6 or less, further preferably 0.4 or less, and particularly preferably 0, because it tends to suppress the formation of zeolite having a framework different from the GIS-type framework.

[0111] When the mixed gel contains an organic structure directing agent, the ratio of the aluminum source to the organic structure directing agent in the mixed gel is expressed as the molar ratio of the organic structure directing agent to Al2O3, i.e., R / Al2O3 (here, R represents the organic structure directing agent). From the perspective of making the crystal formation of the GIS-type skeleton easier, and / or shortening the synthesis time, and improving the economic efficiency when manufacturing zeolite, it is preferably less than 7.0, more preferably less than 6.0, and further preferably less than 5.0. When an organic structure directing agent is used, the organic structure directing agent remains in the pores of the zeolite, carbon dioxide does not enter the pores, and the adsorption amount is reduced. In order to remove the organic structure directing agent, it is necessary to heat to at least 400°C, but GIS-type zeolite will undergo crystal fragmentation and become amorphous at above 350°C, so it is preferably less than the organic structure directing agent. From this perspective, R / Al2O3 is preferably less than 4.0, more preferably less than 3.5, and further preferably less than 3.0.

[0112] As described above, the method for producing GIS type zeolite of the present embodiment includes a step of preparing a mixed gel, wherein the mixed gel contains a silicon oxide source containing silicon, an aluminum source containing aluminum, an alkali metal / alkaline earth metal source, an alkali source, a phosphorus source, and water, wherein the molar ratio of each component in the mixed gel is calculated in the form of oxides of each element with respect to the silicon, aluminum, alkali metal (M1) and alkaline earth metal (M2), alkali metal (L1) and alkaline earth metal (L2) contained in the silicon oxide source, and the phosphorus source, and the following formulas (1), (2), (3) and (4) are used to calculate the molar ratio of each component in the mixed gel. The molar ratios α, β, γ, δ, and ε represented by (3), (4), (5), and (6) preferably satisfy α≦0.30, β≦0.20, 3.0≦γ≦70.0, 210≦δ≦780, and 0≦ε<1.0, and more preferably satisfy α≦0.25, β≦0.16, 3.5≦γ≦65.0, 220≦δ≦778, and 0≦ε≦0.6, and further preferably satisfy α≦0.08, β≦0.10, 4.0≦γ≦60.0, 230≦δ≦775, and 0≦ε≦0.4. The GIS type zeolite of the present embodiment is particularly preferably obtained by the method for producing the GIS type zeolite of the present embodiment described above.

[0113] α=(L12O+L2O) / SiO2 (1)

[0114] β=OH - / (M12O+M2O) (2)

[0115] γ=SiO2 / Al2O3 (3)

[0116] δ=H2O / Al2O3 (4)

[0117] ε=P2O5 / Al2O3 (5)

[0118] In the method for producing GIS-type zeolite of the present embodiment, when the molar ratios α, β, γ, δ, and ε satisfy the above ranges and the mixed gel further contains an organic structure directing agent R, the molar ratio ζ represented by the following formula (6) preferably satisfies ζ≦4.

[0119] ζ=R / Al2O3 (6)

[0120] The presence of seed crystals in the mixed gel is not essential, and the GIS type zeolite of the present embodiment may be obtained by adding a pre-produced GIS type zeolite as seed crystals to the mixed gel.

[0121] [Hybrid Gel Preparation Process]

[0122] The preparation process of the mixed gel is not particularly limited, and may include, for example, the following steps: a mixing process of mixing a silicon oxide source, an aluminum source, an alkali metal source / alkaline earth metal source, water, and, if necessary, an alkali source, a phosphorus source, and an organic structure directing agent at one time or in multiple stages; and a aging process of the mixture obtained in the mixing process.

[0123] In the mixing step, the components including the silicon oxide source, the aluminum source, the alkali metal source / alkaline earth metal source, water, and, if necessary, the alkali source, the phosphorus source, and the organic structure directing agent may be mixed at once or in multiple stages.

[0124] The order when mixing in multiple stages is not limited, and can be suitably selected according to the conditions used. When mixing in multiple stages, it can be carried out with or without stirring. When stirring, as long as it is a commonly used stirring method, it is not particularly limited. As a specific example, a method using paddle stirring, vibration stirring, swing stirring, centrifugal stirring, etc. can be cited.

[0125] The rotation speed of stirring is not particularly limited as long as it is a stirring speed generally used, and for example, it may be 1 rpm or more and less than 2000 rpm.

[0126] The temperature in the mixing step is not particularly limited as long as it is a temperature generally used, and for example, it may be -20°C or higher and lower than 80°C.

[0127] The time of the mixing step is not particularly limited and can be appropriately selected according to the temperature of the mixing step. For example, it can be greater than 0 minutes and 1000 hours or less.

[0128] The aging process can be carried out under standing or stirring. When stirring is carried out in the aging process, there is no particular limitation as long as it is a commonly used stirring method. Specific examples include methods using paddle stirring, vibration stirring, swing stirring, centrifugal stirring, and the like.

[0129] The rotation speed of stirring is not particularly limited as long as it is a stirring speed generally used, and for example, it may be 1 rpm or more and less than 2000 rpm.

[0130] The temperature of the aging step is not particularly limited as long as it is a temperature generally used, and for example, it may be -20°C or higher and lower than 80°C.

[0131] The time of the aging step is not particularly limited and can be appropriately selected according to the temperature of the aging step. For example, it can be greater than 0 minutes and 1000 hours or less.

[0132] It is believed that the zeolite produces the dissolution of raw materials, the generation and redissolution of zeolite precursors in the mixing process and the aging process of raw materials. In the mixing process and the aging process, in order to synthesize GIS-type zeolite with a suitable structure, the silicon oxide source is added successively, and it is important to control the initial nucleation in the synthesis of the zeolite precursor. In the mixing process and the aging process, the ratio of the molar amount S1 of the silicon oxide source present in the initial state of the mixed gel containing the silicon oxide source, the aluminum source and water to the molar amount S2 of the silicon oxide source in the gel supplied to the hydrothermal synthesis process is particularly important. When the molar ratio is set to ψ, it is expressed as ψ=S1 / S2. By making ψ within a suitable range and controlling the initial nucleation, the bonding mode and existence ratio of Si and Al in the zeolite framework can be adjusted, and a GIS with an ideal crystal structure can be synthesized. From the above aspects, ψ is preferably less than 0.90, more preferably less than 0.80, and further preferably less than 0.50. There is no particular restriction on the lower limit of ψ, but if ψ is too small, the generation of impurities such as ANA-type zeolite will increase, and GIS may not be generated. Therefore, ψ is preferably greater than 0.05, more preferably greater than 0.08, and further preferably greater than 0.10. It is preferred that the raw materials are fully mixed and the raw material gel is in a uniform state. In order to obtain a zeolite with a suitable structure, the time for the mixing step and the aging step combined can be appropriately adjusted based on the composition of the raw materials, etc., and is not particularly limited. The above time is representatively preferably greater than 1 minute and less than 24 hours, more preferably greater than 3 minutes and less than 23 hours, further preferably greater than 10 minutes and less than 18 hours, further preferably greater than 12 minutes and less than 15 hours, and further preferably greater than 20 minutes and less than 6 hours.

[0133] [Hydrothermal synthesis process]

[0134] The method for producing GIS-type zeolite of the present embodiment preferably further comprises a hydrothermal synthesis step at a hydrothermal synthesis temperature of 80° C. to 200° C., and the hydrothermal synthesis temperature is more preferably 100° C. to 180° C. That is, the mixed gel obtained by the preparation step is preferably subjected to hydrothermal synthesis by being kept at a predetermined temperature for a predetermined time in a stirring or static state.

[0135] The temperature of the hydrothermal synthesis is not particularly limited as long as it is a temperature commonly used, but is preferably 80° C. or higher from the perspective of shortening the synthesis time and being economical in the production of zeolite. From the perspective of being able to suppress the formation of zeolites having a framework different from the GIS-type framework, it is more preferably 90° C. or higher, and even more preferably 100° C. or higher. From the perspective of being able to suppress the formation of zeolites having a framework different from the GIS-type framework, it is more preferably 200° C. or lower, even more preferably 180° C. or lower, and even more preferably 170° C. or lower. The temperature of the hydrothermal synthesis may be constant or may be changed in stages.

[0136] The time of the hydrothermal synthesis is not particularly limited as long as it is a time commonly used, and can be appropriately selected according to the temperature of the hydrothermal synthesis. The time of the hydrothermal synthesis is preferably 3 hours or more, more preferably 10 hours or more, from the aspect of forming the GIS skeleton. From the aspect of obtaining a highly crystalline GIS-type zeolite, it is further preferably 24 hours or more. From the aspect of excellent economic efficiency during zeolite production, the time of the hydrothermal synthesis is preferably 30 days or less, more preferably 20 days or less, and further preferably 10 days or less.

[0137] In the hydrothermal synthesis step, the container for placing the mixed gel is not particularly limited as long as it is a commonly used container, but when the pressure in the container is increased at a predetermined temperature, or when the gas that does not hinder crystallization is pressurized, it is preferably placed in a pressure-resistant container for hydrothermal synthesis. The pressure-resistant container is not particularly limited, and various shapes such as spherical, vertically elongated, and horizontally elongated can be used.

[0138] When the mixed gel in the pressure-resistant container is stirred, the pressure-resistant container is rotated in the vertical direction and / or the horizontal direction, preferably in the vertical direction. When the pressure-resistant container is rotated in the vertical direction, the rotation speed is not particularly limited as long as it is within the commonly used range, preferably 1 to 50 rpm, more preferably 10 to 40 rpm.

[0139] In the hydrothermal synthesis step, when the mixed gel is preferably stirred, there can be mentioned a method of using a vertically long container as a pressure-resistant container and rotating the container in the up-and-down direction.

[0140] [Separation and drying process]

[0141] After the hydrothermal synthesis step, the solid product and the liquid containing water are separated. The separation method is not particularly limited as long as it is a common method, and filtration, decantation, spray drying (rotary spray, nozzle spray and ultrasonic spray, etc.), drying using a rotary evaporator, vacuum drying, freeze drying or natural drying, etc. can be used. Separation can usually be carried out by filtration or decantation.

[0142] The separated product can be used directly or washed with water or a prescribed solvent. The separated product can be dried if necessary. The temperature for drying the separated product is not particularly limited as long as it is a temperature at which drying is usually performed, and is usually room temperature to below 150° C. The atmosphere during drying is not particularly limited as long as it is a commonly used atmosphere, and an air atmosphere or an atmosphere containing an inert gas such as nitrogen or argon or oxygen is usually used.

[0143] [Firing process]

[0144] GIS type zeolite can be used after being calcined as needed. The calcination temperature is not particularly limited as long as it is a commonly used temperature. When it is desired to remove the organic structure directing agent, it is preferably 300°C or more, more preferably 350°C or more, because it can reduce the residual ratio. From the perspective of shortening the calcination time and excellent economic efficiency when manufacturing zeolite, it is more preferably 360°C or more. Because it tends to maintain the crystallinity of the zeolite, it is preferably less than 450°C, more preferably 420°C or less, and even more preferably 400°C or less.

[0145] The calcination time is not particularly limited as long as it is a time that can sufficiently remove the organic structure directing agent, and can be appropriately selected according to the calcination temperature. Since it tends to reduce the residual ratio of the organic structure directing agent, it is preferably 0.5 hours or more, more preferably 1 hour or more, and even more preferably 3 hours or more. Since it tends to maintain the crystallinity of the zeolite, it is preferably 10 days or less, more preferably 7 days or less, and even more preferably 5 days or less.

[0146] The firing atmosphere is not particularly limited as long as it is a commonly used atmosphere, and an air atmosphere, an atmosphere to which an inert gas such as nitrogen or argon or oxygen is added is usually used.

[0147] [Cation Exchange]

[0148] Cation exchange can be performed as needed to make the GIS type zeolite a desired cationic type. Cation exchange can use, but is not limited to, carbonates such as sodium carbonate, potassium carbonate, lithium carbonate, rubidium carbonate, cesium carbonate, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, and ammonium carbonate; or nitrates such as sodium nitrate, potassium nitrate, lithium nitrate, rubidium nitrate, cesium nitrate, magnesium nitrate, calcium nitrate, strontium nitrate, barium nitrate, and ammonium nitrate; or salts formed by changing the carbonate ions and nitrate ions contained in the above carbonates and nitrates to halide ions, sulfate ions, carbonate ions, bicarbonate ions, acetate ions, phosphate ions, or hydrogen phosphate ions; acids such as nitric acid or hydrochloric acid. From the aspect of improving the selective adsorption capacity of carbon dioxide, it is preferred to include potassium atoms as cationic species in the zeolite.

[0149] The temperature for cation exchange is not particularly limited as long as it is a normal cation exchange temperature, and is usually room temperature to 100° C. or lower.

[0150] When separating the zeolite after cation exchange, the separation method is not particularly limited as long as it is a common method, and filtration, decantation, spray drying (rotary spray, nozzle spray and ultrasonic spray, etc.), drying using a rotary evaporator, vacuum drying, freeze drying or natural drying, etc. can be used. Separation can usually be carried out by filtration or decantation.

[0151] The separated product can be used directly or washed with water or a specified solvent. If necessary, the separated product can be dried.

[0152] The temperature for drying the separated product is not particularly limited as long as it is a normal drying temperature, and is usually room temperature to 150° C. or lower.

[0153] The atmosphere during drying is not particularly limited as long as it is a commonly used atmosphere, and generally, an air atmosphere, an atmosphere to which an inert gas such as nitrogen or argon or oxygen is added is used.

[0154] [Zeolite Molded Body]

[0155] The zeolite molded body of the present embodiment contains the above-mentioned GIS-type zeolite.

[0156] The preferred content of GIS type zeolite may be 50% by mass or more, 60% by mass or more, 70% by mass or more, or 80% by mass or more relative to the total amount 100% by mass of the zeolite molded body. In addition, the content of GIS type zeolite may be 99% by mass or less, 95% by mass or less, or 92% by mass or less relative to the total amount 100% by mass of the zeolite molded body.

[0157] [Carrier]

[0158] The zeolite molded body of the present embodiment preferably includes a carrier. Examples of the carrier include inorganic binders and organic binders.

[0159] As inorganic binders, for example, inorganic oxides such as aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, titanium dioxide, clay minerals such as bentonite and kaolin, calcium silicate, and calcium aluminate can be cited. As aluminum oxide, for example, α-alumina, γ-alumina, boehmite, pseudo-boehmite, bayerite, gibbsite, and diaspore can be cited. As silicon oxide, for example, colloidal silica, water glass, gas phase silica, silica sol, wet silica, dry silica, and natural silica can be cited. These inorganic binders can be used alone or in combination. Among these inorganic binders, aluminum oxide, silicon oxide, magnesium oxide, zirconium oxide, and titanium dioxide are preferred from the aspect of improving the strength of the zeolite molded body, and silicon oxide and aluminum oxide are more preferred.

[0160] The content of the inorganic binder is preferably 1 to 90 mass %, more preferably 1 to 50 mass %, further preferably 5 to 40 mass %, and further preferably 8 to 30 mass % based on 100 mass % of the total amount of the zeolite molded body.

[0161] As organic binder, for example, cellulose, methylcellulose, carboxymethylcellulose, hydroxyethylcellulose, latex, polyvinyl alcohol, vinyl acetate, polyvinyl acetal, vinyl chloride, acrylic, polyamide, urea, melamine, phenol resin, polyester, polyurethane, polyamide, polybenzimidazole, chloroprene rubber, acrylonitrile-butadiene rubber, styrene-butadiene rubber, polysulfide, butyl rubber, silicone rubber, acrylic rubber, urethane rubber can be enumerated. These organic binders can be used alone, and a plurality of combinations can also be used. Among these organic binders, from the aspect of the surface bonding with GIS type zeolite, preferably cellulose, methylcellulose, carboxymethylcellulose, hydroxyethylcellulose, polyvinyl alcohol, more preferably cellulose, methylcellulose and polyvinyl alcohol.

[0162] The content of the organic binder is preferably 1 to 90 mass %, more preferably 1 to 50 mass %, further preferably 5 to 40 mass %, and further preferably 8 to 30 mass %, based on 100 mass % of the total amount of the GIS-type zeolite molded body.

[0163] The carrier preferably contains an inorganic binder and an organic binder. That is, it is preferred that the inorganic binder and the organic binder each contain one or more.

[0164] The total content of the carriers is preferably 1 to 90% by mass, more preferably 1 to 50% by mass, further preferably 5 to 40% by mass, and further preferably 8 to 30% by mass, relative to the total amount of the zeolite molded body (100% by mass). If the content of the carriers is increased, the strength of the molded body tends to increase, but the content of the zeolite itself tends to decrease. Therefore, the content of the carriers can be adjusted according to the strength and performance required for the application.

[0165] The shape of the zeolite molded body is not particularly limited, and examples thereof include spherical, cylindrical, elliptical, bale-shaped, trilobal, annular, powdery, and the like. Among these, spherical and cylindrical shapes are more preferred. The size of the molded body is not particularly limited and varies depending on the conditions in which the molded body is used. For example, in a process using a molded body other than a fluid state such as a fixed bed or a moving bed, a cylindrical shape having a length of 3 mm to 30 mm and a diameter of 1 mm to 30 mm is preferred. The length of the cylinder is more preferably 3 mm to 10 mm, and further preferably 3 mm to 8 mm. The diameter of the cylinder is more preferably 2 mm to 4 mm.

[0166] The length and diameter can be measured by the vernier caliper method using a vernier caliper with a minimum reading of 0.1 mm or less for three samples, and the average values ​​can be measured as the length and diameter, which can be adjusted to the above range by operations such as classification.

[0167] In the process of using a fluidized bed or the like to flow the molded body, particles having a particle size of 20 μm or more and 300 μm or less are preferred. The particle size is more preferably 20 μm or more and 200 μm or less, and further preferably 30 μm or more and 100 μm or less. The particle size can be measured in the form of median diameter (D50) using a laser diffraction / scattering particle size analyzer (MT3000 manufactured by Microtrac) according to the attached operating manual.

[0168] The compressive strength of the zeolite molded body of the present embodiment is preferably 1.0 MPa or more, more preferably 2.2 MPa or more, and even more preferably 3.4 MPa or more. In particular, when the zeolite molded body of the present embodiment is in powder form, it preferably satisfies the above range.

[0169] The compressive strength can be measured 20 times using a micro compression tester (MCT-W500 manufactured by Shimadzu Corporation, compression strength measurement) and measured as an average of the obtained values, and can be adjusted to the above range by, for example, the firing temperature and firing time.

[0170] The breaking strength of the zeolite molded body of the present embodiment is preferably 5 N or more, more preferably 10 N or more, and further preferably 20 N or more. In particular, when the zeolite molded body of the present embodiment is a pellet, it preferably satisfies the above range.

[0171] The above-mentioned breaking strength can be measured 20 times using a digital hardness meter (KHT-40N manufactured by Fujiwara Manufacturing Co., Ltd., with a 3 mm indenter and breaking strength measurement), and the measurement is performed as an average value of the obtained values. The above-mentioned range can be adjusted by, for example, the firing temperature and the firing time.

[0172] [Method for producing zeolite molded body]

[0173] The method for producing the zeolite molded body of the present embodiment is not particularly limited and may include the following steps: a raw material mixing step (X), in which the GIS-type zeolite of the present embodiment is mixed with other optional components (e.g., a carrier) for preparation; a molding treatment step (Y), in which the prepared raw materials are subjected to molding treatment to obtain a precursor; and a firing step (Z), in which the above-mentioned precursor is fired to obtain a zeolite molded body.

[0174] In addition, as a method for producing a zeolite molded body, when obtaining the desired zeolite molded body, molding can be performed, for example, by extrusion molding, injection molding, injection casting, tumbling granulation, compression molding, spray drying, or a method in which two or more of these methods are combined.

[0175] [Raw material mixing step (X)]

[0176] In the raw material mixing step (X), the raw materials used can be used in a state corresponding to the preparation method, such as powder, solvent dispersion, sol, liquid, etc. Among the raw materials used, for example, when an inorganic adhesive is used, it is used in a state corresponding to the preparation method, such as powder, solvent dispersion, sol, liquid, etc., but from the perspective of ease of handling, powder and sol are preferred. These inorganic adhesives can be used alone or in combination. The temperature for mixing the raw materials is not particularly limited, for example, preferably 10°C to 80°C, more preferably 15°C to 60°C. For example, if the state of the raw materials after mixing is a slurry, such as spray drying, when the temperature of the raw materials is below 80°C, there is a tendency to suppress the evaporation of water in the raw materials, and when the temperature of the raw materials is above 10°C, there is a tendency to suppress freezing in the slurry. In addition, for example, if the raw materials are mixed in a clay state from a chain state to a capillary state, such as in an extrusion molding process, when the temperature of the raw materials is below 80°C, there is a tendency to suppress the evaporation of water from the clay and easily keep the water content in the clay constant. When the temperature of the raw materials is above 10°C, there is a tendency to suppress the freezing of water in the clay. As a stirring means when preparing the raw materials, any means can be used. For example, if the state of the raw materials after mixing is a slurry, such as in a spray drying process, a stirring paddle is preferably cited. As the paddle used in stirring, specifically, a propeller shape, an impeller shape, a flat blade paddle shape, a turbine shape, a cone shape, etc. can be cited. In addition, in order to perform effective stirring, a baffle plate, etc. can be set in the tank. Regarding the number of stirrers, the optimal conditions can be selected according to the size of the catalyst raw material liquid tank, the shape of the stirring paddle, etc. In this embodiment, the total stirring time of the raw materials is preferably 1 minute to 24 hours, more preferably 10 minutes to 5 hours, and further preferably 15 minutes to 3 hours. When the stirring time of the mixed solution is more than 1 minute, the composition of the raw materials tends to become uniform; when it is less than 24 hours, the influence of the evaporation of water in the raw materials tends to decrease. In addition, for example, in the case of a clay-like state from a chain state to a capillary state after the raw materials are mixed, such as in an extrusion molding process, it is preferred to select a mixer, a kneading machine, etc. according to the state of the raw materials. In the present embodiment, the total mixing and kneading time of the raw materials is preferably 1 minute to 24 hours, more preferably 2 minutes to 5 hours, and further preferably 3 minutes to 3 hours. When the stirring time of the mixed solution is more than 1 minute, the composition of the raw materials tends to become uniform, and when it is less than 24 hours, the influence of the evaporation of water in the raw materials tends to decrease. In addition, in the case of an organic binder such as methyl cellulose that is easily gelled due to heat, the gelation of the organic binder can be suppressed by maintaining the internal temperature of the mixer, the kneading machine, etc. at a value lower than the thermal gelation temperature of the organic binder, and there is a tendency to easily obtain a raw material of uniform composition.

[0177] The clay-like raw material may be left to stand and mature. By aging, water can easily reach between the raw zeolites, which tends to improve the moldability. In addition, water can be replaced with air or other gas existing between the zeolites to obtain a denser molded body.

[0178] [Molding process (Y)]

[0179] Examples of the molding treatment in the molding treatment step (Y) include extrusion molding treatment, compression molding treatment, and spray drying treatment.

[0180] The extrusion molding process is not particularly limited. For example, depending on the properties of the raw material used (also referred to as "raw clay" in the extrusion molding process), the temperature during extrusion molding is preferably 10° C. to 80° C., and more preferably 15° C. to 75° C. The water content in the raw clay is preferably 35% to 50% by mass, and more preferably 38% to 45% by mass. When the water content is 50% by mass or less, the softness of the raw clay can be prevented from being excessively increased, and the moldability tends to be improved. When the water content is 35% by mass or more, the softness of the raw clay can be prevented from being moderately reduced, and the moldability tends to be improved.

[0181] When extrusion molding is used as the molding process step (Y), there is no particular limitation on the extrusion molding machine, and examples thereof include screw type, roller type, scraper type, self-molding type, plunger type, disc granulation type, etc. Among these, it is particularly preferred to implement the extrusion molding process using a roller type, screw type, or disc granulation type extrusion molding machine.

[0182] When compression molding is used as the molding step (Y), the compression molding machine is not particularly limited, and examples thereof include uniaxial press molding, hot press molding, and the like.

[0183] In the spray drying process, for example, the atomization of the slurry can be carried out by methods such as a rotating disk method, a two-fluid nozzle method and a high-pressure nozzle method which are usually implemented in industry, and is particularly preferably carried out by a rotating disk method. As a drying heat source in the drying of the droplets obtained by spraying, air heated by steam, an electric heater, etc. is preferably used. The temperature at the inlet of the dryer can be in the range of 100°C to 400°C, preferably 150°C to 300°C. The temperature at the outlet of the dryer can be in the range of 40°C to 150°C, preferably 50°C to 130°C.

[0184] [Firing process (Z)]

[0185] The firing temperature in the firing step (Z) is not particularly limited as long as it is a temperature commonly used, but is preferably less than 550° C., more preferably 530° C. or less, and even more preferably 500° C. or less, because it tends to maintain the crystallinity of the zeolite while ensuring strength. The firing temperature is preferably 110° C. or more, and more preferably 120° C. or more.

[0186] The calcination time in the calcination step (Z) is not particularly limited as long as it is a time for the carrier to be fully dried or sintered, and can be appropriately selected according to the calcination temperature. Since it tends to be able to maintain the crystallinity of the zeolite while ensuring the strength, it is preferably 20 days or less, more preferably 10 days or less, and even more preferably 7 days or less.

[0187] The firing atmosphere in the firing step (Y) is not particularly limited as long as it is an atmosphere commonly used, and an air atmosphere, an atmosphere to which an inert gas such as nitrogen or argon or oxygen is added is usually used.

[0188] The firing in the firing step (Z) can be performed using a firing furnace such as a rotary furnace, a tunnel furnace, or a muffle furnace.

[0189] The use of the GIS-type zeolite of this embodiment is not particularly limited, and it can be used, for example, as a separator or separation membrane for various gases and liquids, an electrolyte membrane for fuel cells, etc., a filler for various resin molded bodies, a membrane reactor, or a catalyst for hydrogen cracking, alkylation, etc., a catalyst carrier for loading metals, metal oxides, etc., an adsorbent, a desiccant, a detergent builder, an ion exchanger, a wastewater treatment agent, a fertilizer, a food additive, a cosmetic additive, etc.

[0190] Among the above, the GIS-type zeolite of the present embodiment can be suitably used as a carbon dioxide adsorbent.

[0191] [Adsorption device]

[0192] The adsorption device of the present embodiment includes the zeolite molded body of the present embodiment. Since the adsorption device of the present embodiment is configured as described above, carbon dioxide can be sufficiently adsorbed, and the selectivity of carbon dioxide adsorption relative to the adsorption amount of methane is high. Therefore, for example, it can be particularly preferably used for the purpose of selectively removing carbon dioxide from natural gas.

[0193] The adsorption device of the present embodiment includes a zeolite molded body including the GIS type zeolite of the present embodiment, which can be Figure 2 The configuration example shown. Figure 2The adsorption device 1 of the present embodiment illustrated in the example has filters 3 arranged at both the inlet side and the outlet side, and a plurality of zeolite molded bodies 4 filled between the two filters 3, inside the container 2. As the filter 3, for example, a filter made of quartz can be used. For example, when the adsorption device 1 is used to separate carbon dioxide from natural gas, natural gas can be introduced from an upper pipeline, and after impurities are removed by the filter 3, carbon dioxide is further selectively adsorbed and removed by the zeolite molded body 4, and methane-rich gas is taken out from the lower pipeline. However, the object supplied to the adsorption device is not limited to natural gas, and the internal structure of the adsorption device is not limited to natural gas. Figure 2 Example shown.

[0194] [Method for producing purified gas]

[0195] In the method for producing a purified gas of the present embodiment, an adsorption device including the GIS type zeolite of the present embodiment is used to separate one or more selected from the group consisting of CO2, H2O, He, Ne, Cl2, NH3 and HCl from a mixture containing two or more gases selected from the group consisting of H2, N2, O2, CO and hydrocarbons. In the present embodiment, it is preferred to separate one or more selected from the group consisting of CO2 and H2O from one or more gases selected from the group consisting of N2, O2, CO and hydrocarbons. It should be noted that the hydrocarbon is not particularly limited, and examples thereof include methane, ethane, ethylene, propane, propylene, 1-butene, 2-butene, 2-methylpropylene, dimethyl ether, acetylene and the like.

[0196] In the GIS type zeolite of the present embodiment, the adsorption capacity of CO2 is large, and physical adsorption without chemical bonding is observed. There is no particular limitation on the separation method using the GIS type zeolite of the present embodiment, and a method with low energy and excellent economic efficiency during the regeneration of the adsorbent material is preferred. There is no particular limitation on the specific example of the method, and it is preferred to use any one of a pressure swing adsorption separation method, a temperature swing adsorption separation method, or a pressure swing-temperature swing adsorption separation method. The pressure swing adsorption separation method (PSA: Pressure Swing Adsorption) refers to the following method: the pressure during gas desorption is lower than the pressure during adsorption, and the gas is separated by using the difference between the adsorption amount at high pressure and the adsorption amount at low pressure. In addition, the temperature swing adsorption separation method (TSA: Thermal Swing Adsorption) refers to the following method: the temperature during gas desorption is higher than the temperature during adsorption, and the gas is separated by using the difference between the adsorption amount at low temperature and the adsorption amount at high temperature. In addition, the method of combining them is a pressure swing-temperature swing adsorption separation method (PTSA: Pressure and Thermal Swing Adsorption). These methods can be implemented under various known conditions.

[0197] Example

[0198] The present embodiment will be described in more detail below with reference to Examples and the like, but these are merely illustrative and the present embodiment is not limited to the following Examples.

[0199] [X-ray diffraction; crystal structure analysis (P CO2 , P de )]

[0200] X-ray diffraction was performed by the following steps.

[0201] (1) The zeolite molded body obtained in each example and comparative example (dried product after treatment at 350°C for 24 hours) was used as a sample and crushed using an agate mortar. Furthermore, 10% by mass of crystalline silicon (manufactured by Rare Metallic Co., Ltd.) was added to the zeolite molded body (dried product), and mixed using an agate mortar until it became uniform, and the mixture was used as a sample for structural analysis.

[0202] (2) The sample of (1) above is placed in a quartz capillary (0.5 mm Φ), installed in a sample holder connected to a N2 storage bottle, a CO2 storage bottle, a vacuum pump, and a pressure gauge by means of gas piping, and then installed in an X-ray diffraction device and measured under the following conditions.

[0203] X-ray diffraction apparatus (XRD): Powder X-ray diffraction apparatus "Ultima-IV" (trade name) manufactured by Rigaku Corporation

[0204] Determination method: permeation method

[0205] X-ray source: Cu tube (40kV, 40mA)

[0206] Measuring range: 5~90°(0.02° / step)

[0207] Measuring speed: 0.5° / min

[0208] Slit width (scattering, divergence, light receiving): Release 1°

[0209] (3) The diffraction peak P based on X-ray diffraction in the dehydrated state and nitrogen adsorption conditions de The measurement was performed by the following steps.

[0210] The nitrogen gas heated by the heater was directly blown into the capillary tube containing the sample, and the temperature was calibrated to 350°C using a thermocouple. The pressure in the sample holder was further reduced to 1.0 mmHg using a vacuum pump. After the temperature and vacuum were maintained for 3 hours, N2 was introduced from the N2 storage bottle into the sample holder, and after the temperature was cooled to 25°C, X-ray diffraction was measured. The diffraction peak with the strongest intensity observed between the diffraction angles 2θ = 25.81 and 34.57° according to the obtained spectrum was set as P de .

[0211] (4) Diffraction peak P based on X-ray diffraction under dehydrated state and carbon dioxide adsorption conditions CO2 The measurement was performed by the following steps.

[0212] The nitrogen gas heated by the heater is blown directly into the capillary tube containing the sample, and the temperature is calibrated to 350°C using a thermocouple. The pressure in the sample rack is further reduced to 1.0 mmHg using a vacuum pump. After the temperature and vacuum are maintained for 3 hours, N2 is introduced into the sample rack from an N2 storage bottle, and the temperature is cooled to 25°C. The pressure in the sample rack is again reduced to 1.0 mmHg using a vacuum pump, and CO2 is then introduced into the sample rack from a CO2 storage bottle so that the pressure in the sample rack is 300 kPa, and X-ray diffraction is measured. The diffraction angle (2θ) of the diffraction peak with the strongest intensity in the obtained spectrum is set as P CO2 .

[0213] [ 29 Si-MAS-NMR spectrum, SAR measurement]

[0214] The SAR of the zeolite in the zeolite molded body can be determined by 29 First, as a humidity control for the zeolite, the bottom of the desiccator was filled with water, and the zeolite placed in the test tube was kept at the top for 48 hours. After the humidity control, the zeolite was tested under the following conditions. 29 Determination of Si-MAS-NMR.

[0215] Device: JEOL RESONANCE ECA700

[0216] Magnetic field strength: 16.44T( 1 H resonance frequency 700MHz)

[0217] Determination of the core: 29 Si

[0218] Resonance frequency: 139.08MHz

[0219] NMR tube: 4mm Ф (zirconia rotor)

[0220] Measurement method: DD / MAS (dipolar decoupling magic angle spinning)

[0221] Pulse width: 45°

[0222] Waiting time: 50 seconds

[0223] Integration times: 800 times (measurement time: about 22 hours)

[0224] MAS: 10,000Hz

[0225] Chemical shift standard: Silicone rubber (-22.34ppm) external standard

[0226] In the molded body comprising GIS type zeolite, 29 The Si-MAS-NMR spectrum showed the following five peaks.

[0227] (1) Q4 (0Al): Peak of Si that is not bonded to Al via oxygen

[0228] (2) Q4 (1Al): Peak of Si bonded to one Al via oxygen

[0229] (3) Q4 (2Al): Peak of Si bonded to two Al atoms via oxygen

[0230] (4) Q4 (3Al): Peak of Si bonded to three Al atoms via oxygen

[0231] (5) Q4 (4Al): Peak of Si bonded to four Al atoms via oxygen

[0232] In addition, 29 In the Si-MAS-NMR spectrum, these peak positions are usually present in the range of -112ppm to -80ppm, and can be assigned to Q4(0Al), Q4(1Al), Q4(2Al), Q4(3Al), and Q4(4Al) from the high magnetic field side. The peak positions may vary depending on the cationic species present in the zeolite framework, but the peak positions are usually present in the following ranges.

[0233] (1) Q4(0Al): -105ppm to -112ppm

[0234] (2) Q4(1Al): -100ppm to -105ppm

[0235] (3) Q4 (2Al): -95ppm to -100ppm

[0236] (4) Q4 (3Al): -87ppm to -95ppm

[0237] (5) Q4 (4Al): -80 ppm to -87 ppm

[0238] about 29 The peak area intensity of the Si-MAS-NMR spectrum was analyzed by Gaussian and Lorentzian functions using the analysis program dmfit (version #202000113), and the four parameters of amplitude (height of the maximum value of the spectrum), position (spectral position, ppm), width (full width at half maximum of the spectrum, ppm), and Gaussian / Lorentzian ratio (xG / (1-x)L) were optimized and calculated by the least squares algorithm. When the peak areas of Q4(0Al), Q4(1Al), Q4(2Al), Q4(3Al), and Q4(4Al obtained in this way are each taken as A_Q4(0Al), A_Q4(1Al), A_Q4(2Al), A_Q4(3Al), and A_Q4(4Al), and the total value of A_Q4(0Al), A_Q4(1Al), A_Q4(2Al), A_Q4(3Al), and A_Q4(4Al) is taken as A_total, SAR can be obtained as follows.

[0239] SAR=100 / [A_Q4(1Al) / 4+2×A_Q4(2Al) / 4+3×A_Q4(3Al) / 4+4×A_Q4(4Al) / 4]×2

[0240] [Evaluation of embrittlement resistance of zeolite molded bodies in CO2 atmosphere]

[0241] The embrittlement resistance of the zeolite molded bodies obtained in Examples and Comparative Examples in a CO 2 atmosphere was evaluated by the following procedure.

[0242] (1) 100 g of a zeolite molded body is weighed and the short diameter of the zeolite molded body is measured. The average value of the short diameter of the zeolite molded body is taken as ds. A sieve having a mesh size smaller than ds and having the largest mesh size is selected and prepared according to the mesh size disclosed in JIS Z 8801-1. The zeolite molded body remaining on the sieve after the sieving is used for evaluation of embrittlement resistance under a CO2 atmosphere. This is used as a test sample.

[0243] (2) The test sample was dried in a N2 atmosphere at 200°C for 3 hours. After cooling to room temperature in the N2 atmosphere, it was exposed to CO2 at room temperature for 30 minutes.

[0244] (3) After measuring the mass W1 of the test sample after CO2 exposure, the sample is sieved using the above-mentioned mesh size sieve, and the mass W2 of the zeolite molded body that has passed the sieve is measured. The value calculated using formula (1) is defined as the pulverization rate [mass %] of the zeolite molded body. The lower the pulverization rate of the zeolite molded body, the more resistant it is to embrittlement in a CO2 atmosphere.

[0245] [Number 1]

[0246]

[0247] [Alkali metal content]

[0248] The concentrations of aluminum and potassium in the zeolite were measured by ICP-atomic emission spectrometry (hereinafter referred to as "ICP-AES", SPS3520UV-DD manufactured by Hitachi High-Tech Science Co., Ltd.: device name) using a liquid obtained by heat-dissolving the zeolite with an aqueous sodium hydroxide solution or aqua regia and then diluting it appropriately. The potassium and lithium contents in the zeolite were calculated as a ratio (Z / T) of the total amount of potassium and lithium in the zeolite (Z) to the total amount of each alkali metal (T). K / T was calculated in the same manner.

[0249] [CO2 adsorption and hysteresis; gas adsorption-desorption isotherm determination]

[0250] The gas adsorption-desorption isotherm measurement was performed by the following procedure.

[0251] (1) 0.2 g of the zeolite molded body obtained in each of Examples and Comparative Examples (dried product after treatment at 350° C. for 24 hours) was added as a sample to a 12 mm sample cell (manufactured by Micro Meritics).

[0252] (2) The sample put into the sample cell in (1) above was placed in a gas adsorption measuring device "3-Flex" (trade name) manufactured by Micro Meritics, and subjected to a heating vacuum degassing treatment at 250°C and 0.001 mmHg or less for 12 hours.

[0253] (3) The sample added to the sample cell after the treatment in (2) above is placed in a constant temperature circulating water at 25°C. After the temperature of the sample reaches 25±0.2°C, it is measured using liquefied carbon dioxide (manufactured by Sumitomo Seika Co., Ltd., purity 99.9% by mass or more) at an absolute pressure of 0.25 to 760 mmHg. It should be noted that in the above measurement, the pressure is measured over time, and when the pressure change is less than 0.001% / 10sec, it is determined that the saturated adsorption amount has been reached, and this is taken as the CO2 adsorption amount at 25°C (unit: cm3 / g).

[0254] (4) Following the measurement in (3), the pressure was reduced over time at an absolute pressure of 760 to 0.25 mmHg to measure the desorption isotherm of carbon dioxide. It should be noted that, as an equilibrium determination, the measurement was performed with the pressure change being 0.001% / 10 sec or less as in (3).

[0255] (5) As an index indicating the hysteresis amount in the carbon dioxide adsorption-desorption isotherm, when the equilibrium adsorption amount at 75 mmHg of the adsorption isotherm measured in (3) and the equilibrium adsorption amount at 75 mmHg of the desorption isotherm measured in (4) are respectively set to q(Ad) and q(De), q(Ad) / q(De) is used as an index indicating the hysteresis amount. When q(Ad) / q(De)=1.00, it indicates no hysteresis, and the smaller q(Ad) / q(De), the larger the hysteresis.

[0256] [CH4 adsorption; gas adsorption isotherm determination]

[0257] The gas adsorption isotherm measurement was performed by the following procedure.

[0258] (1) The dried product obtained in each of the Examples and Comparative Examples was used as a sample, and 0.2 g of the dried product was added to a 12 mm sample cell (manufactured by MicroMeritics).

[0259] (2) The sample put into the sample cell in (1) above was placed in a gas adsorption measuring device "3-Flex" (trade name) manufactured by Micro Meritics, and subjected to a heating vacuum degassing treatment at 250°C and 0.001 mmHg or less for 12 hours.

[0260] (3) The sample added to the sample cell after the treatment in (2) above is placed in a constant temperature circulating water at 25°C. After the temperature of the sample reaches 25±0.2°C, it is measured using methane gas (manufactured by Fujii Shoji Co., Ltd., purity 99.99% by mass or more) at an absolute pressure of 0.25 to 760 mmHg. It should be noted that in the above measurement, the pressure is measured over time, and when the pressure change is less than 0.001% / 10sec, it is determined that the saturated adsorption amount has been reached, and this is taken as the CH4 adsorption amount at 25°C (unit: cm 3 / g).

[0261] [Example 1]

[0262] 61.93 g of water, 0.202 g of sodium hydroxide (NaOH, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), 3.39 g of sodium nitrate (NaNO3, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), 1.64 g of sodium aluminate (NaAlO2, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.) and 5.41 g of colloidal silica (Ludox AS-40, solid content concentration 40% by mass, manufactured by Grace Co., Ltd.) were mixed and stirred for 24 hours, and then 5.41 g of colloidal silica (Ludox AS-40, solid content concentration 40% by mass, manufactured by Grace Co., Ltd.) was added and stirred for 30 minutes to prepare a mixed gel. The composition of the mixed gel is α=(L12O+L2O) / SiO2=0.00, β=OH - / (M12O+M2O)=0.14, γ=SiO2 / Al2O3=8.17, δ=H2O / Al2O3=431.0, ε=P2O5 / Al2O3=0.00, ζ=R / Al2O3=0.00, ψ=S1 / S2=0.50. The mixed gel was put into a 200mL stainless steel micro-storage bottle (manufactured by HIRO COMPANY) with a fluororesin inner cylinder, and hydrothermal synthesis was carried out for 4 days at a stirring speed of 30rpm and 135°C using a stirring thermostatic bath (manufactured by HIRO COMPANY) that can rotate along the up and down directions of the micro-storage bottle. The product was filtered out and dried at 120°C to obtain a powdered zeolite. The obtained zeolite was confirmed to be a GIS type zeolite by XRD spectrum. In addition, no peaks derived from other zeolites or amorphous silica-alumina were observed, so it was evaluated as a high-purity GIS type zeolite.

[0263] The obtained zeolite is used 29 The Si-MAS-NMR spectrum calculated the silicon oxide-aluminum oxide ratio, and the result was SAR = 6.92, and (a+d) / (b+c) = 0.305. The potassium and lithium contents in the zeolite were Z / T = 0.00 (= K / T). The above-mentioned X-ray diffraction measurement was also performed, and the result was P CO2 =28.84, P de =28.86, P CO2 / P de =1.00.

[0264] 40 parts by mass of the GIS type zeolite obtained by synthesis, 1.2 parts by mass of methyl cellulose (Serander YB-132A manufactured by Highchem Co., Ltd.), 0.2 parts by mass of polyvinyl alcohol (Gohsenol N-300 manufactured by Mitsubishi Chemical Corporation), 10.4 parts by mass of powdered alumina hydrate (manufactured by JGC Catalysts & Chemicals Co., Ltd., alumina content: 70% by mass), and 48.2 parts by mass of alumina sol (manufactured by Nissan Chemical Co., Ltd., alumina content: 10.5% by mass) were mixed.

[0265] The mixture was manually extruded into a cylindrical shape with a diameter of 3 mm using a clay gun, and then fired in an electric furnace at 350° C. for 24 hours in an air atmosphere. The pulverization rate of the GIS-type zeolite molded body thus obtained was 0.1%.

[0266] When the CO2 desorption isotherm of the obtained GIS type zeolite molded body was measured, the adsorption amount at 760 mmHg was 59.6 cm 3 / g, q(Ad) / q(De)=1.000. In addition, when the adsorption isotherm of CH4 was measured in the same manner, the adsorption amount at 760 mmHg was 3.2 cm 3 / g.

[0267] [Example 2]

[0268] 61.65 g of water, 0.30 g of a 48% by mass sodium hydroxide aqueous solution (NaOH, manufactured by Tokuyama Soda Co., Ltd.), 2.27 g of sodium carbonate (Na2CO3, manufactured by Tokuyama Soda Co., Ltd.), 1.64 g of sodium aluminate (NaAlO2, manufactured by Hokuriku Chemical Industry Co., Ltd.) and 0.82 g of colloidal silica (Ludox AS-40, solid content concentration 40% by mass, manufactured by Grace Co., Ltd.) were mixed and stirred for 30 minutes, and then 10.00 g of colloidal silica (Ludox AS-40, solid content concentration 40% by mass, manufactured by Grace Co., Ltd.) was added and stirred for 30 minutes to prepare a mixed gel. The composition of the mixed gel is α=(L12O+L2O) / SiO2=0.00, β=OH - / (M12O+M2O)=0.10, γ=SiO2 / Al2O3=8.17, δ=H2O / Al2O3=431.2, ε=P2O5 / Al2O3=0.00, ζ=R / Al2O3=0.00, ψ=S1 / S2=0.082. The mixed gel was put into a 200 mL stainless steel micro-storage bottle (manufactured by HIRO COMPANY) with a fluororesin inner cylinder, and hydrothermal synthesis was carried out for 5 days at a stirring speed of 30 rpm and 130°C using a stirring thermostatic bath (manufactured by HIRO COMPANY) that can rotate along the micro-storage bottle in the up and down directions. The product was filtered out and dried at 120°C to obtain a powdered zeolite. 1 g of the obtained zeolite was added to 500 mL of a 0.05N potassium carbonate aqueous solution prepared using potassium carbonate (K2CO3, manufactured by Nippon Soda Co., Ltd.), and stirred at 500 rpm for 3 hours at room temperature. The product was filtered out and dried at 120°C to obtain a powdered zeolite in which a portion of the cations were exchanged for potassium. The obtained zeolite was confirmed to be a GIS type zeolite by XRD spectrum. In addition, no peaks derived from other zeolites, amorphous silica-alumina, etc. were observed, so it was evaluated as a high-purity GIS type zeolite.

[0269] The values ​​were measured using the same method as in Example 1. 29 Si-MAS-NMR spectrum, SAR = 7.20, and (a + d) / (b + c) = 0.244. The potassium and lithium contents in the zeolite are Z / T = 0.98 (= K / T). The above-mentioned X-ray diffraction measurement was also performed, and the results were P CO2 =29.02, P de =29.12, P CO2 / P de =0.997.

[0270] In addition, after molding in the same manner as in Example 1, the powderization rate of the obtained GIS type zeolite molded body was measured, and the powderization rate was 0.9%. When the CO2 desorption isotherm was measured, the adsorption amount at 760 mmHg was 61.0 cm 3 / g, q(Ad) / q(De)=1.000. When the adsorption isotherm of CH4 was measured in the same manner, the adsorption amount at 760 mmHg was 0.1 cm 3 / g.

[0271] [Example 3]

[0272] 141.41 g of water, 8.53 g of sodium nitrate (NaNO3, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.), 3.85 g of sodium aluminate (NaAlO2, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.) and 15.67 g of precipitated silica (Perkasil SM500, manufactured by Grace) were mixed and stirred for 60 minutes, and then 1.74 g of precipitated silica (Perkasil SM500, manufactured by Grace) was added and stirred for 15 minutes to prepare a mixed gel. The composition of the mixed gel is α=(L12O+L2O) / SiO2=0.00, β=OH - / (M12O+M2O)=0.00, γ=SiO2 / Al2O3=14.00, δ=H2O / Al2O3=379.3, ε=P2O5 / Al2O3=0.00, ζ=R / Al2O3=0.00, ψ=S1 / S2=0.90. The mixed gel was put into a 300mL stainless steel micro-storage bottle (manufactured by HIRO COMPANY) with a fluororesin inner cylinder, and hydrothermal synthesis was carried out for 4 days at a stirring speed of 30rpm and 130°C using a stirring thermostatic bath (manufactured by HIRO COMPANY) that can rotate along the up and down directions of the micro-storage bottle. The product was filtered out and dried at 120°C to obtain a powdered zeolite. The obtained zeolite was confirmed to be a GIS type zeolite based on the XRD spectrum. In addition, no peaks derived from other zeolites, amorphous silica-alumina, etc. were observed, so it was evaluated as a high-purity GIS type zeolite.

[0273] The values ​​were measured using the same method as in Example 1. 29 Si-MAS-NMR spectrum, SAR = 10.40, and (a + d) / (b + c) = 0.192. The potassium and lithium contents in the zeolite are Z / T = 0.00 (= K / T). The above-mentioned X-ray diffraction measurement was performed, and the result was P CO2 =28.60, P de =29.51, P CO2 / P de =0.969.

[0274] In addition, after molding in the same manner as in Example 1, the powderization rate of the obtained GIS type zeolite molded body was measured, and the powderization rate was 1.4%. When the CO2 desorption isotherm was measured, the adsorption amount at 760 mmHg was 58.0 cm 3 / g, q(Ad) / q(De)=1.000. In addition, when the adsorption isotherm of CH4 was measured in the same manner, the adsorption amount at 760 mmHg was 4.1 cm 3 / g.

[0275] [Comparative Example 1]

[0276] Based on the content of non-patent document 1, 143.10 g of water, 40.00 g of 50% sodium hydroxide aqueous solution (NaOH, solid content concentration 50% by mass, manufactured by Aldrich), 2.70 g of aluminum powder (Al, manufactured by Fujifilm-Wako Pure Chemical Industries, Ltd.) and 75.10 g of colloidal silica (Ludox HS-40, solid content concentration 40% by mass, manufactured by Aldrich) were mixed and stirred for 24 hours to prepare a mixed gel. The composition of the mixed gel is α=(L12O+L2O) / SiO2=0.00, β=OH - / (M12O+M2O)=1.00, γ=SiO2 / Al2O3=10.00, δ=H2O / Al2O3=220.0, ε=P2O5 / Al2O3=0.00, ζ=R / Al2O3=0.00. The mixed gel was put into a 300mL stainless steel micro-storage bottle (manufactured by HIRO COMPANY) with a fluororesin inner cylinder, and hydrothermal synthesis was carried out for 3 days at a stirring speed of 60rpm and 150°C using a stirring thermostatic bath (manufactured by HIRO COMPANY) that can rotate along the up and down directions of the micro-storage bottle. The product was filtered out and dried at 120°C to obtain a powdered zeolite. The obtained zeolite was confirmed to be a GIS type zeolite by XRD spectrum. In addition, no peaks derived from other zeolites, amorphous silica-alumina, etc. were observed, so it was evaluated as a high-purity GIS type zeolite.

[0277] The values ​​were measured using the same method as in Example 1. 29 Si-MAS-NMR spectrum, SAR = 6.00, and (a + d) / (b + c) = 0.176. The potassium and lithium contents in the zeolite are Z / T = 0.00 (= K / T). The above-mentioned X-ray diffraction measurement was performed, and the result was P CO2 =34.04, P de =28.05, P de / P CO2 =0.824. In addition, when the adsorption isotherm of CH4 was measured in the same way, the adsorption amount at 760 mmHg was 7.3 cm 3 / g.

[0278] In addition, after molding in the same manner as in Example 1, the pulverization rate of the obtained GIS-type zeolite molded body was measured to be 52%, and when the desorption isotherm of CO2 was measured, q(Ad) / q(De)=0.365.

[0279] [Comparative Example 2]

[0280] Based on the content of Patent Document 1, 207.30 g of water, 8.78 g of sodium hydroxide, 16.4 g of sodium aluminate and 248.3 g of No. 3 water glass were mixed and stirred for 15 minutes to prepare a mixed gel. The composition of the mixed gel was α = (L12O + L2O) / SiO2 = 0.32, β = OH - / (M12O+M2O)=0.35, γ=SiO2 / Al2O3=12.40, δ=H2O / Al2O3=197.9, ε=P2O5 / Al2O3=0.00, ζ=R / Al2O3=0.00. The mixed gel was put into a 1000 mL stainless steel autoclave with a fluororesin inner cylinder, and hydrothermally synthesized at 130°C for 5 days without stirring. The product was filtered out and dried at 120°C to obtain a powdered zeolite. In addition, no peaks derived from other zeolites, amorphous silica-alumina, etc. were observed, so it was evaluated as a high-purity GIS type zeolite.

[0281] The values ​​were measured using the same method as in Example 1. 29 Si-MAS-NMR spectrum, SAR = 4.10, and (a + d) / (b + c) = 0.151. The potassium and lithium contents in the zeolite are Z / T = 0.00 (= K / T). The above-mentioned X-ray diffraction measurement was performed, and the result was P CO2 =28.05, P de =29.55, P CO2 / P de =0.949.

[0282] In addition, after molding in the same manner as in Example 1, the powderization rate of the obtained GIS type zeolite molded body was measured, and the powderization rate was 39%. When the CO2 desorption isotherm was measured, the adsorption amount at 760 mmHg was 37.8 cm 3 / g, q(Ad) / q(De)=0.365. In addition, when the adsorption isotherm of CH4 was measured in the same manner, the adsorption amount at 760 mmHg was 8.0 cm 3 / g.

[0283] Industrial Applicability

[0284] The GIS-type zeolite of the present invention has industrial applicability as a carbon dioxide adsorbent.

[0285] Explanation of symbols

[0286] 1. Adsorption device

[0287] 2 Containers

[0288] 3 Filters

[0289] 4 Zeolite shaped body

Claims

1. A GIS type zeolite, wherein: In the spectrum obtained by X-ray diffraction under the condition of dehydration and carbon dioxide adsorption, among the diffraction peaks observed between the diffraction angles 2θ=25.81° and 34.57°, the diffraction peak P with the strongest intensity CO2 The diffraction angle (2θ) is 28.60°~29.54°.

2. A GIS type zeolite, wherein: In the spectrum obtained by X-ray diffraction under dehydrated state and nitrogen adsorption conditions, the diffraction peak with the strongest intensity observed between the diffraction angle 2θ = 25.81° and 34.57° is defined as P de When P CO2 / P de ≧0.

969.

3. The GIS type zeolite according to claim 1, wherein In the spectrum obtained by X-ray diffraction under dehydrated state and nitrogen adsorption conditions, the diffraction peak with the strongest intensity observed between the diffraction angle 2θ = 25.81° and 34.57° is defined as P de When P CO2 / P de ≧0.

969.

4. The GIS type zeolite according to any one of claims 1 to 3, wherein The silica-alumina ratio of the GIS type zeolite is 3.40 or more. 5 . The GIS type zeolite according to claim 1 , comprising potassium or lithium as a cationic species in the GIS type zeolite.

6. The GIS type zeolite according to claim 5, wherein The ratio (Z / T) of the total amount of substance (Z) of potassium and lithium to the total amount of substance (T) of alkali metals in the GIS-type zeolite is 0.05 or more.

7. The GIS type zeolite according to any one of claims 1 to 3, wherein Will be in 29 The peak area intensities attributed to Q4(3Al), Q4(2Al), Q4(1Al) and Q4(0Al) observed in the Si-MAS-NMR spectrum are set to a, b, c and d, respectively, satisfying (a+d) / (b+c)≧0.

192.

8. The GIS type zeolite according to any one of claims 1 to 3, having a diameter of 10 cm 3 / g or more carbon dioxide adsorption capacity. 9 . A zeolite molded body comprising the GIS-type zeolite according to claim 1 .

10. The zeolite shaped body according to claim 9, comprising a carrier.

11. The zeolite molded body according to claim 10, wherein The carrier includes an inorganic binder and an organic binder.

12. The zeolite shaped body according to any one of claims 10, wherein The total content of the carriers is 1% by mass to 99% by mass based on 100% by mass of the total amount of the zeolite molded body.

13. The zeolite molded body according to claim 9, which has a cylindrical shape.

14. The zeolite shaped body according to claim 13, wherein The length is greater than or equal to 3 mm and less than or equal to 30 mm, and the diameter is greater than or equal to 1 mm and less than or equal to 30 mm.

15. An adsorption device comprising the zeolite molded body according to claim 9.

16. A method for producing a purified gas, comprising: The separation step uses the adsorption device described in claim 15 to separate one or more gases selected from the group consisting of CO2, H2O, He, Ne, Cl2, NH3 and HCl from a mixture containing two or more gases selected from the group consisting of H2, N2, O2, Ar, CO and hydrocarbons.

17. The manufacturing method according to claim 16, wherein: In the separation step, the gas is separated by a pressure swing adsorption separation method, a temperature swing adsorption separation method, or a pressure swing-temperature swing adsorption separation method.

Citation Information

Patent Citations

  • SCM-8 molecular sieve and preparation method therefor

    CN105460953A

  • Use of molecular sieves for decarbonating natural gas

    CN108348834A

  • GIS zeolite

    CN108495813A

  • GIS-type zeolite

    CN111051242A

  • Relaxation oscillator with an aging effect reduction technique

    CN111684720A