A long-lasting fragrance type air filter element and a method of making the same

By using a fixed frame structure and aromatherapy particles coated with semi-degradable water-based paint in the air filter, the fragrance is slowly released, solving the problem of short-lived fragrance in aromatherapy air filters and achieving long-lasting fragrance and economical production.

CN118925359BActive Publication Date: 2026-11-24DONGGUAN AIR GUARD FILTER MANUFACTURING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411152907.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2026-11-24
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The fragrance of existing aromatherapy air filters is not long-lasting enough, leading to frequent replacements, which affects the user experience and economic costs.

Method used

It adopts a fixed frame structure, including a PET short fiber primary filter layer, a meltblown PP layer, a honeycomb carrier and a mesh cover. The honeycomb pores are filled with activated carbon and aroma particles. The particle body is coated with a semi-degradable water-based coating to control the membrane thickness and component ratio, slowly release fragrance, and form a microporous structure to maintain the fragrance.

Benefits of technology

It achieves a long-lasting fragrance effect for the aromatherapy air filter, lasting for 5-7 months, avoiding frequent replacements and reducing production costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118925359B_ABST
    Figure CN118925359B_ABST
Patent Text Reader

Abstract

This invention relates to the field of air filter technology, specifically to a long-lasting fragrance air filter and its preparation method. The air filter includes a fixed frame, and a PET short fiber primary filter layer, a melt-blown PP layer, a first mesh cover, a honeycomb carrier, and a second mesh cover, all fixedly installed within the fixed frame and sequentially bonded together. The honeycomb pores of the honeycomb carrier are filled with a number of activated carbon particles and a number of fragrance particles. The fragrance particles consist of a particle body and a membrane layer covering the particle body. The membrane layer is formed by coating the surface of the particle body with a semi-degradable water-based coating at least twice and then drying it. The entire fragrance retention process lasts for 5-7 months, achieving a longer-lasting fragrance effect and avoiding frequent replacement of the air filter due to the loss of fragrance in a short period of time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of air filter technology, specifically to a long-lasting fragrance air filter and its preparation method. Background Technology

[0002] When a car is in motion, it typically draws in outside air, which contains many different particles such as dust, pollen, soot, abrasive particles, ozone, odors, nitrogen oxides, sulfur dioxide, carbon dioxide, and benzene. An air filter can separate solid impurities like dust, pollen, and abrasive particles from the air, and can also absorb moisture, soot, ozone, odors, carbon oxides, SO2, and CO2, providing excellent protection. For typical city passenger cars, the air filter usually only needs to be replaced every six months.

[0003] A car air freshener filter is a car accessory that combines air filtration and fragrance functions. It improves the air quality inside the car and provides a long-lasting scent. It works by attaching fragrance molecules to the filter, which then fills the entire cabin with fragrance as the air enters. This product not only helps improve air quality and reduce odors, but also enhances driving comfort.

[0004] However, the fragrance of aromatherapy filters gradually weakens, and the fragrance of commercially available aromatherapy filters is not long-lasting. Even if fragrance is added to the filter, it will usually lose its fragrance completely after 3 months of use, so it needs to be replaced frequently every 3 months. Summary of the Invention

[0005] In order to overcome the shortcomings and deficiencies of the existing technology, the purpose of this invention is to provide a long-lasting fragrance air filter, which has a longer-lasting fragrance in actual use.

[0006] Another objective of this invention is to provide a method for preparing a long-lasting fragrance air filter element. This method is simple to operate, easy to control, has high production efficiency, low production cost, and can be used for large-scale production.

[0007] The objective of this invention is achieved through the following technical solution: a long-lasting fragrance air filter, comprising a fixed frame, and a PET short fiber primary filter layer, a melt-blown PP layer, a first mesh cover, a honeycomb carrier, and a second mesh cover, all fixedly installed within the fixed frame and sequentially bonded together. The honeycomb pores of the honeycomb carrier are filled with a number of activated carbon particles and a number of fragrance particles. The fragrance particles consist of a particle body and a membrane layer covering the particle body. The membrane layer is formed by coating the surface of the particle body with a semi-degradable water-based coating at least twice and then drying it.

[0008] This invention relates to a long-lasting fragrance-type air filter. A fixed frame secures a PET short-fiber primary filter layer, a melt-blown PP layer, a first mesh cover, a honeycomb carrier, and a second mesh cover. The PET short-fiber primary filter layer, the melt-blown PP layer, and the honeycomb carrier filled with activated carbon particles sequentially filter the air to ensure the filter's effectiveness. The honeycomb pores of the honeycomb carrier are also filled with several fragrance particles, and the particles are coated with a membrane to prevent the fragrance oils from rapidly diffusing and losing their aroma. When installed in a car's air conditioning system, the fragrance is slowly released during the initial stage due to the intermolecular diffusion of the fragrance particles. The appropriate number of fragrance particles helps ensure a slow, minute release of fragrance into the car's interior, achieving a more comfortable fragrance concentration. After 2-4 months of use, the fragrance gradually fades due to the particles... As the fragrance essential oil content of the filter itself decreases, the diffusion and release of fragrance from the low-concentration fragrance essential oil molecules is reduced. However, the membrane layer is formed by coating the surface of the filter particles with semi-degradable water-based paint at least twice and then drying it. During this drying process, the semi-degradable water-based paint membrane layer is affected by environmental microorganisms, temperature, and humidity. The semi-degradation of the membrane layer forms a microporous structure, which creates channels for releasing fragrance, allowing the fragrance essential oil to diffuse and maintain the fragrance. Over time, after the air filter is used for another 1-2 months, the fragrance essential oil content of the filter particles themselves decreases further, while the microporous structure formed by the semi-degradation of the membrane layer becomes larger and more numerous, creating larger and more numerous channels for releasing fragrance. This allows the lower concentration of fragrance essential oil in the filter particles to be released until the fragrance is lost. The entire fragrance retention process lasts for 5-7 months, achieving a longer-lasting fragrance effect and avoiding frequent replacement of the air filter due to the loss of fragrance in a short period of time.

[0009] Preferably, the thickness of the membrane layer is 0.5-1.0 mm; in the honeycomb pores, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:3-5.

[0010] Using the above technical solution, semi-degradable water-based coating is applied to the surface of the granules at least twice to increase the film thickness. The film thickness is controlled at 0.5-1.0 mm to improve the diffusion barrier effect on the fragrance essential oils of the granules, preventing the rapid diffusion of high-concentration fragrance essential oils and loss of fragrance. The activated carbon granules and aromatherapy granules are mixed at a weight ratio of 2:3-5. At the same time, due to the barrier effect of the film thickness, it is more conducive to ensuring that the fragrance of the air filter element is moderate in the early stage of use.

[0011] Preferably, the particulate body comprises the following components in parts by weight:

[0012] 60-70 parts of ethylene-vinyl acetate copolymer

[0013] 30-40 parts perlite powder loaded with fragrance essential oils

[0014] 1-3 parts of lubricating dispersant

[0015] Colorant 1-3 parts.

[0016] Using the above technical solution, the particle body is based on ethylene-vinyl acetate copolymer. Under the action of lubricating dispersant, the perlite micro powder loaded with fragrance essential oil and the colorant are uniformly dispersed in the particle body. On the one hand, the ethylene-vinyl acetate copolymer coats most of the perlite micro powder loaded with fragrance essential oil, avoiding the rapid diffusion of high concentration of fragrance essential oil and loss of fragrance. On the other hand, the perlite micro powder acts as a carrier to adsorb a large amount of fragrance essential oil, further avoiding the rapid diffusion of high concentration of fragrance essential oil and loss of fragrance. It makes full use of intermolecular diffusion to slowly release fragrance, avoiding the high concentration of fragrance essential oil in the air filter at the beginning of use, which is not conducive to long-lasting fragrance retention, and at the same time avoiding the discomfort caused by high concentration of fragrance.

[0017] Preferably, the density of the ethylene-vinyl acetate copolymer is 0.94-0.96 g / cm³. 3 The melting temperature is 45-66℃; the perlite micro powder loaded with fragrance essential oil is made by mixing fragrance essential oil and perlite micro powder in a weight ratio of 5-7:4-5.

[0018] By adopting the above technical solution, an ethylene-vinyl acetate copolymer with a melting temperature of 45-66℃ is selected. This allows for granulation at a lower melt extrusion temperature during particle preparation, avoiding excessively high temperatures that would accelerate the volatilization of essential oils, leading to increased essential oil loss and reduced fragrance retention. This also helps reduce production costs and save energy. The essential oils and perlite powder are mixed at a weight ratio of 5-7:4-5. The microporous adsorption properties of perlite powder are utilized to adsorb the essential oils, improving the utilization rate of both perlite powder and essential oils, and enhancing the long-lasting fragrance retention of the aromatherapy particles. Furthermore, the type of the ethylene-vinyl acetate copolymer includes, but is not limited to, Arkema EVATANE42-60, EA33045, or Hanwha 1529; the particle size of the perlite powder is 10-30 μm; the type of fragrance essential oil includes, but is not limited to, at least one of bergamot essential oil, lemon essential oil, lavender essential oil, jasmine essential oil, rose essential oil, ylang-ylang essential oil, lemongrass essential oil, peppermint essential oil, cedarwood essential oil, or eucalyptus essential oil, and more preferably, the fragrance essential oil is lemon essential oil.

[0019] Preferably, the lubricating dispersant is pentaerythritol stearate and / or carboxymethyl cellulose; the colorant is at least one of titanium dioxide, carbon black, mica powder, iron oxide yellow or iron oxide red.

[0020] In a more preferred embodiment of the above technical solution, the lubricating dispersant is a mixture of pentaerythritol stearate and carboxymethyl cellulose in a 1:1 weight ratio. The synergistic effect of these two components further promotes the uniform dispersion of the perlite powder and colorant loaded with fragrance essential oils. Pentaerythritol stearate helps maintain the dispersed state of the solid particles, while the unique network structure of carboxymethyl cellulose serves as an excellent carrier for the perlite powder and colorant, enabling them to be uniformly and stably dispersed on the carrier. This not only ensures good dispersion of the perlite powder and colorant in the ethylene-vinyl acetate copolymer matrix, preventing agglomeration and improving the dispersion of the perlite powder and colorant within the particle body, but also facilitates the slow release of fragrance essential oils and long-lasting fragrance retention.

[0021] Preferably, the method for preparing the granule body includes the following steps: mixing ethylene-vinyl acetate copolymer, perlite micro powder loaded with fragrance essential oil, lubricant dispersant and colorant evenly according to weight parts, and then extruding and granulating the mixture through a twin-screw extruder to obtain the granule body; wherein, the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are 45-55℃, 55-65℃, 65-75℃, 65-80℃, and 60-75℃, respectively, the die head temperature is 60-75℃, the screw length-to-diameter ratio is 25:1, and the screw speed is 60-150 r / min.

[0022] By adopting the above technical solution, granulation is performed at a lower melt extrusion temperature, which avoids excessively high temperatures that would accelerate the volatilization of fragrance oils, leading to increased loss of fragrance oils and reduced fragrance retention. This helps to reduce production costs and save energy.

[0023] Preferably, the semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0024]

[0025]

[0026] Using the above technical solution, the semi-degradable waterborne coating uses waterborne acrylic resin and waterborne polyurethane resin as the main resins, and adds polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent, and deionized water. After curing, the semi-degradable waterborne coating has film-forming barrier and semi-degradation effects. Among them, polylactic acid is fully mixed with other components and then coated to form a uniform film layer. Initially, the air filter element has a good air filtration effect. After a period of use, due to the presence of dust, microorganisms, etc. in the air, microorganisms may adhere to the air filter element. Affected by environmental microorganisms, temperature, and humidity, polylactic acid gradually degrades, resulting in the semi-degradation of the film layer and the formation of a microporous structure, that is, forming channels for releasing fragrance, allowing the fragrance essential oil to diffuse and maintain the fragrance.

[0027] Preferably, the waterborne acrylic resin is NeocryI XK-540 or DB3618; the waterborne polyurethane resin is PU-3486 or H-34P; and the polylactic acid has an average molecular weight of 30,000-50,000 and a molecular weight distribution between 10,000-60,000.

[0028] The above technical solution controls the average molecular weight of polylactic acid to be 30,000-50,000, with a molecular weight distribution between 10,000-60,000. This allows lower molecular weight polylactic acid to completely degrade in a shorter time, forming local micropores to release fragrance. Higher molecular weight polylactic acid then undergoes complete degradation, resulting in a larger and more numerous micropore structure formed by the semi-degradation of the membrane layer. This creates larger and more numerous channels for releasing fragrance, allowing the lower concentration of fragrance essential oil in the particle itself to be maintained until the fragrance is lost. The entire fragrance retention process lasts for 6-7 months, achieving a longer-lasting fragrance effect and avoiding frequent replacement of the air filter due to the loss of fragrance in a short period.

[0029] Preferably, the dispersant is BYK-190 or BYK192; the defoamer is BYK-028; the wetting agent is BASF WE3229 or TEGO WET280; the thickener is at least one of sodium carboxymethyl cellulose, propylene glycol alginate, or sodium carboxymethyl starch; the film-forming aid is dipropylene glycol butyl ether or diethylene glycol monobutyl ether; and the cosolvent is isopropanol and / or ethanol.

[0030] More preferably, the preparation method of the semi-degradable waterborne coating includes the following steps:

[0031] (R1) Take waterborne acrylic resin, waterborne polyurethane resin, polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water in parts by weight, and set aside.

[0032] (R2) Add polylactic acid to the co-solvent and mix well to obtain a premixed solution;

[0033] (R3) Add waterborne acrylic resin, waterborne polyurethane resin, fumed silica, wetting agent, dispersant, premix and defoamer to deionized water and mix evenly. Then add thickener and film-forming aid and mix evenly to obtain semi-degradable waterborne coating.

[0034] Another objective of the present invention is achieved through the following technical solution: the preparation method of the above-mentioned long-lasting fragrance air filter includes the following steps:

[0035] (S1) The PET short fiber primary filter layer, meltblown PP layer, first mesh cover and honeycomb carrier are bonded together in sequence to form a multi-layer structure. Then the outer periphery of the multi-layer structure is bonded to the inner wall of the fixed frame to obtain the filter element semi-finished product.

[0036] (S2) After filling the honeycomb cells of the honeycomb carrier with a number of activated carbon particles and a number of aroma particles, the second mesh cover is glued to the side of the honeycomb carrier away from the first mesh cover, and after sealing, a long-lasting fragrance air filter is obtained.

[0037] In the honeycomb carrier, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:3-5 within the honeycomb pores.

[0038] The beneficial effects of this invention are as follows: The long-lasting fragrance air filter of this invention uses a fixed frame to fix the PET short fiber primary filter layer, melt-blown PP layer, first mesh cover, honeycomb carrier, and second mesh cover. The PET short fiber primary filter layer, melt-blown PP layer, and honeycomb carrier filled with activated carbon particles sequentially filter the air to ensure the filtration effect of the air filter itself. The honeycomb pores of the honeycomb carrier are also filled with several fragrance particles, and the particle body is covered by a membrane layer to prevent the fragrance essential oil in the particle body from rapidly diffusing and losing its fragrance due to high concentration of fragrance essential oil. In the initial stage of use when installed in the car's air conditioning air filter, the fragrance is slowly released through the intermolecular diffusion of the fragrance particles. Furthermore, the appropriate number of fragrance particles helps to ensure a slow, trace release of fragrance in the car's interior space, achieving a more comfortable fragrance concentration for the human body. After 2-4 months of use, the air filter... Because the essential oil content of the particles themselves decreases, the diffusion and release of fragrance from the low-concentration essential oil molecules is reduced. However, the membrane layer is made by coating the surface of the particles with semi-degradable water-based paint at least twice and then drying it. During this drying process, the semi-degradable water-based paint membrane layer is affected by environmental microorganisms, temperature, and humidity. The membrane layer semi-degrades and forms a microporous structure, which forms channels for releasing fragrance, allowing the essential oil to diffuse and maintain the fragrance. Over time, after the air filter is used for another 1-2 months, the essential oil content of the particles themselves decreases, while the microporous structure formed by the semi-degradation of the membrane layer becomes larger and more numerous, forming larger and more numerous channels for releasing fragrance. This allows the lower concentration of essential oil in the particles to be released until the fragrance is lost. The entire fragrance retention process lasts for 6-7 months, achieving a longer-lasting fragrance effect and avoiding frequent replacement of the air filter due to the loss of fragrance in a short period of time.

[0039] The preparation method of the present invention is simple to operate, easy to control, has high production efficiency, low production cost, and can be used for large-scale production. Attached Figure Description

[0040] Figure 1 This is a schematic diagram of the structure of the present invention;

[0041] Figure 2 This is a SEM image of the initial aromatherapy particles in Example 1 of the present invention;

[0042] Figure 3This is a SEM image of the aromatherapy granules after 3 months of use in Example 1 of the present invention;

[0043] Figure 4 This is a SEM image of the aromatherapy granules after 5 months of use in Example 1 of the present invention.

[0044] The attached diagram is labeled as follows: 1. Fixed frame; 2. PET short fiber primary filter layer; 3. Meltblown PP layer; 4. First mesh cover; 5. Honeycomb carrier; 6. Second mesh cover; 7. Activated carbon particles; 8. Aromatherapy particles. Detailed Implementation

[0045] To facilitate understanding by those skilled in the art, the present invention will be further described below with reference to embodiments and accompanying drawings. The content mentioned in the embodiments is not intended to limit the present invention.

[0046] Example 1

[0047] like Figure 1 As shown, a long-lasting fragrance air filter includes a fixed frame 1, and a PET short fiber primary filter layer 2, a melt-blown PP layer 3, a first mesh cover 4, a honeycomb carrier 5, and a second mesh cover 6, all fixedly installed within the fixed frame 1 and sequentially bonded together. The honeycomb pores of the honeycomb carrier 5 are filled with a number of activated carbon particles 7 and a number of fragrance particles 8. The fragrance particles 8 consist of a particle body and a membrane layer covering the particle body. The membrane layer is formed by coating the surface of the particle body twice with a semi-degradable water-based coating and then drying it.

[0048] The thickness of the membrane is 0.6 mm; in the honeycomb pores of the honeycomb carrier, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:4.

[0049] The particle body comprises the following components in parts by weight:

[0050]

[0051] The perlite micro powder loaded with fragrance essential oil is made by mixing fragrance essential oil and perlite micro powder in a weight ratio of 6:4.5. The particle size of the perlite micro powder is 20 μm; the fragrance essential oil is lemon essential oil.

[0052] The lubricating dispersant is a mixture of pentaerythritol stearate and carboxymethyl cellulose in a weight ratio of 1:1; the colorant is iron oxide red.

[0053] The preparation method of the granule body includes the following steps: ethylene-vinyl acetate copolymer EA33045, perlite micro powder loaded with fragrance essential oil, lubricant dispersant and colorant are mixed evenly according to weight parts, and then extruded and granulated by a twin-screw extruder to obtain the granule body; wherein, the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are 50℃, 60℃, 70℃, 75℃, and 65℃, respectively, the die head temperature is 62℃, the screw length-to-diameter ratio is 25:1, and the screw speed is 120r / min.

[0054] The semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0055]

[0056] The waterborne acrylic resin is NeoCryI XK-540; the waterborne polyurethane resin is PU-3486; the polylactic acid has an average molecular weight of 40,000 and a molecular weight distribution between 10,000 and 60,000.

[0057] The dispersant is BYK-190; the defoamer is BYK-028; the wetting agent is TEGO WET280; the thickener is propylene glycol alginate; the film-forming aid is dipropylene glycol butyl ether; and the cosolvent is a mixture of isopropanol and ethanol in a volume ratio of 10:1.

[0058] The preparation method of the semi-degradable water-based coating includes the following steps:

[0059] (R1) Take waterborne acrylic resin, waterborne polyurethane resin, polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water in parts by weight, and set aside.

[0060] (R2) Add polylactic acid to the co-solvent and mix well to obtain a premixed solution;

[0061] (R3) Add waterborne acrylic resin, waterborne polyurethane resin, fumed silica, wetting agent, dispersant, premix and defoamer to deionized water and mix evenly. Then add thickener and film-forming aid and mix evenly to obtain semi-degradable waterborne coating.

[0062] The method for preparing the long-lasting fragrance air filter includes the following steps:

[0063] (S1) The PET short fiber primary filter layer 2, meltblown PP layer 3, first mesh cover 4, and honeycomb carrier 5 are bonded together in sequence to form a multi-layer structure. Then the outer periphery of the multi-layer structure is bonded to the inner wall of the fixed frame 1 to obtain the filter element semi-finished product.

[0064] (S2) After filling the honeycomb holes of the honeycomb carrier 5 with a number of activated carbon particles 7 and a number of aroma particles 8, the second mesh cover 6 is glued to the side of the honeycomb carrier 5 away from the first mesh cover 4, and after encapsulation, a long-lasting fragrance air filter is obtained.

[0065] Example 2

[0066] like Figure 1 As shown, a long-lasting fragrance air filter includes a fixed frame 1, and a PET short fiber primary filter layer 2, a melt-blown PP layer 3, a first mesh cover 4, a honeycomb carrier 5, and a second mesh cover 6, all fixedly installed within the fixed frame 1 and sequentially bonded together. The honeycomb pores of the honeycomb carrier 5 are filled with a number of activated carbon particles 7 and a number of fragrance particles 8. The fragrance particles 8 consist of a particle body and a membrane layer covering the particle body. The membrane layer is formed by coating the surface of the particle body twice with a semi-degradable water-based coating and then drying it.

[0067] The thickness of the membrane is 0.5 mm; in the honeycomb pores of the honeycomb carrier, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:3.

[0068] The particle body comprises the following components in parts by weight:

[0069]

[0070] The perlite micro powder loaded with fragrance essential oil is made by mixing fragrance essential oil and perlite micro powder in a weight ratio of 5:5. The particle size of the perlite micro powder is 10 μm; the fragrance essential oil is lemon essential oil.

[0071] The lubricating dispersant is a mixture of pentaerythritol stearate and carboxymethyl cellulose in a weight ratio of 1:1; the colorant is iron oxide red.

[0072] The preparation method of the granule body includes the following steps: ethylene-vinyl acetate copolymer EA33045, perlite micro powder loaded with fragrance essential oil, lubricant dispersant and colorant are mixed evenly according to weight parts, and then extruded and granulated by a twin-screw extruder to obtain the granule body; wherein, the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are 50℃, 60℃, 70℃, 75℃, and 65℃, respectively, the die head temperature is 62℃, the screw length-to-diameter ratio is 25:1, and the screw speed is 120r / min.

[0073] The semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0074]

[0075] The waterborne acrylic resin is NeoCryI XK-540; the waterborne polyurethane resin is PU-3486; the polylactic acid has an average molecular weight of 30,000 and a molecular weight distribution between 10,000 and 60,000.

[0076] The dispersant is BYK-190; the defoamer is BYK-028; the wetting agent is TEGO WET280; the thickener is propylene glycol alginate; the film-forming aid is dipropylene glycol butyl ether; and the cosolvent is a mixture of isopropanol and ethanol in a volume ratio of 10:1.

[0077] The preparation method of the semi-degradable water-based coating includes the following steps:

[0078] (R1) Take waterborne acrylic resin, waterborne polyurethane resin, polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water in parts by weight, and set aside.

[0079] (R2) Add polylactic acid to the co-solvent and mix well to obtain a premixed solution;

[0080] (R3) Add waterborne acrylic resin, waterborne polyurethane resin, fumed silica, wetting agent, dispersant, premix and defoamer to deionized water and mix evenly. Then add thickener and film-forming aid and mix evenly to obtain semi-degradable waterborne coating.

[0081] The method for preparing the long-lasting fragrance air filter includes the following steps:

[0082] (S1) The PET short fiber primary filter layer 2, meltblown PP layer 3, first mesh cover 4, and honeycomb carrier 5 are bonded together in sequence to form a multi-layer structure. Then the outer periphery of the multi-layer structure is bonded to the inner wall of the fixed frame 1 to obtain the filter element semi-finished product.

[0083] (S2) After filling the honeycomb holes of the honeycomb carrier 5 with a number of activated carbon particles 7 and a number of aroma particles 8, the second mesh cover 6 is glued to the side of the honeycomb carrier 5 away from the first mesh cover 4, and after encapsulation, a long-lasting fragrance air filter is obtained.

[0084] Example 3

[0085] like Figure 1As shown, a long-lasting fragrance air filter includes a fixed frame 1, and a PET short fiber primary filter layer 2, a melt-blown PP layer 3, a first mesh cover 4, a honeycomb carrier 5, and a second mesh cover 6, all fixedly installed within the fixed frame 1 and sequentially bonded together. The honeycomb pores of the honeycomb carrier 5 are filled with a number of activated carbon particles 7 and a number of fragrance particles 8. The fragrance particles 8 consist of a particle body and a membrane layer covering the particle body. The membrane layer is formed by coating the surface of the particle body twice with a semi-degradable water-based coating and then drying it.

[0086] The thickness of the membrane layer is 1.0 mm; in the honeycomb pores of the honeycomb carrier, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:5.

[0087] The particle body comprises the following components in parts by weight:

[0088]

[0089]

[0090] The perlite micro powder loaded with fragrance essential oil is made by mixing fragrance essential oil and perlite micro powder in a weight ratio of 7:5. The particle size of the perlite micro powder is 30 μm; the fragrance essential oil is lemon essential oil.

[0091] The lubricating dispersant is a mixture of pentaerythritol stearate and carboxymethyl cellulose in a weight ratio of 1:1; the colorant is iron oxide red.

[0092] The preparation method of the granule body includes the following steps: ethylene-vinyl acetate copolymer EA33045, perlite micro powder loaded with fragrance essential oil, lubricant dispersant and colorant are mixed evenly according to weight parts, and then extruded and granulated by a twin-screw extruder to obtain the granule body; wherein, the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are 50℃, 60℃, 70℃, 75℃, and 65℃, respectively, the die head temperature is 62℃, the screw length-to-diameter ratio is 25:1, and the screw speed is 120r / min.

[0093] The semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0094]

[0095] The waterborne acrylic resin is NeoCryI XK-540; the waterborne polyurethane resin is PU-3486; the polylactic acid has an average molecular weight of 50,000 and a molecular weight distribution between 10,000 and 60,000.

[0096] The dispersant is BYK-190; the defoamer is BYK-028; the wetting agent is TEGO WET280; the thickener is propylene glycol alginate; the film-forming aid is dipropylene glycol butyl ether; and the cosolvent is a mixture of isopropanol and ethanol in a volume ratio of 10:1.

[0097] The preparation method of the semi-degradable water-based coating includes the following steps:

[0098] (R1) Take waterborne acrylic resin, waterborne polyurethane resin, polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water in parts by weight, and set aside.

[0099] (R2) Add polylactic acid to the co-solvent and mix well to obtain a premixed solution;

[0100] (R3) Add waterborne acrylic resin, waterborne polyurethane resin, fumed silica, wetting agent, dispersant, premix and defoamer to deionized water and mix evenly. Then add thickener and film-forming aid and mix evenly to obtain semi-degradable waterborne coating.

[0101] The method for preparing the long-lasting fragrance air filter includes the following steps:

[0102] (S1) The PET short fiber primary filter layer 2, meltblown PP layer 3, first mesh cover 4, and honeycomb carrier 5 are bonded together in sequence to form a multi-layer structure. Then the outer periphery of the multi-layer structure is bonded to the inner wall of the fixed frame 1 to obtain the filter element semi-finished product.

[0103] (S2) After filling the honeycomb holes of the honeycomb carrier 5 with a number of activated carbon particles 7 and a number of aroma particles 8, the second mesh cover 6 is glued to the side of the honeycomb carrier 5 away from the first mesh cover 4, and after encapsulation, a long-lasting fragrance air filter is obtained.

[0104] Example 4

[0105] like Figure 1 As shown, a long-lasting fragrance air filter includes a fixed frame 1, and a PET short fiber primary filter layer 2, a melt-blown PP layer 3, a first mesh cover 4, a honeycomb carrier 5, and a second mesh cover 6, all fixedly installed within the fixed frame 1 and sequentially bonded together. The honeycomb pores of the honeycomb carrier 5 are filled with a number of activated carbon particles 7 and a number of fragrance particles 8. The fragrance particles 8 consist of a particle body and a membrane layer covering the particle body. The membrane layer is formed by coating the surface of the particle body twice with a semi-degradable water-based coating and then drying it.

[0106] The thickness of the membrane is 0.7 mm; in the honeycomb pores of the honeycomb carrier, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:4.

[0107] The particle body comprises the following components in parts by weight:

[0108]

[0109] The perlite micro powder loaded with fragrance essential oil is made by mixing fragrance essential oil and perlite micro powder in a weight ratio of 6:5. The particle size of the perlite micro powder is 10 μm; the fragrance essential oil is lemon essential oil.

[0110] The lubricating dispersant is a mixture of pentaerythritol stearate and carboxymethyl cellulose in a weight ratio of 1:1; the colorant is iron oxide red.

[0111] The preparation method of the granule body includes the following steps: ethylene-vinyl acetate copolymer EA33045, perlite micro powder loaded with fragrance essential oil, lubricant dispersant and colorant are mixed evenly according to weight parts, and then extruded and granulated by a twin-screw extruder to obtain the granule body; wherein, the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are 50℃, 60℃, 70℃, 75℃, and 65℃, respectively, the die head temperature is 62℃, the screw length-to-diameter ratio is 25:1, and the screw speed is 120r / min.

[0112] The semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0113]

[0114]

[0115] The waterborne acrylic resin is NeoCryI XK-540; the waterborne polyurethane resin is PU-3486; the polylactic acid has an average molecular weight of 40,000 and a molecular weight distribution between 10,000 and 60,000.

[0116] The dispersant is BYK-190; the defoamer is BYK-028; the wetting agent is TEGO WET280; the thickener is propylene glycol alginate; the film-forming aid is dipropylene glycol butyl ether; and the cosolvent is a mixture of isopropanol and ethanol in a volume ratio of 10:1.

[0117] The preparation method of the semi-degradable water-based coating includes the following steps:

[0118] (R1) Take waterborne acrylic resin, waterborne polyurethane resin, polylactic acid, fumed silica, dispersant, defoamer, wetting agent, thickener, film-forming aid, cosolvent and deionized water in parts by weight, and set aside.

[0119] (R2) Add polylactic acid to the co-solvent and mix well to obtain a premixed solution;

[0120] (R3) Add waterborne acrylic resin, waterborne polyurethane resin, fumed silica, wetting agent, dispersant, premix and defoamer to deionized water and mix evenly. Then add thickener and film-forming aid and mix evenly to obtain semi-degradable waterborne coating.

[0121] The method for preparing the long-lasting fragrance air filter includes the following steps:

[0122] (S1) The PET short fiber primary filter layer 2, meltblown PP layer 3, first mesh cover 4, and honeycomb carrier 5 are bonded together in sequence to form a multi-layer structure. Then the outer periphery of the multi-layer structure is bonded to the inner wall of the fixed frame 1 to obtain the filter element semi-finished product.

[0123] (S2) After filling the honeycomb holes of the honeycomb carrier 5 with a number of activated carbon particles 7 and a number of aroma particles 8, the second mesh cover 6 is glued to the side of the honeycomb carrier 5 away from the first mesh cover 4, and after encapsulation, a long-lasting fragrance air filter is obtained.

[0124] Comparative Example 1

[0125] The difference between this comparative example and Example 1 is as follows:

[0126] The semi-degradable water-based coating comprises the following raw materials in parts by weight:

[0127]

[0128] Eight parts of deionized water; that is, the semi-degradable water-based coating does not contain polylactic acid.

[0129] Comparative Example 2

[0130] The difference between this comparative example and Example 1 is as follows:

[0131] The film layer is formed by coating the surface of the particle body with a semi-degradable water-based coating once and then drying it, and the thickness of the film layer is 0.2 mm.

[0132] Comparative Example 3

[0133] The difference between this comparative example and Example 1 is as follows:

[0134] The particle body comprises the following components in parts by weight:

[0135]

[0136] The titanium dioxide doped with fragrance essential oil is made by mixing fragrance essential oil and titanium dioxide in a weight ratio of 6:4.5. The particle size of the titanium dioxide is 20 μm.

[0137] The preparation method of the granule body includes the following steps: ethylene-vinyl acetate copolymer EA33045, titanium dioxide doped with fragrance essential oil, lubricant dispersant and colorant are mixed evenly according to the weight parts, and then extruded and granulated by a twin-screw extruder to obtain the granule body.

[0138] Comparative Example 4

[0139] An air filter element, from a commercially available brand: Qingxi, product name: car air conditioning air filter element, product number: 10054267311135.

[0140] Example 5

[0141] Performance testing:

[0142] I. Multiple sets of air filter elements from Example 1 were assembled into the same model of vehicle (Great Wall C50) and used in urban areas. Initial fragrance particles, fragrance particles after 3 months of use, and fragrance particles after 5 months of use were collected and scanned using SEM. SEM morphology images of the initial fragrance particles, fragrance particles after 3 months of use, and fragrance particles after 5 months of use were obtained, as shown below. Figure 2-4 As shown, it can be seen that the membrane layer of the aromatherapy particles can be semi-degraded to obtain a microporous structure during actual use. As time goes by, the microporous structure formed by the semi-degradation of the membrane layer is larger and more numerous, that is, the channels for releasing fragrance are larger and more numerous.

[0143] II. Multiple sets of air filters from Examples 1-4 and Comparative Examples 1-4 were assembled into the same model of vehicle (Great Wall C50) and used in urban areas. Initial air filters, air filters after 1 month of use, air filters after 3 months of use, air filters after 5 months of use, and air filters after 7 months of use were collected. The fragrance level was tested using an XP-329IIIR odor detector. During the test, the detector probe was placed against the center of the second mesh cover, and the values ​​were recorded. The test results are shown in Table 1 below:

[0144]

[0145]

[0146] As shown in Table 1 above, the long-lasting fragrance air filter of this application has a better fragrance retention effect and longer-lasting fragrance. From the usage results of Examples 1-4, the air filter after 3 months of use has a stronger fragrance than the one-month-old air filter. This is mainly because the semi-degradation of the membrane layer forms microporous channels, promoting the diffusion and release of fragrance essential oils to maintain the fragrance retention effect of the air filter. The fragrance of the air filter after 5 months of use is somewhat weakened, mainly because the concentration of residual fragrance essential oils is lower, but the microporous channels are larger and more numerous, further promoting the diffusion and release of fragrance essential oils to maintain the fragrance intensity to a certain extent. The weakening of the fragrance is not significant and is not difficult for consumers to notice, thus still demonstrating its fragrance retention effect. However, after 7 months of use, the fragrance essential oils in the air filter have almost completely evaporated, and consumers cannot smell the fragrance. For Example 3, due to its thicker membrane layer, more fragrance particles, and larger average molecular weight of polylactic acid, the fragrance retention effect and longer-lasting fragrance are better. Compared to Comparative Example 1, the membrane layer of Example 1 contains a certain amount of polylactic acid, which is beneficial for the degradation of polylactic acid to form a microporous structure after a period of use, so as to release the fragrance essential oil. Otherwise, with low concentrations of fragrance essential oil blocked by the membrane layer and the particle body, it only relies on intermolecular diffusion, which, although the fragrance lasts longer, results in a weaker fragrance and poor fragrance retention. Compared to Comparative Example 2, the membrane layer of Example 1 is controlled at 0.5-1 mm to improve its fragrance release blocking effect, which is conducive to the slow release of fragrance essential oil in the early stage of use, avoiding excessively high release concentration and overly strong fragrance that may cause consumer discomfort. Compared to Comparative Example 3, Example 1 uses perlite micropowder to load fragrance essential oil, and utilizes the adsorption properties of perlite micropowder to avoid rapid evaporation and diffusion of fragrance essential oil, which would lead to insufficient fragrance retention in the later stage of use. Compared to Comparative Example 4, Example 1 uses the specific air filter of this invention, which has a better fragrance retention effect and longer-lasting fragrance retention.

[0147] The above embodiments are preferred implementations of the present invention. In addition, the present invention can be implemented in other ways. Any obvious substitutions without departing from the concept of the present invention are within the protection scope of the present invention.

Claims

1. A long-lasting fragrance air filter, characterized in that: The device includes a fixed frame, and a PET short fiber primary filter layer, a meltblown PP layer, a first mesh cover, a honeycomb carrier, and a second mesh cover, all fixedly installed within the fixed frame and sequentially bonded together. The honeycomb pores of the honeycomb carrier are filled with a number of activated carbon particles and a number of aromatherapy particles. The aromatherapy particles consist of a particle body and a membrane layer covering the particle body. The membrane layer is formed by coating the surface of the particle body with a semi-degradable water-based coating at least twice and then drying it. The thickness of the membrane layer is 0.5-1.0 mm; in the honeycomb pores, activated carbon particles and aromatherapy particles are mixed in a weight ratio of 2:3-5. The semi-degradable water-based coating comprises the following raw materials in parts by weight: 40-50 parts of water-based acrylic resin 20-30 parts of waterborne polyurethane resin 10-15 parts of polylactic acid 8-10 parts of fumed silica Dispersant 0.8-1.5 parts Defoamer 0.1-0.3 parts 0.3-0.5 parts wetting agent Thickener 1-2 parts 2-3 parts of film-forming aid 5-10 parts of cosolvent 5-10 parts deionized water; The particle body comprises the following components in parts by weight: 60-70 parts of ethylene-vinyl acetate copolymer 30-40 parts perlite powder loaded with fragrance essential oils 1-3 parts of lubricating dispersant Colorant 1-3 parts.

2. The long-lasting fragrance air filter element according to claim 1, characterized in that: The density of the ethylene-vinyl acetate copolymer is 0.94-0.96 g / cm³. 3 The melting temperature is 45-66℃; the perlite micro powder loaded with fragrance essential oil is made by mixing fragrance essential oil and perlite micro powder in a weight ratio of 5-7:4-5.

3. The long-lasting fragrance air filter element according to claim 1, characterized in that: The lubricating dispersant is pentaerythritol stearate and / or carboxymethyl cellulose; the colorant is at least one of titanium dioxide, carbon black, mica powder, iron oxide yellow or iron oxide red.

4. The long-lasting fragrance air filter element according to claim 1, characterized in that: The preparation method of the granule body includes the following steps: ethylene-vinyl acetate copolymer, perlite micro powder loaded with fragrance essential oil, lubricant dispersant and colorant are mixed evenly according to weight parts, and then extruded and granulated by a twin-screw extruder to obtain the granule body; wherein, the processing temperatures of each section of the twin-screw extruder, starting from the feeding section, are 45-55℃, 55-65℃, 65-75℃, 65-80℃, and 60-75℃, respectively, the die head temperature is 60-75℃, the screw length-to-diameter ratio is 25:1, and the screw speed is 60-150 r / min.

5. The long-lasting fragrance air filter element according to claim 1, characterized in that: The waterborne acrylic resin is NeoCryI XK-540 or DB3618; the waterborne polyurethane resin is PU-3486 or H-34P; the polylactic acid has an average molecular weight of 30,000-50,000 and a molecular weight distribution between 10,000-60,000.

6. The long-lasting fragrance air filter element according to claim 1, characterized in that: The dispersant is BYK-190 or BYK192; the defoamer is BYK-028; the wetting agent is BASF WE3229 or TEGO WET280; the thickener is at least one of sodium carboxymethyl cellulose, propylene glycol alginate, or sodium carboxymethyl starch; the film-forming aid is dipropylene glycol butyl ether or diethylene glycol monobutyl ether; and the cosolvent is isopropanol and / or ethanol.

7. A method for preparing a long-lasting fragrance-type air filter element as described in any one of claims 1-6, characterized in that, Includes the following steps: (S1) The PET short fiber primary filter layer, meltblown PP layer, first mesh cover and honeycomb carrier are bonded together in sequence to form a multi-layer structure. Then the outer periphery of the multi-layer structure is bonded to the inner wall of the fixed frame to obtain the filter element semi-finished product. (S2) After filling the honeycomb cells of the honeycomb carrier with a number of activated carbon particles and a number of aroma particles, the second mesh cover is glued to the side of the honeycomb carrier away from the first mesh cover, and after sealing, a long-lasting fragrance air filter is obtained.

Citation Information

Patent Citations

  • Clot retrieval system

    EA033045B1

  • High-concentration polyolefin aromatic master batch and its preparation method

    CN102766294A

  • Honeycomb activated carbon filter and manufacturing method thereof

    CN108993025A

  • Aroma-enhancing and cooling particles for cigarettes as well as preparation method and application thereof

    CN112273717A