Paste

By using a specific paste formulation and controlling the heating process, the problem of paste overflowing and solidifying at high temperatures has been solved. This achieves the effect of thickening at low initial viscosity without solidifying, making it suitable for high-temperature environments.

CN118922474APending Publication Date: 2024-11-08NIPPON VALQUA IND LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027962.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-23
Publication Date
2024-11-08

Smart Images

  • Figure BDA0005044410520000061
    Figure BDA0005044410520000061
  • Figure BDA0005044410520000111
    Figure BDA0005044410520000111
  • Figure BDA0005044410520000221
    Figure BDA0005044410520000221
Patent Text Reader

Abstract

A paste containing a polysiloxane (A) having a mercapto group, a compound (B) containing two or more groups having an ethylenically unsaturated bond in one molecule, and a radical initiator (C).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a paste. Background Art

[0002] For components such as sliding components, brake components, and vibration suppression and absorption components, paste (also called paste) is used between the components to ensure the prescribed movement, wear resistance, seizure resistance, etc. of these components. In addition, between the heating element and the heat dissipation part of the electronic component, a heat dissipation (thermal conductivity) material is used in order to efficiently transfer the heat generated by the heating element to the heat dissipation part. As the heat dissipation material, there are mainly two forms: sheet type and paste type. However, the sheet type has increased contact thermal resistance due to the poor adhesion between the sheet and the target surface of the heating element or the heat dissipation part, and the sheet itself needs a certain degree of thickness. Therefore, from the perspective of being able to form a thin film during coating, good adhesion between the target surface, and excellent heat dissipation performance, paste type is used as the heat dissipation material.

[0003] If the viscosity of the above-mentioned paste is low during coating, the operability and productivity such as coating performance are improved, and it is easy to arrange a specified amount, especially a small amount of paste, at a specified location. Therefore, for example, in the case of the above-mentioned heat dissipation material, the thickness of the paste layer can be thinned, which can improve the heat dissipation performance, so a low viscosity is required during coating.

[0004] On the other hand, the paste is required to be stored in a predetermined location in order to achieve the desired purpose of the paste. As such a paste, for example, a silicone-based paste containing a silicone-based compound as a base oil is known (Patent Documents 1 and 2). Prior art literature Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2013-227374 Patent Document 2: Japanese Patent Application Publication No. 2017-165791 Summary of the invention

[0006] However, conventional pastes have a lower viscosity when the temperature rises, and are prone to flow out from a predetermined location (hereinafter also referred to as "overflow"). Due to the overflow or the degradation or solidification of the paste itself at high temperature, the paste cannot achieve its intended purpose.

[0007] In addition, the paste formed at a predetermined location may be heated and thickened once before use in order to suppress outflow from the location. However, a paste having a low viscosity during coating tends to overflow even after being heated and thickened in this way, and there is a problem that it is difficult to maintain predetermined performance for a long period of time.

[0008] One embodiment of the present invention provides a paste that does not solidify even after heat-thickening, and that can suppress overflow even when heat-thickening is performed at a relatively low heating temperature despite having a low initial viscosity. The initial viscosity here refers to the viscosity when the paste is prepared, and is the viscosity before the paste is heated and thickened, and is usually the viscosity during coating. Solutions to technical problems

[0009] The configuration examples of the present invention are as follows.

[0010] [1] A paste comprising a polysiloxane having a mercapto group (A), a compound having two or more groups having an ethylenically unsaturated bond in one molecule (B), and a radical initiator (C).

[0011] [2] The paste according to [1], wherein the ratio of the functional groups represented by the following formula (1) is 3 or less: Functional group ratio = (the blending amount of the polysiloxane (A) / the functional group equivalent of the polysiloxane (A)) / (the blending amount of the compound (B) / the functional group equivalent of the compound (B)) ... (1)

[0012] [3] The paste according to [1] or [2], wherein the paste satisfies the following condition (I): Condition (I): Heat curing is performed for 10 minutes at a temperature of 1 minute half-life of the free radical initiator (C), 0.2 g of the heat-cured paste is drawn into a 5 mm square, and then compressed at 23°C at a pressure of 1.0 MPa to a thickness of less than 200 μm.

[0013] [4] The paste according to any one of [1] to [3], wherein the initial shear viscosity at 23°C is 500 Pa·s or less.

[0014] [5] A paste as described in any one of [1] to [4], wherein the ratio of the shear viscosity after heating the paste at a temperature of the one-minute half-life of the free radical initiator (C) for 10 minutes and then cooling to 23°C to the initial shear viscosity of the paste at 23°C is 3 times or more.

[0015] [6] The paste according to any one of [1] to [5], comprising a thermally conductive filler (D). [7] The paste according to [6], wherein the content of the thermally conductive filler (D) is 30 to 80% by volume relative to 100% by volume of the paste. Effects of the Invention

[0016] According to one embodiment of the present invention, a paste can be provided that does not solidify even after heating and thickening (does not solidify but remains in a paste state), and the paste can suppress overflow even when heating and thickening at a relatively low heating temperature (e.g., the 1-minute half-life temperature of a free radical initiator) despite having a low initial viscosity. In addition, according to one embodiment of the present invention, a paste having heat resistance (eg, heat resistance of 150° C. or higher) can be provided. For example, a paste having almost no (extremely long) pot life under storage conditions at room temperature can be provided. Since the paste according to one embodiment of the present invention does not solidify even at high temperatures but remains in a paste state, the performance required of a member using the paste can be maintained for a long period of time even at high temperatures.

[0017] The paste according to one embodiment of the present invention is defined as having a thickness of 200 μm or less after 0.2 g of the paste is pulled into a 5 mm square and then compressed at a pressure of 1.0 MPa at 23° C. Since the paste of one embodiment of the present invention is a paste that does not solidify even after being heated and thickened, it is preferably a paste that is heat-cured for 10 minutes at a temperature of 1 minute half-life of the above-mentioned free radical initiator (C), 0.2 g of the heat-cured paste is stretched into a 5 mm square, and then compressed at a pressure of 1.0 MPa at 23°C to a thickness of less than 200 μm. Specifically, the method for measuring the thickness is as described in the following examples. DETAILED DESCRIPTION

[0018] Paste A paste according to one embodiment of the present invention (hereinafter also referred to as "the present paste") comprises a polysiloxane (A) having a mercapto group [hereinafter also referred to as "component (A)", and the same applies to other components], a compound (B) having two or more groups having ethylenically unsaturated bonds in one molecule, and a free radical initiator (C).

[0019] <Polysiloxane (A)> The component (A) is not particularly limited as long as it is a polysiloxane having a mercapto group (—SH). By using such a component (A), a paste having excellent heat resistance and not solidifying even after thickening by heating can be easily obtained, and a paste having low initial viscosity but suppressing overflow even after thickening by heating at a relatively low heating temperature can be easily obtained. The component (A) used in the present paste may be one kind or two or more kinds.

[0020] The bonding position of the mercapto group is not particularly limited and may be a so-called side chain type, a terminal type (including a single terminal type and a dual terminal type), or a side chain dual terminal type. The side chain type or the dual terminal type is preferred, and the side chain type is more preferred.

[0021] As the component (A), an organopolysiloxane in which an organic group is bonded to a silicon atom, and a polysiloxane having a mercapto group in at least a part of the organopolysiloxane is preferred.

[0022] Examples of the organic group bonded to the silicon atom include a linear alkyl group, a branched alkyl group, a cyclic alkyl group, an aryl group, an aralkyl group, a halogenated alkyl group and an alkoxy group. Examples of the linear alkyl group include a group having 1 to 20 carbon atoms, preferably 1 to 6 carbon atoms, such as methyl group, ethyl group, propyl group, hexyl group, octyl group and decyl group. Examples of the branched alkyl group include a group having 1 to 20 carbon atoms, preferably 1 to 6 carbon atoms, such as isopropyl, isobutyl, tert-butyl, and 2-ethylhexyl. Examples of the cyclic alkyl group include groups having 3 to 20 carbon atoms, such as cyclopentyl and cyclohexyl. Examples of the aryl group include groups having 6 to 20 carbon atoms, such as a phenyl group and a tolyl group. Examples of the aralkyl group include groups having 7 to 20 carbon atoms, such as benzyl, 2-phenethyl, and 2-methyl-2-phenethyl. Examples of the haloalkyl group include groups having 1 to 20 carbon atoms, preferably 1 to 6 carbon atoms, such as 3,3,3-trifluoropropyl, 2-(nonadecafluorobutyl)ethyl, and 2-(heptadecafluorooctyl)ethyl. Examples of the alkoxy group include groups having 1 to 20 carbon atoms, preferably 1 to 6 carbon atoms, such as a methoxy group and an ethoxy group.

[0023] As the organic group bonded to the silicon atom, a linear alkyl group or an aryl group is preferred, a linear alkyl group or an aryl group having 1 to 6 carbon atoms is more preferred, and a methyl group or a phenyl group is particularly preferred. That is, as a structure other than the part having a mercapto group in the above-mentioned organopolysiloxane, it is preferable to have at least one polysiloxane structure selected from dimethylpolysiloxane, methylphenylpolysiloxane and diphenylpolysiloxane, and a dimethylpolysiloxane structure is more preferable.

[0024] The mercapto group may be directly bonded to the silicon atom or may be bonded to the silicon atom via an organic group bonded to the silicon atom.

[0025] The molecular structure of component (A) is not particularly limited, and examples thereof include linear, branched, linear with a portion of branches, and dendrimer, preferably linear or linear with a portion of branches. Component (A) may be a homopolymer having these molecular structures, a copolymer having these molecular structures, or a mixture of two or more of these polymers.

[0026] Specific examples of the component (A) include polysiloxanes represented by the following formula (2).

[0027]

Chemistry 1

[0028] As R 1 and R 2 The unsubstituted or substituted monovalent hydrocarbon group in the above is preferably an unsubstituted or substituted monovalent hydrocarbon group having 1 to 20 carbon atoms, and examples thereof include the same groups as those exemplified as the organic group bonded to the silicon atom (except the alkoxy group). Among them, a monovalent hydrocarbon group having 1 to 6 carbon atoms is preferred, and an alkyl group or an aryl group having 1 to 6 carbon atoms is more preferred.

[0029] As R 1 Examples of the alkoxy group in R2 include the same groups as exemplified above as the organic group bonded to the silicon atom.

[0030] R 1 and R 2 The alkanethio group having 1 to 6 carbon atoms is a group represented by -R-SH (R is an alkylene group having 1 to 6 carbon atoms), and as such R, there can be mentioned a group obtained by removing one hydrogen atom from the group exemplified as the organic group bonded to the silicon atom (a group other than a haloalkyl group and an alkoxy group).

[0031] As the component (A), a component synthesized by a conventionally known method may be used, or a commercially available product may be used.

[0032] The shear viscosity of component (A) at 23°C measured with a cone and plate viscometer is preferably at least 0.005 Pa·s, more preferably at least 0.01 Pa·s, and is preferably at most 60.00 Pa·s, more preferably at most 5.00 Pa·s. If the viscosity of component (A) is within the above range, a paste having a low initial viscosity and excellent coating properties can be easily obtained. In addition, when the paste having a low initial viscosity is a heat dissipation paste, a thin paste layer can be easily formed at a predetermined location such as between a heating element and a heat dissipation portion, and a paste layer can be easily formed to fit the target surface of a heating element or a heat dissipation portion, thereby reducing the thermal resistance generated by the paste layer, and easily obtaining electronic components having excellent heat dissipation properties.

[0033] From the perspective of being able to easily obtain a paste having a viscosity that can suppress overflow after heating and thickening, but which does not solidify and maintains a paste state after heating and thickening, the functional group (thiol) equivalent of component (A) is preferably 1000 g / mol or more, more preferably 1500 g / mol or more, preferably 50000 g / mol or less, and more preferably 35000 g / mol or less.

[0034] In addition, as component (A), from the perspective of being able to easily obtain a paste having a viscosity that can suppress overflow after heating and thickening but does not solidify and maintains a paste state after heating and thickening, it is preferable to use a polysiloxane (A1) having a functional group equivalent of preferably 1000 to 5000 g / mol, more preferably 1500 to 5000 g / mol, and a polysiloxane (A2) having a functional group equivalent of preferably 15000 g / mol or more, more preferably 20000 g / mol or more and preferably 50000 g / mol or less, more preferably 3500 g / mol or less. When such polysiloxanes (A1) and (A2) are used, the proportion of polysiloxane (A2) relative to their total 100 mass % is preferably 50.0 mass % or more, more preferably 75.0 mass % or more, and is preferably 99.5 mass % or less, more preferably 99.0 mass % or less.

[0035] From the perspective of being able to easily obtain a paste having a viscosity that can suppress overflow after heating and thickening but does not solidify and maintains a paste state after heating and thickening, the number average molecular weight (Mn) of component (A) measured by gel permeation chromatography (GPC) is preferably 3,000 or more, more preferably 15,000 or more, preferably 50,000 or less, and more preferably 25,000 or less.

[0036] From the perspective of being able to easily obtain a paste having a viscosity that can suppress overflow after heating and thickening, but which does not solidify and maintains a paste state after heating and thickening, the content of component (A) in the present paste is preferably 40.0 mass% or more, more preferably 70.0 mass% or more, further preferably 85.0 mass% or more, and preferably 99.0 mass% or less, and more preferably 98.5 mass% or less, relative to 100 mass% of the total of components (A) and (B) in the present paste.

[0037] From the perspective of being able to easily obtain an excellent paste having a good balance between heat resistance, low initial viscosity and overflow inhibition, when the present paste does not contain the following component (D), the content of component (A) in the present paste is preferably 40.0 mass% or more, more preferably 60.0 mass% or more, preferably 95.0 mass% or less, and more preferably 90.0 mass% or less, relative to 100 mass% of the present paste. For the same reason, when the present paste contains the following component (D), the content of component (A) in the present paste is preferably 5.0 mass % or more, more preferably 10.0 mass % or more, and preferably 30.0 mass % or less, more preferably 20.0 mass % or less, relative to 100 mass % of the present paste.

[0038] <Compound (B)> The component (B) is not particularly limited as long as it is a compound other than the above-mentioned component (A) and contains two or more groups having an ethylenically unsaturated bond in one molecule, and a conventionally known compound (co-crosslinking agent) can be used. By using the component (B), a paste having excellent overflow suppression property after heat thickening can be easily obtained. The component (B) used in the present paste may be one kind or two or more kinds.

[0039] The number of groups having an ethylenically unsaturated bond in the component (B) may be 2, but is preferably 3 or more, more preferably 3 to 6, from the viewpoint of being able to further suppress bleeding. The two or more groups having an ethylenically unsaturated bond contained in the component (B) may be the same or different. That is, the component (B) may contain two or more types of groups having an ethylenically unsaturated bond.

[0040] Examples of the group having an ethylenically unsaturated bond include alkenyl groups having 2 to 8 carbon atoms, such as vinyl, methylvinyl, allyl, propenyl, isopropenyl, butenyl, pentenyl, hexenyl, and heptenyl; vinylphenyl, (meth)acryloyl, allyloxy, styryl, propargyl, and maleimide. Among them, alkenyl groups having 2 to 8 carbon atoms and (meth)acryloyl are preferred, alkenyl groups having 2 to 4 carbon atoms and (meth)acryloyl are more preferred, and vinyl, allyl, and (meth)acryloyl are particularly preferred.

[0041] As component (B), for example, there can be mentioned: polysiloxane containing two or more groups having ethylenically unsaturated bonds in one molecule; Ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butylene glycol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, alkoxylated bisphenol A di(meth)acrylate, alkoxylated bisphenol F di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, glycerol tri(meth)acrylate ) acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, tripentaerythritol octa(meth)acrylate, ethylene oxide added trimethylolpropane tri(meth)acrylate, ethylene oxide added ditrimethylolpropane tetra(meth)acrylate, ethylene oxide added pentaerythritol tetra(meth)acrylate, ethylene oxide added diquaternary Pentaerythritol hexa(meth)acrylate, propylene oxide added trimethylolpropane tri(meth)acrylate, propylene oxide added ditrimethylolpropane tetra(meth)acrylate, propylene oxide added pentaerythritol tetra(meth)acrylate, propylene oxide added dipentaerythritol hexa(meth)acrylate, ε-caprolactone added trimethylolpropane tri(meth)acrylate, ε-caprolactone added ditrimethylolpropane tetra(meth)acrylate, ε-caprolactone added pentaerythritol tetra(meth)acrylate, Polyfunctional (meth)acrylate compounds such as ε-caprolactone-added dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate succinic acid-modified products, pentaerythritol tri(meth)acrylate succinic acid-modified products, dipentaerythritol penta(meth)acrylate phthalic acid-modified products, pentaerythritol tri(meth)acrylate phthalic acid-modified products, tris((meth)acryloyloxyethyl)isocyanurate, and alkylene oxide-added tris((meth)acryloyloxyethyl)isocyanurate; Ethylene glycol divinyl ether, diethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butanediol divinyl ether, hexanediol divinyl ether, alkoxylated bisphenol A divinyl ether, alkoxylated bisphenol F divinyl ether, trimethylolpropane trivinyl ether, ditrimethylolpropane tetravinyl ether, glycerol trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, dipentaerythritol hexavinyl ether, ethylene oxide added trimethylolpropane trivinyl ether, ethylene oxide added ditrimethylolpropane tetravinyl ether, ethylene oxide added pentaerythritol tetravinyl ether, ethylene oxide added dipentaerythritol hexavinyl ether and other multifunctional vinyl ethers; (meth)acrylates containing a vinyl ether group, such as 2-vinyloxyethyl (meth)acrylate, 3-vinyloxypropyl (meth)acrylate, 1-methyl-2-vinyloxyethyl (meth)acrylate, 2-vinyloxypropyl (meth)acrylate, 4-vinyloxybutyl (meth)acrylate, 4-vinyloxycyclohexyl (meth)acrylate, 5-vinyloxypentyl (meth)acrylate, 6-vinyloxyhexyl (meth)acrylate, 4-vinyloxymethylcyclohexyl (meth)acrylate, p-vinyloxymethylphenylmethyl (meth)acrylate, 2-(vinyloxyethoxy)ethyl (meth)acrylate, and 2-(vinyloxyethoxyethoxyethoxy)ethyl (meth)acrylate; Ethylene glycol diallyl ether, diethylene glycol diallyl ether, polyethylene glycol diallyl ether, propylene glycol diallyl ether, butanediol diallyl ether, hexanediol diallyl ether, alkoxylated bisphenol A diallyl ether, alkoxylated bisphenol F diallyl ether, trimethylolpropane triallyl ether, ditrimethylolpropane tetraallyl ether, diallyl phthalate, glycerol triallyl ether, pentaerythritol tetraallyl ether, dipentaerythritol pentaallyl ether Polyfunctional allyl compounds such as propylene glycol, propylene glycol, propylene glycol, propylene glycol ether, dipentaerythritol hexaallyl ether, ethylene oxide addition trimethylolpropane triallyl ether, ethylene oxide addition ditrimethylolpropane tetraallyl ether, ethylene oxide addition pentaerythritol tetraallyl ether, ethylene oxide addition dipentaerythritol hexaallyl ether, triallyl isocyanurate, triallyl cyanurate, triallyl formaldehyde, triallyl trimellitate, tetraallyl terephthalamide, etc.; Allyl (meth)acrylates such as allyl (meth)acrylate; Multifunctional (meth)acrylamide compounds such as N,N-ethylenebis(meth)acrylamide; Poly(dipropylene terephthalate) and other multifunctional propargyl compounds; Multifunctional maleimide compounds such as N,N′-m-phenylenebismaleimide; Polyfunctional urethane (meth)acrylates obtained by reacting a polyfunctional isocyanate such as toluene diisocyanate, isophorone diisocyanate, or xylene diisocyanate with a hydroxyl-containing (meth)acrylate such as 2-hydroxyethyl (meth)acrylate or 2-hydroxypropyl (meth)acrylate; Polyfunctional aromatic vinyls such as divinylbenzene.

[0042] Among them, from the perspective of being able to easily obtain a paste with excellent reactivity and excellent heat resistance, polyfunctional (meth)acrylate compounds, polyfunctional allyl compounds, and polyfunctional (meth)acrylamide compounds are preferred, trifunctional or higher-functional (meth)acrylate compounds and trifunctional or higher-functional allyl compounds are more preferred, and triaryl isocyanurate and trimethylolpropane tri(meth)acrylate are particularly preferred.

[0043] Examples of the polysiloxane containing two or more ethylenically unsaturated groups in one molecule include dimethyl polysiloxane terminated with dimethylvinylsiloxane at both ends of the molecular chain, dimethyl polysiloxane terminated with methylphenylvinylsiloxane at both ends of the molecular chain, dimethyl polysiloxane-methylphenylsiloxane copolymer terminated with dimethylvinylsiloxane at both ends of the molecular chain, dimethyl polysiloxane-methylphenylsiloxane copolymer terminated with dimethylvinylsiloxane at both ends of the molecular chain, dimethyl polysiloxane-methylvinylsiloxane copolymer terminated with dimethylvinylsiloxane at both ends of the molecular chain, dimethyl polysiloxane-methylvinylsiloxane copolymer terminated with silanol groups at both ends of the molecular chain, dimethyl polysiloxane-methylvinylsiloxane-methylphenylsiloxane copolymer terminated with silanol groups at both ends of the molecular chain, dimethyl polysiloxane-methylvinylsiloxane copolymer terminated with trimethylsilylalkyl groups at both ends of the molecular chain, methyl (3,3,3-trifluoropropyl) polysiloxane terminated with dimethylvinylsiloxy groups at both ends of the molecular chain, and polysiloxane having the formula: (CH 3 ) 3 SiO 1 / 2 The siloxane unit represented by the formula: (CH 3 ) 2 (CH 2 =CH)SiO 1 / 2 The siloxane unit represented by the formula: CH 3 SiO 3 / 2 The siloxane unit represented by the formula: (CH 3 ) 2 SiO 2 / 2 An organosiloxane composed of the siloxane units represented.

[0044] Specific examples of the polysiloxane containing two or more ethylenically unsaturated bond groups in one molecule include compounds represented by the following formula (3).

[0045]

Chemistry 2

[0046] R 3 Each is independently an unsubstituted or substituted monovalent hydrocarbon group preferably having 1 to 10 carbon atoms, and examples thereof include the same groups as exemplified as the organic group bonded to the silicon atom and alkenyl groups. Among them, monovalent hydrocarbon groups having 1 to 6 carbon atoms are preferred, and alkenyl groups, aryl groups, and alkyl groups having 1 to 3 carbon atoms are more preferred.

[0047] As R 4 The alkyl group in may be, for example, the same linear alkyl group, branched alkyl group, and cyclic alkyl group as exemplified above as the organic group bonded to the silicon atom. As R 4 The alkoxyalkyl group in the above-mentioned group may be a group having 2 to 10 carbon atoms, such as a methoxyethyl group and a methoxypropyl group. As R 3 and R 4 The alkenyl group in " may be the same alkenyl group as exemplified as the group having an ethylenically unsaturated bond. As R 4 The acyl group in the acyl group may, for example, be a group having 2 to 10 carbon atoms such as acetyl and octanoyl. The sum of c and d is preferably an integer of 10 to 50, and e is preferably 1.

[0048] From the perspective of being able to easily obtain a paste having a viscosity that can suppress overflow after heating and thickening but maintaining a paste state without solidifying after heating and thickening, the functional group (ethylenically unsaturated bond) equivalent of component (B) is preferably 4 g / mol or more, more preferably 50 g / mol or more, further preferably 75 g / mol or more, preferably 25000 g / mol or less, and more preferably 130 g / mol or less.

[0049] From the perspective of being able to easily obtain a paste having a viscosity that can suppress overflow after heating and thickening but which does not solidify and maintains a paste state after heating and thickening, the ratio of the functional groups represented by the following formula (1) of the component (B) used is preferably 3 or less, more preferably 2 or less, further preferably 1 or less, particularly preferably 0.45 or less, and more preferably 0.01 or more, further preferably 0.015 or more, and particularly preferably 0.02 or more. Functional group ratio = (amount of component (A) blended / functional group equivalent of component (A)) / (amount of component (B) blended / functional group equivalent of component (B)) ... (1)

[0050] In addition, for example, when a component (A) having a functional group equivalent of a g / mol is used in a blending amount of x1 mass % and a component (A) having a functional group equivalent of b g / mol is used in a blending amount of x2 mass %, the numerator of the above formula (1) is "(x1 / a+x2 / b)". The same applies to the case where two or more components (A) or (B) are used.

[0051] The content of component (B) is an amount satisfying the above formula (1) relative to 100% by mass of the present paste, but the content of component (B) in the present paste is preferably as small as possible. Therefore, from this point of view and the perspective of being able to easily obtain a paste having a viscosity that can suppress overflow after heating and thickening, but which does not solidify and maintains a paste state after heating and thickening, the content of component (B) is preferably not less than 0.2% by mass, more preferably not less than 0.3% by mass, further preferably not less than 0.5% by mass, preferably not more than 50% by mass, more preferably not more than 15% by mass, and further preferably not more than 5.5% by mass.

[0052] <Free Radical Initiator (C)> The component (C) is not particularly limited as long as it is a radical initiator, and a conventionally known radical initiator can be used. By using component (C) to react (crosslink) components (A) and (B), a paste with suppressed overflow can be obtained without using a platinum-based catalyst used in conventional pastes, and a paste with almost no (extremely long) pot life can be obtained if stored under a room temperature environment. The component (C) used in the present paste may be one kind or two or more kinds.

[0053] Examples of the component (C) include 2,5-dimethyl-2,5-di(tert-butylperoxide)hexane, diisopropyl benzene peroxide, 2,4-dichlorobenzoyl peroxide, di-tert-butyl peroxide, diisopropyl tert-butyl peroxide, benzoyl peroxide, 2,5-dimethyl-2,5-(tert-butylperoxide)-3-hexyne, 2,5-dimethyl-2,5-bis(benzoylperoxide)hexane, α,α'-bis(tert-butylperoxide-m-isopropyl)benzene, tert-butylperoxyisopropyl carbonate, bis-(4-tert-butylcyclohexyl)peroxydicarbonate, p-chlorobenzoyl peroxide, peroxy Peroxides such as tert-butyl-2-ethylhexanoate and tert-butyl perbenzoate, and azo compounds such as 2,2'-azobis(2-methylpropionitrile), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobisisovaleronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 4,4'-azobis(4-cyanovaleric acid), 1,1'-azobis(cyclohexanecarbonitrile), 2,2'-azobis(2-methylpropane), 2,2'-azobisisobutyric acid methyl ester, and 2,2'-azobis(2-methylpropionamidine) dihydrochloride.

[0054] From the perspective of being able to easily obtain a paste having a viscosity that can suppress overflow after heating and thickening, but which does not solidify and maintains a paste state after heating and thickening, the content of component (C) in the present paste is preferably 0.05 parts by mass or more, more preferably 0.5 parts by mass or more, particularly preferably 1 part by mass or more, and preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less, relative to 100 parts by mass of the total of components (A) and (B) in the present paste.

[0055] The content of component (C) is preferably as small as possible relative to 100% by mass of the present paste. Therefore, from this point of view and the perspective of being able to easily obtain a paste having a viscosity that can suppress overflow after heating and thickening but does not solidify and maintains a paste state after heating and thickening, the content of component (C) in 100% by mass of the present paste is preferably 0.4% by mass or more, more preferably 0.5% by mass or more, further preferably 1% by mass or more, preferably 15% by mass or less, more preferably 9% by mass or less, and further preferably 7.5% or less.

[0056] <Thermal conductive filler (D)> When the present paste is used as a heat dissipation paste, the present paste preferably contains the component (D). When component (D) is used in the present paste, the component (D) used may be one or more. When two or more components (D) are used, two or more components (D) having different materials or different shapes or average particle sizes may be used.

[0057] As the component (D), it is preferred to use a filler having a thermal conductivity of 1 W / m·K or more. Examples of such component (D) include metal powders, metal oxide powders, metal nitride powders, metal hydroxide powders, metal oxynitride powders, metal carbide powders, and carbon materials, and specifically aluminum oxide (Al 2 O 3 ), silicon oxide (SiO 2 ), magnesium oxide (MgO), beryllium oxide (BeO), zinc oxide (ZnO), silicon nitride (Si 3 N 4 ), boron nitride (e.g. hexagonal BN or cubic BN), aluminum nitride (AlN), silicon carbide (SiC), graphite, diamond, carbon nanotubes.

[0058] The shape of the component (E) is not particularly limited, and may be a granular shape, a flaky shape, or a needle shape. However, a granular shape is preferred because it can be packed at a higher density. The average particle size of the particulate component (D) is, for example, 0.1 μm or more, preferably 0.5 μm or more, and for example, 100 μm or less, preferably 50 μm or less. The average particle size is the d50 value in the particle size distribution obtained by a laser diffraction / scattering method (MICROTRAC method).

[0059] When the present paste contains component (D), the content of component (D) is preferably 30% by volume or more, more preferably 50% by volume or more, and preferably 80% by volume or less, more preferably 70% by volume or less, relative to 100% by volume of the present paste.

[0060] In addition, the greater the amount of component (D) blended, for example, when the paste is used as a heat dissipation material, there is a tendency for the thermal properties to be excellent (for example, the thermal diffusion value increases and the thermal resistance value decreases), so depending on the application, it is sometimes desirable to blend more component (D). However, in conventional pastes, if the blending amount of component (D) is increased, the initial viscosity becomes higher and the workability decreases (it is difficult to form the paste at a predetermined location by coating or pouring, etc.), so conventional pastes cannot be blended with a large amount of component (D). On the other hand, since the initial viscosity of the present paste is low, by using the present paste, even if the blending amount of the component (D) is increased, the workability is unlikely to decrease. Therefore, according to one embodiment of the present invention, for the purpose of obtaining a paste having particularly excellent thermal properties, even if component (D) is added in an amount of preferably 40% by volume or more, more preferably 50% by volume or more and preferably 80% by volume or less, more preferably 70% by volume or less relative to 100% by volume of the present paste, a paste having a low initial viscosity and excellent workability can be obtained.

[0061] <Other ingredients> The paste may also contain the following other components besides the above-mentioned components (A) to (D) as required, unless the effects of the present invention are impaired: plasticizers such as fluorine-based oils or silicone-based oils; silane coupling agents; surfactants; crosslinking accelerators; solvents; dispersants; anti-aging agents; antioxidants; flame retardants; pigments, etc. These other components may be used alone or in combination of two or more.

[0062] The present paste preferably does not contain a platinum-based catalyst from the viewpoint that a paste having almost no (extremely long) pot life can be obtained under a storage environment at room temperature. Conventional pastes use platinum catalysts, but once platinum catalysts are used, the shelf life is shortened and the paste cannot be stored for a long time. The phrase “containing no platinum-based catalyst” means that the content of the platinum-based catalyst is, for example, 0.0001 parts by mass or less relative to 100 parts by mass of the total of components (A) and (B), and the lower limit is preferably 0 parts by mass.

[0063] <Method for preparing the paste> The present paste can be prepared by mixing the above-mentioned components (A) to (C) and the above-mentioned component (D) or the above-mentioned other components as required, and kneading and dispersing them with a stirrer, a roll or the like.

[0064] <Physical properties of this paste> The initial shear viscosity of the paste at 23°C measured by a cone and plate viscometer (this viscosity is the initial viscosity) is preferably as low as possible, specifically, preferably 500 Pa·s or less, more preferably 300 Pa·s or less, particularly preferably 250 Pa·s or less, and preferably 1 Pa·s or more. If the initial viscosity of the present paste is within the above range, a paste with excellent workability (easy to form the paste at a predetermined location by coating or pouring, etc.) can be easily obtained. In addition, when the paste with a low initial viscosity is a heat dissipation paste, a thin paste layer can be easily formed at a predetermined location such as between a heating element and a heat dissipation portion, and can be easily adhered to the target surface of the heating element or the heat dissipation portion, thereby reducing the thermal resistance generated by the paste layer, and easily obtaining electronic components with excellent heat dissipation characteristics. Generally, a paste having a low initial viscosity tends to overflow even after being heated and thickened. However, by using the paste of the present invention, overflow can be suppressed even after being heated and thickened despite having a low initial viscosity.

[0065] The ratio of the shear viscosity after heating (hereinafter also referred to as "viscosity after heating") measured by a cone and plate viscometer after heating the paste at a 1-minute half-life temperature of component (C) for 10 minutes and then cooling to 23°C to the initial viscosity (viscosity after heating / initial viscosity) is preferably 3 times or more, more preferably 4 times or more, and even more preferably 5 times or more. If the ratio of the viscosity after heating to the initial viscosity is within the above range, an excellent paste having a good balance between low initial viscosity and overflow suppressing property can be easily obtained.

[0066] The above-mentioned viscosity after heating is preferably a viscosity that makes the ratio of the viscosity after heating to the initial viscosity within the above-mentioned range, but from the perspective of being able to suppress overflow, etc., it is preferably 40 Pa·s or more, more preferably 50 Pa·s or more, and when the present paste is used for an application where overflow suppression is extremely important, as an example of a specific numerical value of the viscosity after heating, it is preferably 500 Pa·s or more, more preferably 1000 Pa·s or more, and particularly preferably 1500 Pa·s or more. When the viscosity after heating is within the above range, overflow after heating and thickening can be easily suppressed by flow resistance.

[0067] <Application of this paste> The present paste can be used without restriction for any purpose in which conventional pastes can be used. However, from the perspective of being able to better exert the effects of the present invention, the present paste is suitable for use in applications where it may be exposed to high temperatures (e.g., above 200°C), for applications where it is required to be stored in a paste form at a specified location even when the temperature is increased (even when heated), and in particular, for applications where it is required to have a low viscosity when the paste is formed at a specified location by coating or casting, and to be stored in a paste form at a specified location even when the temperature is increased (even when heated).

[0068] As the above-mentioned use, specifically, there can be mentioned the use of components such as sliding components or brake components, vibration suppression and absorption components, and further, as the use of the present paste containing the above-mentioned component (D), there can be mentioned the use of heat dissipation paste used between the heating element and the heat dissipation part of electronic components, etc. As the use in which the above-mentioned overflow suppression is extremely important, there can be mentioned the use of the heat dissipation paste.

[0069] In particular, the present paste containing the above-mentioned component (D) has a low initial viscosity and is a paste that can suppress overflow, base oil detachment, solidification, sagging, etc. after heating, and can maintain heat dissipation (thermal conductivity) for a long time, so it can be applied to devices, equipment, components, etc. with a heating element. By using this paste for this purpose, devices, equipment, components, etc. with excellent long-term reliability can be obtained. In particular, the initial viscosity of the paste is low and the adhesion with the heating element or the heat dissipation part is good, so a thin paste layer can be formed between the heating element and the heat dissipation part, reducing the thermal resistance generated by the paste layer, so it is suitable for use as a heat dissipation paste arranged between the heating element and the heat dissipation part. Furthermore, since it is not solidified, not easy to crack, and can absorb (suppress) vibration, it is particularly suitable for use as a heat dissipation paste for semiconductor devices such as power modules, and a heat dissipation paste for vehicles such as automobiles, and is particularly suitable for use as a heat dissipation paste for power modules.

[0070] As a method for forming the present paste at a predetermined position, there can be cited a method of applying the present paste to a predetermined position by a conventionally known coating method, or causing the present paste to flow into a predetermined position. When the present paste is formed between two components, after the present paste is applied or flows between these components, pressure can be applied while performing the following heating as required. For example, in the case where the present paste is formed between a heating element and a heat dissipation portion, the thickness of the present paste (layer) formed is preferably thin in consideration of thermal resistance. Therefore, in this case, it is preferred that after the present paste is formed between the heating element and the heat dissipation portion, pressure is applied to extend the present paste.

[0071] By heating (heating and thickening) the present paste formed at a predetermined location as described above, it is possible to prevent the paste from moving from the predetermined location where it is formed. The heating temperature at this time can be appropriately set according to the components used in the preparation of the paste, especially according to the type of component (C) used, and is preferably above 80°C, more preferably above 100°C, preferably below 200°C, more preferably below 170°C. Example

[0072] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0073] [Examples 1 to 21 and Comparative Examples 1 to 6] The respective blending components in Table 1 or 2 were mixed at the blending ratios (the numerical unit is parts by mass) shown in Table 1 or 2 to prepare a paste. The components in Table 1 and Table 2 are as follows.

[0074] Polysiloxane A-1: ​​"KF-2001" manufactured by Shin-Etsu Chemical Co., Ltd. (polysiloxane having a mercapto group, functional group equivalent weight: 1900 g / mol) Polysiloxane A-2: "KF-2004" manufactured by Shin-Etsu Chemical Co., Ltd. (polysiloxane having a mercapto group, functional group equivalent: 30,000 g / mol) Polysiloxane A-3: "X-22-167C" manufactured by Shin-Etsu Chemical Co., Ltd. (polysiloxane having a mercapto group, functional group equivalent: 2300 g / mol) Polysiloxane A': "KF-96-100CS" (dimethyl polysiloxane) manufactured by Shin-Etsu Chemical Co., Ltd. Compound B-1: "DMS-V25" produced by Gelest (polysiloxane containing two groups having ethylenically unsaturated bonds in one molecule, functional group equivalent: 8600 g / mol) Compound B-2: "DMS-V35" produced by Gelest (polysiloxane containing two groups having ethylenically unsaturated bonds in one molecule, functional group equivalent: 24750 g / mol) Compound B-3: "KE-1950-10A" manufactured by Shin-Etsu Chemical Co., Ltd. (polysiloxane having two ethylenically unsaturated bond groups in one molecule, functional group equivalent: 55350 g / mol) Compound B-4: "Hi-Cross M" manufactured by Seiko Chemical Industries, Ltd. (trimethylolpropane trimethacrylate, functional group equivalent: 112 g / mol) Compound B-5: "TAIC" manufactured by Mitsubishi Chemical Corporation (triallyl isocyanurate, functional group equivalent: 83 g / mol) Compound B-6: "Poly(ethylene glycol divinyl ether)" produced by Sigma-Aldrich (functional group equivalent weight: 125 g / mol) HEMA: 2-Hydroxyethyl Methacrylate · Initiator C-1: "PERCURE O" produced by NOF Corporation Initiator C-2: 2,2'-azobis(2-methylbutyronitrile) Initiator C-3: 2,2'-azobis(dimethyl isobutyrate) Initiator C-4: "PERHEXA 25B" produced by NOF Corporation Filler D-1: Advanced Alumina AA-1.5 (alumina powder) produced by Sumitomo Chemical Co., Ltd.

[0075] <Initial viscosity> The viscosity (initial viscosity) of the prepared paste at 23° C. was measured using a cone and plate viscometer (manufactured by Brookfield). The rotation speed was set to 200 rpm for Examples 1 to 10, Comparative Examples 1 to 3 and Comparative Example 5, the rotation speed was set to 100 rpm for Comparative Example 4, and the rotation speed was set to 1.5 rpm for Examples 11 to 21 and Comparative Example 6.

[0076] <Viscosity after heating> The viscosity of the prepared pastes after heating for 10 minutes at the 1-minute half-life temperature of the radical initiator (C) used in each paste and then cooling to 23° C. (post-heating viscosity) was measured using a cone and plate viscometer (Brookfield). Among them, in Examples 1 to 2 and Comparative Example 2, the rotational speed was set to 200 rpm for measurement, in Example 8, the rotational speed was set to 100 rpm for measurement, in Examples 4 to 7 and Example 9, the rotational speed was set to 10 rpm for measurement, in Example 10, Comparative Example 1 and Comparative Examples 3 to 5, the rotational speed was set to 1.5 rpm for measurement, in Example 3, the rotational speed was set to 0.5 rpm for measurement, and in Examples 11 to 21 and Comparative Example 6, the rotational speed was set to 0.1 rpm for measurement.

[0077] Tables 1 and 2 show the ratio of the shear viscosity after heating to the initial viscosity (viscosity after heating / initial viscosity) measured above.

[0078] <Paste properties> The prepared pastes were heat cured for 10 minutes at a temperature of 1 minute half-life of the free radical initiator (C) used in each paste. Then, 0.2 g of the heat-cured sample obtained by cooling to 23°C was drawn into a 5 mm square, and the thickness of the sample after compression at 23°C and 1.0 MPa was measured according to the following method. The results are shown in Tables 1 and 2.

[0079] The sample was compressed by stretching the sample by 0.2 g to a 5 mm square on a metal disc with a screw portion, then clamping it with another metal disc, and then tightening the screw at the screw portion with a torque wrench to load the sample with a load of 1.0 MPa.

[0080] The thickness was measured as follows. First, two metal discs were stacked and screwed together. After a load of 1 MPa was applied, the lengths of both ends of the two metal discs (without sample length) were measured after 3 minutes when a load of 1 MPa was applied. Next, on the metal disc, after stretching 0.2g of the sample to 5mm square, clamp it with another metal disc, tighten the screws, and load the sample with a load of 1.0MPa. Then, in order to eliminate the obstruction of the screw part, loosen the screws and remove the sample from the metal disc. The above-mentioned process of stretching 0.2g of the sample to 5mm square on the metal disc and then removing the sample from the metal disc is regarded as one cycle. After this one cycle is performed 5 times and 3 minutes after the 1MPa load in the 5th cycle is loaded, the length of the two ends of the two metal discs under the state of being loaded with a load of 1MPa (with sample length) is measured. The thickness of the sample was calculated by subtracting the length without the sample from the length with the sample, and the paste-like properties were evaluated based on the thickness of the sample. The thickness of the fifth cycle is measured as described above in order to prevent a part of the fluidity sample to be discharged from the characteristics of the measuring jig from being retained (clogged) in the screw portion and thus preventing a state in which an appropriate thickness cannot be measured.

[0081] When applying the above pressure, a pressure sample holder (made by NETZSCH Japan Co., Ltd., Flash Analyzer LFA467 accessories) and a torque wrench were used, and the thickness was measured using LITEMATIC VL-50 (made by Mitutoyo Co., Ltd.). As the metal disc, a metal disc made of SUS304, with a diameter of 14 mm, a thickness of 3 mm, and a surface roughness of Ra 0.2 was used.

[0082] Table 1

[0083] Table 2

[0084] The pastes obtained in Examples 1 to 21 were pastes that did not solidify even after being heated and thickened, and were pastes that could suppress overflow even when heated and thickened at a relatively low heating temperature despite having a low initial viscosity. The paste obtained in Comparative Example 2 could not be prevented from overflowing after being heated and thickened, and the pastes obtained in Comparative Examples 1 and 3 to 6 could not be called pastes (no fluidity) after being heated and solidified.

[0085] Since the present paste contains the above-mentioned components (A) to (C), the above-mentioned effects are exhibited. As an example of the reason why such effects are exhibited, the following reason is considered. In the present paste, it is considered that, in particular, by using the above-mentioned component (A), the component (A) reacts during heat curing (heat thickening), functions as a suitable plasticizer, and functions to promote crosslinking, and since it is not easy to bleed out, it is possible to thicken while maintaining the paste state. On the other hand, when polysiloxane containing a group having an ethylenically unsaturated bond or a conventional silicone oil is used instead of component (A) as in Comparative Examples 3 to 6, it is considered that the paste properties cannot be maintained after heat curing due to inability to perform appropriate thickening (thickening does not occur) or due to oozing of the silicone oil.

Claims

1. A paste comprising a polysiloxane having a mercapto group (A), a compound having two or more groups having an ethylenically unsaturated bond in one molecule (B), and a radical initiator (C).

2. The paste according to claim 1, wherein The ratio of the functional groups represented by the following formula (1) is less than 3: Functional group ratio = (the blending amount of the polysiloxane (A) / the functional group equivalent of the polysiloxane (A)) / (the blending amount of the compound (B) / the functional group equivalent of the compound (B)) ... (1) 3. The paste according to claim 1, wherein It satisfies the following condition (I): Condition (I): Heat curing is performed for 10 minutes at a temperature of 1 minute half-life of the free radical initiator (C), 0.2 g of the heat-cured paste is drawn into a 5 mm square, and then compressed at 23°C at a pressure of 1.0 MPa to a thickness of less than 200 μm.

4. The paste according to any one of claims 1 to 3, wherein The initial shear viscosity at 23°C is below 500 Pa·s.

5. The paste according to any one of claims 1 to 3, wherein The ratio of the shear viscosity after heating the paste at the 1-minute half-life temperature of the free radical initiator (C) for 10 minutes and then cooling to 23° C. to the initial shear viscosity of the paste at 23° C. is more than 3 times.

6. The paste according to any one of claims 1 to 3, wherein Contains thermally conductive filler (D).

7. The paste according to claim 6, wherein The content of the thermally conductive filler (D) is 30 to 80 volume % relative to 100 volume % of the paste.