Separation membrane based on metal organic framework, preparation method of separation membrane and lithium extraction device
By using a metal organic frame separation membrane modified with functional coating in membrane separation technology, the problems of membrane stability and bond strength are solved, and efficient separation of lithium ions and the improvement of long-term consumption performance are achieved.
Patent Information
- Application Number
- CN202411032631.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-30
AI Technical Summary
During the magnesium-lithium separation process, existing membrane separation technology has problems such as membrane loss, membrane pollution, poor stability and high and low-price ion retention rate optimization. Especially, metal organic frame MOFs are unstable and difficult to process in actual applications, resulting in their Applications in separation membranes are limited.
Using a separation membrane based on a metal organic frame, the bond strength between the metal organic frame and the base film is improved by forming a functional coating on the surface of the base film, including bulk crosslinked polymer and metal organic frame, using polymers in oxygen-containing The acylation reaction and complexing treatment were carried out under conditions to form a stable metal organic framework structure.
It improves the service life and long-term use performance of the separation membrane, enhances the flux and selective permeability of lithium ions, and ensures efficient separation of lithium ions and the stability of the membrane.
Smart Images

Figure CN118925514A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of separation membranes, and in particular to a separation membrane based on a metal organic framework, a preparation method thereof, and a lithium extraction device. Background Art
[0002] Compared with the traditional lithium extraction process from salt lakes, membrane separation has the advantages of high efficiency, energy saving, environmental protection, small footprint and high operational flexibility. Among them, nanofiltration technology (NF) and electrodialysis technology (ED) are used for Li extraction from brine. + Forward Osmosis (FO), reverse osmosis (RO) and membrane distillation (MD) are used for the purification of Li + In practical applications, multi-process coupling technology is usually used to achieve higher magnesium-lithium separation requirements. At present, although membrane separation technology has a good prospect, it still has problems such as membrane loss, membrane pollution, poor stability and optimization of high and low valence ion retention rate.
[0003] MOFs separation membranes based on metal organic frameworks are widely used in magnesium-lithium separation due to their precise pore size, high porosity, unique pore structure and abundant molecular / ion-specific functional groups on the framework. Due to the instability and difficult processing of MOFs, their practical application in membrane materials is limited. They are generally composited with base membranes to prepare MOFs-based heterogeneous membranes. MOFs-based heterogeneous membranes are mainly divided into MOFs polycrystalline membranes formed by nucleation and growth of MOFs on substrates, MOFs polyamide membranes prepared by embedding MOFs in polyamide layers, and channel membranes.
[0004] In MOFs polycrystalline films, multiphase crystallization forms a continuous MOFs film, while homogeneous crystallization may produce film defects. Substrate modification is conducive to MOFs heterogeneous nucleation and promotes the formation of defect-free films. Xu (https: / / doi.org / 10.1016 / j.memsci.2021.119101) disclosed a MOFs heterogeneous nucleation polycrystalline film, first using tannic acid-Zn complex to modify the base film, and then adding ligand imidazole to make the Zn in the tannic acid-Zn complex 2+ Partially converted into metal organic framework ZIF (complex of Zn and imidazole); 2+ The partial conversion results in residual tannic acid in the membrane. Due to the low molecular weight and good water solubility of tannic acid, it is easy to migrate in the water body, resulting in unstable membrane flux. It also causes water pollution when precipitated, thereby causing microbial membrane pollution, which in turn leads to a decline in the long-term performance of the membrane.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a separation membrane based on a metal organic framework, a preparation method thereof and a lithium extraction device, aiming to improve the bonding strength between the metal organic framework and the base membrane in the separation membrane, thereby improving the service life and long-term performance of the membrane.
[0007] The present invention can be implemented like this:
[0008] In a first aspect, the present invention provides a metal organic framework-based separation membrane, wherein the metal organic framework-based separation membrane comprises a base membrane and a functional coating on the surface of the base membrane; the functional coating comprises a bulk cross-linked polymer and a metal organic framework.
[0009] In some embodiments of the present invention, the metal organic framework-based separation membrane comprises at least one of the following features:
[0010] Feature 1: The bulk cross-linked polymer is obtained by bulk cross-linking a polymer under oxygen-containing conditions, and the polymer is polyethyleneimine grafted with catechol;
[0011] Feature 2: The base film includes one of polysulfone, polyethersulfone, polyvinylidene fluoride, polypropylene, polyethylene, polyacrylonitrile, polyimide or polytetrafluoroethylene; preferably, the base film is one of polypropylene, polyethersulfone and polyvinylidene fluoride;
[0012] Feature 3: The metal ion of the metal organic framework is a zinc ion, and the ligand is an imidazole compound;
[0013] Feature 4: The functional coating covers both sides of the base film, and the thickness of the functional coating on one side is 80 to 150 nm;
[0014] Feature 5: The thickness of the base film is 90 to 150 μm;
[0015] Feature 6: The average pore size of the base film is 100-1000nm, preferably 400-800nm.
[0016] In some embodiments of the present invention, the metal organic framework-based separation membrane further comprises at least one of the following features:
[0017] Feature 7: The polymer is prepared by acylation reaction of polyethyleneimine and catechol monomer; the catechol monomer includes at least one of 3,4-dihydroxyphenylpropionic acid, 3,4-dihydroxyphenylbutyric acid, 3-(2,3-dihydroxyphenyl)propionic acid, α-methyl-3,4-dihydroxyphenylpropionic acid, and 5-(3,4-dihydroxyphenyl)pentanoic acid; preferably, the catechol monomer is 3,4-dihydroxyphenylpropionic acid;
[0018] Feature 8: The number average molecular weight of the polyethyleneimine is 600 to 10,000 g / mol; preferably, the number average molecular weight of the polyethyleneimine is 10,000 g / mol;
[0019] Feature 9: The amine value of the polyethyleneimine is 18 to 22 mmol / g;
[0020] Feature 10: The molar ratio of the amino group to the catechol group in the polymer is (2:3) to (5:1);
[0021] Feature 11: The imidazole compound includes at least one of benzimidazole, 2-methylimidazole, 4-methylimidazole, and 2-aminobenzimidazole.
[0022] In some embodiments of the present invention, the metal organic framework-based separation membrane further comprises at least one of the following features:
[0023] Feature 12: The lithium ion flux of the metal organic framework-based separation membrane during the first operation of 1 hour is not less than 0.3 mol·h -1 ·m -2 ;
[0024] Feature 13: The lithium ion permselectivity of the metal organic framework-based separation membrane is not less than 8.4;
[0025] Feature 14: The metal organic framework-based separation membrane has a lithium ion flux retention rate of not less than 95.4% after continuous operation for 24 hours.
[0026] In a second aspect, the present invention provides a method for preparing a separation membrane based on a metal organic framework, comprising the following steps:
[0027] Step 1: Polyethyleneimine and catechol monomer undergo acylation reaction to prepare a polymer;
[0028] Step 2: preparing a polymer solution and a zinc salt solution respectively, and applying the polymer solution and the zinc salt solution to the surface of the base film in sequence to form a complex coating modified base film;
[0029] Step 3: prepare a ligand solution, apply it to the surface of the complex coating-modified base membrane, and heat and dry it under oxygen-containing conditions to obtain a metal organic framework-based separation membrane.
[0030] In some embodiments of the present invention, step one includes at least one of the following features:
[0031] Feature 1: The acylation reaction is added with a catalyst 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride;
[0032] Feature 2: The acylation reaction uses water and / or alcohol as solvent;
[0033] Feature 3: The acylation reaction is carried out in an acidic environment;
[0034] Feature 4: The ratio of the molar amount of the catechol monomer to the total molar amount of the primary amine and the secondary amine in the polyethyleneimine is 0.2 to 0.6:1.
[0035] In some embodiments of the present invention, the step 2 includes at least one of the following features:
[0036] Feature 5: The mass percentage concentration of the polymer solution is 2% to 6%;
[0037] Feature 6: The mass percentage concentration of the zinc salt solution is 0.5% to 1.5%;
[0038] Feature 7: The zinc salt includes at least one of zinc acetate, zinc chloride and zinc nitrate;
[0039] Feature 8: The complex coating covers both sides of the base film, and the thickness of the complex coating on one side of the base film modified by the complex coating is 80 to 160 nm.
[0040] In some embodiments of the present invention, the step three includes at least one of the following features:
[0041] Feature 9: The ligand includes at least one of benzimidazole, 2-methylimidazole, 4-methylimidazole, and 2-aminobenzimidazole;
[0042] Feature 10: The molar concentration of the ligand solution is 2 to 4 M;
[0043] Feature 11: The solvent of the ligand solution includes one of ethanol, methanol and water.
[0044] In some embodiments of the present invention, heating and drying under oxygen-containing conditions is heating and drying under air purge.
[0045] In a third aspect, the present invention provides a lithium extraction device, comprising the metal organic framework-based separation membrane described in the first aspect or the metal organic framework-based separation membrane prepared by the preparation method of the second aspect.
[0046] The beneficial effects of the present invention include:
[0047] The metal organic framework-based separation membrane provided by the present invention contains a functional coating including a bulk cross-linked polymer and a metal organic framework. The bulk cross-linked polymer can improve the bonding strength between the metal organic framework and the base membrane in the separation membrane, thereby improving the service life and long-term performance of the membrane. The metal organic framework-based separation membrane prepared by the preparation method provided by the present invention has good ion flux and lithium selective permeability. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0049] Figure 1 XRD patterns of the metal organic framework-based separation membrane (1), the complex coating modified base membrane (2), ZIF-8, and polypropylene (PP) prepared in Example 1;
[0050] Figure 2 The cross-sectional SEM images of the metal organic framework-based separation membrane (c), the complex coating modified base membrane (b) and the polypropylene base membrane (a) prepared in Example 1;
[0051] Figure 3 It is a lithium extraction device. DETAILED DESCRIPTION
[0052] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0053] The metal organic framework-based separation membrane and its preparation method and lithium extraction device provided by the present invention are described in detail below.
[0054] The present invention provides a separation membrane based on a metal organic framework, which comprises a base membrane and a functional coating on the surface of the base membrane; the functional coating comprises a bulk cross-linked polymer and a metal organic framework.
[0055] The metal organic framework-based separation membrane provided by the present invention contains a functional coating including a bulk cross-linked polymer and a metal organic framework. The bulk cross-linked polymer can improve the bonding strength between the metal organic framework and the base membrane in the separation membrane, thereby improving the service life and long-term performance of the membrane.
[0056] The above-mentioned bulk cross-linked polymer is obtained by bulk cross-linking of the polymer under oxygen-containing conditions, that is, under natural air conditions, the polymer can undergo cross-linking between polymer molecules and / or within the molecules without the need for additional treatment, and there is no need to add a cross-linking agent. Compared with linear polymer adhesives, bulk cross-linkable polymers can increase the bonding strength between the metal organic framework and the base membrane in the separation membrane, thereby increasing the service life and long-term performance of the membrane.
[0057] In some embodiments of the present invention, the polymer in the bulk cross-linked polymer is polyethyleneimine grafted with catechol, which is prepared by acylation reaction of polyethyleneimine and catechol monomers.
[0058] In some optional embodiments, the catechol monomer includes at least one of 3,4-dihydroxyphenylpropionic acid, 3,4-dihydroxyphenylbutyric acid, 3-(2,3-dihydroxyphenyl)propionic acid, α-methyl-3,4-dihydroxyphenylpropionic acid, and 5-(3,4-dihydroxyphenyl)pentanoic acid; the alkyl chain length in the catechol monomer affects the water solubility of the polymer, and the position of the phenolic hydroxyl group in the catechol monomer affects the acylation reaction rate, thereby affecting the grafting rate and cross-linking density, and ultimately affecting the bonding strength between the metal organic framework and the base membrane in the separation membrane; 3,4-dihydroxyphenylpropionic acid is a preferred embodiment of the present invention.
[0059] In some optional embodiments, the number average molecular weight of the polyethyleneimine is 600-10000 g / mol; the number average molecular weight of polyethyleneimine affects the bonding strength of the formed bulk cross-linked polymer. The larger the molecular weight, the more entanglements between molecules and the stronger the bonding strength. However, an excessively large molecular weight causes the polymer to have a high viscosity and is difficult to process, and has poor dispersibility on the base film. Preferably, the number average molecular weight of the polyethyleneimine is 10000 g / mol.
[0060] In some optional embodiments, the amine value of the polyethyleneimine is 18 to 22 mmol / g; the amine value of the polyethyleneimine affects the grafting rate of the catechol group in the polymer and the bulk crosslinking density, and ultimately affects the bonding strength between the metal organic framework and the base membrane in the separation membrane.
[0061] In some optional embodiments, the molar ratio of the amino group to the catechol group in the polymer is (2:3) to (5:1); the bulk crosslinking described in the present invention refers to the chemical reaction of the phenolic hydroxyl group and the amino group according to the following formula I or / and formula II to achieve crosslinking. It can be seen that the ratio of the two affects the bulk crosslinking degree of the polymer, thereby affecting the bonding strength, hardness and lithium separation selectivity between the metal organic framework and the base membrane in the separation membrane.
[0062] Formula I:
[0063]
[0064] Formula II:
[0065]
[0066] In some embodiments of the present invention, the base membrane includes one of polysulfone, polyethersulfone, polyvinylidene fluoride, polypropylene, polyethylene, polyacrylonitrile, polyimide or polytetrafluoroethylene; the type, thickness and pore size of the base membrane have an impact on the ion flux, lithium selective permeability and durability of the separation membrane; preferably, the base membrane is one of polypropylene, polyethersulfone and polyvinylidene fluoride.
[0067] In some optional embodiments, the base film has a thickness of 90 to 150 μm.
[0068] In some optional embodiments, the average pore size of the base membrane is 100-1000 nm, preferably 400-800 nm.
[0069] In some embodiments of the present invention, the metal ion of the metal organic framework is a zinc ion, and the ligand is an imidazole compound; the imidazole compound includes at least one of benzimidazole, 2-methylimidazole, 4-methylimidazole, and 2-aminobenzimidazole.
[0070] In some embodiments of the present invention, the functional coating covers the outer surfaces on both sides of the base membrane, and the two sides refer to the two planes with the largest area formed by the length direction and the width direction of the membrane; the single-side thickness of the functional coating is 80 to 150 nm; the thickness will affect the ion flux and lithium selective permeability of the separation membrane.
[0071] In some embodiments of the present invention, the lithium ion flux of the metal organic framework-based separation membrane during the first operation for 1 h is not less than 0.3 mol·h -1 ·m -2 .
[0072] In some embodiments of the present invention, the lithium ion permselectivity of the metal organic framework-based separation membrane is not less than 8.4.
[0073] In some embodiments of the present invention, the metal organic framework-based separation membrane has a lithium ion flux retention rate of not less than 95.4% after continuous operation for 24 hours.
[0074] The present invention provides a method for preparing a separation membrane based on a metal organic framework, comprising the following steps:
[0075] Step 1: Polyethyleneimine and catechol monomer undergo acylation reaction to prepare a polymer;
[0076] Step 2: preparing a polymer solution and a zinc salt solution respectively, and applying the polymer solution and the zinc salt solution to the surface of the base film in sequence to form a complex coating modified base film;
[0077] Step 3: prepare a ligand solution, apply it to the surface of the complex coating-modified base membrane, and heat and dry it under oxygen-containing conditions to obtain a metal organic framework-based separation membrane.
[0078] The polymer provided by the present invention is grafted with catechol groups, which are beneficial to Zn 2+ The polymer is first applied to the surface of the base film, and then Zn 2+ , so that Zn 2+ Due to the complexation, it is fixed on the surface of the basement membrane; when the ligand is added, due to the ligand and Zn 2+ The coordination effect is stronger and can form an orderly arrangement, so that Zn 2+ It is converted into the metal center of the metal organic framework, forming metal organic framework crystals with separation activity on the surface of the base membrane; and the polymer undergoes bulk cross-linking when subsequently heated and dried under oxygen-containing conditions, thereby converting into an adhesive between the metal organic framework and the base membrane. This bonding method greatly improves the bonding strength between the two, thereby improving the service life and long-term performance of the membrane.
[0079] In some embodiments of the present invention, the step 1 specifically includes the following steps: dissolving polyethyleneimine in a solvent, then adding acid to adjust the pH value, adding catechol monomer and catalyst, stirring at room temperature to carry out acylation reaction, and obtaining a polymer after purification and drying.
[0080] In some optional embodiments, the catalyst is 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride.
[0081] In some optional embodiments, the solvent is water and / or alcohol.
[0082] In some optional embodiments, the pH value is 4-6; and the acid is selected from at least one of hydrochloric acid, acetic acid, sulfuric acid, and nitric acid.
[0083] In some optional embodiments, the ratio of the molar amount of the catechol monomer to the total molar amount of the primary and secondary amines in polyethyleneimine is 0.2 to 0.6: 1. The molar ratio of the catechol monomer to the amine group will affect the grafting ratio of the catechol group on the polyethyleneimine. On the one hand, the more catechol groups there are, the more active sites there are for coordination with zinc ions, and thus the more amount of subsequent conversion into a metal organic framework, thereby improving the lithium ion permselectivity; on the other hand, due to the subsequent bulk cross-linking reaction between the catechol group and the amine group, the excessive amount of the catechol group leads to a smaller amount of the remaining amine group in the polymer, which in turn affects the cross-linking density of the subsequent polymer, thereby affecting the bonding strength and the lithium ion permselectivity.
[0084] The purpose of step 2 of the present invention is to form a uniform complex coating on the surface of the base film. Therefore, there is no limitation on the method of applying the polymer solution and the zinc salt solution to the surface of the base film, which specifically includes but is not limited to: soaking, spraying, scraping, pouring, etc.
[0085] In some embodiments of the present invention, the step 2 specifically includes the following steps: prepare a polymer solution and a zinc salt solution respectively, first immerse the base film in the polymer solution, let it stand for a first time and then take it out; then immerse it in a zinc salt solution, let it stand for a second time and then take it out; rinse with water and dry, repeat the above steps until the target thickness is reached to obtain a complex coating modified base film.
[0086] In some optional embodiments, the mass percentage concentration of the polymer solution is 2% to 6%.
[0087] In some optional embodiments, the mass percentage concentration of the zinc salt solution is 0.5% to 1.5%.
[0088] In some optional embodiments, the zinc salt includes at least one of zinc acetate, zinc chloride, and zinc nitrate.
[0089] In some optional embodiments, the target thickness refers to the thickness of the complex coating on one side of the base film surface, and the target thickness is 80 to 160 nm.
[0090] In some optional embodiments, the first standing time is 5 to 10 minutes; the second standing time is 8 to 12 minutes.
[0091] The purpose of step three of the present invention is to uniformly apply the ligand on the surface of the complex coating modified base film, so there is no limitation on the method of applying the ligand solution on the surface of the base film, including but not limited to: soaking, spraying, scraping, pouring, etc.
[0092] In some embodiments of the present invention, the step three specifically includes the following steps: dissolving the ligand in a solvent to form a ligand solution, immersing the modified base membrane in the above ligand solution, taking it out after a third standing and rinsing it with water, and obtaining a separation membrane after air blowing and heating and drying.
[0093] In some optional embodiments, the ligand is an imidazole compound; the imidazole compound includes at least one of benzimidazole, 2-methylimidazole, 4-methylimidazole, and 2-aminobenzimidazole.
[0094] In some optional embodiments, the molar concentration of the ligand solution is 2-4M.
[0095] In some optional embodiments, the solvent of the ligand solution includes one of ethanol, methanol and water.
[0096] In some optional embodiments, the third standing time is 30 to 60 minutes.
[0097] In some optional modes, the drying under air blowing and heating refers to drying in a blower box at 60 to 80° C. for 12 to 24 hours.
[0098] In addition, the present invention also provides a lithium extraction device, comprising the metal organic framework-based separation membrane of any one of the aforementioned embodiments.
[0099] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0100] Example 1
[0101] This embodiment provides a separation membrane based on a metal organic framework, and the preparation method is as follows:
[0102] (1) Preparation of polymer
[0103] Weigh polyethyleneimine (PEI) and dissolve it in deionized water. Add hydrochloric acid to adjust the pH to 5, then add 3,4-dihydroxyphenylpropionic acid and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC), stir at room temperature for 6 hours to carry out acylation reaction, and after the reaction is completed, dialysis purification is carried out, and then the polymer is obtained after drying at 120°C.
[0104] The number average molecular weight of the PEI is 10000 g / mol, and the amine value is 18 mmol / g.
[0105] The ratio of the molar amount of the 3,4-dihydroxyphenylpropionic acid to the total molar amount of the primary amine and the secondary amine in PEI is 0.4:1.
[0106] The molar amount of the EDC fed is twice the molar amount of the catechol monomer.
[0107] The proton peaks of the H-NMR spectrum of the prepared polymer are as follows, and the solvent is D2O:
[0108] 1 H-NMR (400MHz, D2O), (ppm): 2.42 (t, Ar-CH2), 2.4 (t, O=C-CH2), 2.69 (m, PEI-CH2), 6.55 (d, Ar-H), 6.67 (s, Ar-H), 6.72 (d, Ar-H), 8.22 (s, O=C-NH), 9.58 (s, Ar-OH). Since the amide hydrogen proton peak can be observed in the H-NMR spectrum, it indicates that the catechol group is successfully grafted onto polyethyleneimine. Through the peak area analysis of the proton peak in the H-NMR spectrum, the molar ratio of the amine group (primary amine and secondary amine) to the catechol group in the polymer can be obtained, which is 5:1.5.
[0109] (2) Complex coating modified base film
[0110] The polymer was dissolved in deionized water to obtain a polymer solution with a concentration of 4wt%, and zinc acetate was dissolved in deionized water to obtain a zinc salt solution with a concentration of 1wt%. First, the polypropylene base film was immersed in the polymer solution and allowed to stand for 5 minutes. After being taken out, it was immersed in the zinc salt solution and allowed to stand for 10 minutes. Then, it was taken out, rinsed with deionized water 5 times, and dried by nitrogen purge. The above steps were repeated until the complex coating on the surface of the single-side base film reached the target thickness of 160nm, thereby obtaining a complex coating modified base film.
[0111] The thickness of the polypropylene-based membrane was 120 μm and the average pore size was 600 nm.
[0112] (3) Preparation of separation membranes based on metal organic frameworks
[0113] Benzimidazole was dissolved in ethanol to form a ligand solution with a concentration of 3 M. The complex coating modified base membrane was immersed in the above ligand solution, and after standing for 45 minutes, it was taken out and rinsed with deionized water for 3 times, and dried in a 60°C forced air oven for 12 hours to obtain a separation membrane based on a metal organic framework.
[0114] Example 2
[0115] The difference from Example 1 is that the ratio of the molar amount of the 3,4-dihydroxyphenylpropionic acid fed in step (1) to the total molar amount of the primary amine and the secondary amine in PEI is 0.2:1.
[0116] The molar ratio of amine groups (primary and secondary amines) to catechol groups in the polymer is 5:1.
[0117] Example 3
[0118] The difference from Example 1 is that the ratio of the molar amount of the 3,4-dihydroxyphenylpropionic acid fed in step (1) to the total molar amount of the primary amine and the secondary amine in PEI is 0.6:1.
[0119] The molar ratio of amine groups (primary and secondary amines) to catechol groups in the polymer is 5:2.6.
[0120] Example 4
[0121] The difference from Example 1 is that the target thickness in step (2) is 80 nm.
[0122] Example 5
[0123] The difference from Example 1 is that the target thickness in step (2) is 120 nm.
[0124] Example 6
[0125] The difference from Example 1 is that in step (3), an aqueous solution of 2-methylimidazole is used as the ligand solution instead of an ethanol solution of benzimidazole.
[0126] Example 7
[0127] This embodiment provides a separation membrane based on a metal organic framework, and the preparation method is as follows:
[0128] (1) Preparation of polymer
[0129] Weigh polyethyleneimine (PEI) and dissolve it in deionized water. Add hydrochloric acid to adjust the pH to 4, then add 3,4-dihydroxyphenylbutyric acid and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC), stir at room temperature for 6 hours to carry out acylation reaction, and after the reaction is completed, dialysis purification is carried out, and then the polymer is obtained after drying at 120°C.
[0130] The number average molecular weight of the PEI is 600 g / mol, and the amine value is 20 mmol / g.
[0131] The ratio of the molar amount of the 3,4-dihydroxyphenylbutyric acid to the total molar amount of the primary amine and the secondary amine in PEI is 0.4:1.
[0132] The molar amount of the EDC fed is twice the molar amount of the catechol monomer.
[0133] The molar ratio of amine groups (primary and secondary amines) to catechol groups in the polymer is 5:1.3.
[0134] (2) Complex coating modified base film
[0135] The polymer was dissolved in deionized water to obtain a polymer solution with a concentration of 6wt%, and zinc chloride was dissolved in deionized water to obtain a zinc salt solution with a concentration of 0.5wt%. The polyethersulfone base membrane was first immersed in the polymer solution and allowed to stand for 8 minutes. After being taken out, it was immersed in the zinc salt solution and allowed to stand for another 8 minutes. Then, it was taken out, rinsed with deionized water 5 times, and dried by nitrogen purge. The above steps were repeated until the complex coating reached the target thickness of 160nm on one side of the base membrane surface to obtain a complex coating modified base membrane.
[0136] The thickness of the polyethersulfone-based membrane is 150 μm and the average pore size is 1000 nm.
[0137] (3) Preparation of separation membranes based on metal organic frameworks
[0138] 4-Methylimidazole was dissolved in deionized water to form a ligand solution with a concentration of 2M. The complex coating modified base membrane was immersed in the above ligand solution, and after standing for 30 minutes, it was taken out and rinsed with deionized water for 3 times, and dried in a forced air oven at 80°C for 12 hours to obtain a separation membrane based on a metal organic framework.
[0139] Example 8
[0140] This embodiment provides a separation membrane based on a metal organic framework, and the preparation method is as follows:
[0141] (1) Preparation of polymer
[0142] Weigh polyethyleneimine (PEI) and dissolve it in deionized water. Add hydrochloric acid to adjust the pH to 6, then add 5-(3,4-dihydroxyphenyl)pentanoic acid and 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (EDC), stir at room temperature for 6 hours to carry out acylation reaction, and after the reaction is completed, dialysis purification is carried out, and then the polymer is obtained after drying at 120°C.
[0143] The number average molecular weight of the PEI is 1800 g / mol, and the amine value is 19 mmol / g.
[0144] The ratio of the molar amount of the 5-(3,4-dihydroxyphenyl)pentanoic acid to the total molar amount of the primary amine and the secondary amine in PEI is 0.4:1.
[0145] The molar amount of the EDC fed is twice the molar amount of the catechol monomer.
[0146] The molar ratio of amine groups (primary and secondary amines) to catechol groups in the polymer is 5:1.
[0147] (2) Complex coating modified base film
[0148] The polymer was dissolved in deionized water to obtain a polymer solution with a concentration of 2wt%, and zinc nitrate was dissolved in deionized water to obtain a zinc salt solution with a concentration of 1.5wt%. First, the polyvinylidene fluoride based membrane was immersed in the polymer solution and allowed to stand for 10 minutes. After being taken out, it was immersed in the zinc salt solution and allowed to stand for 12 minutes. Then, it was taken out, rinsed with deionized water 5 times, and dried by nitrogen purge. The above steps were repeated until the complex coating reached the target thickness of 160nm on one side of the base film surface to obtain a complex coating modified base film.
[0149] The thickness of the polyvinylidene fluoride based membrane is 90 μm and the average pore size is 400 nm.
[0150] (3) Preparation of separation membranes based on metal organic frameworks
[0151] 2-Aminobenzimidazole was dissolved in ethanol to form a ligand solution with a concentration of 4 M. The complex coating modified base membrane was immersed in the above ligand solution, and after standing for 60 minutes, it was taken out and rinsed with deionized water for 3 times, and dried in a 60°C forced air oven for 24 hours to obtain a separation membrane based on a metal organic framework.
[0152] Comparative Example 1
[0153] The difference from Example 1 is that in step (2), the aqueous solution of tannic acid is used instead of the aqueous solution of the polymer.
[0154] Comparative Example 2
[0155] This comparative example prepares a separation membrane, and the preparation method is as follows:
[0156] A polypropylene-based membrane (thickness of 120 μm, average pore size of 600 nm) was placed at the bottom of the mold, and then the precursor solution was poured. After standing at room temperature for 24 hours, the membrane was taken out and rinsed with deionized water 5 times and dried to obtain a separation membrane. The precursor solution refers to an aqueous solution containing 2.7 mg / mL zinc acetate and 57 mg / mL 2-methylimidazole. The ratio of the area of the polypropylene-based membrane to the volume of the precursor solution is 1 cm 2 :0.5mL.
[0157] Comparative Example 3
[0158] The difference from Example 1 is that the ratio of the molar amount of 3,4-dihydroxyphenylpropionic acid in step (1) to the total molar amount of primary amines and secondary amines in PEI is 0.1:1.
[0159] The molar ratio of amine groups (primary and secondary amines) to catechol groups in the polymer is 10:1.
[0160] Comparative Example 4
[0161] The difference from Example 1 is that the ratio of the molar amount of 3,4-dihydroxyphenylpropionic acid in step (1) to the total molar amount of primary amines and secondary amines in PEI is 0.7:1.
[0162] The molar ratio of amine groups (primary and secondary amines) to catechol groups in the polymer is 5:3.2.
[0163] Test example
[0164] (1) The metal organic framework-based separation membrane (1) and the complex coating modified base membrane (2) prepared in Example 1 were characterized by X-ray diffraction. The obtained XRD pattern is as follows: Figure 1 shown.
[0165] Depend on Figure 1 It can be seen that the XRD spectra of the metal-organic framework-based separation membranes include the diffraction peaks of the pure metal-organic framework (ZIF-8) and the inclusion peaks of the polypropylene base membrane (PP), indicating that the metal-organic framework is successfully grown on the base membrane.
[0166] (2) The metal organic framework-based separation membrane (c), the complex coating modified base membrane (b), and the polypropylene base membrane (a) prepared in Example 1 were observed by scanning electron microscopy. The obtained SEM images are as follows: Figure 2 shown.
[0167] contrast Figure 2 As can be seen from (a) and (b), the complex coating successfully modified the base film; by comparing (b) and (c), it can be seen that crystals grew on the surface of the film and the roughness increased significantly; and the thickness of the polymer layer became smaller, indicating that the polymer underwent bulk polymerization.
[0168] (3) The separation membranes prepared in the examples and comparative examples were tested for lithium extraction performance. The separation membranes were assembled into an electrodialysis lithium extraction device, and the ion flux (J) and lithium ion permselectivity (P) were tested.
[0169] Electrodialysis lithium extraction device as attached Figure 3 As shown, it consists of a polarization chamber (including a cathode polarization chamber and an anode polarization chamber), a concentration chamber and a desalination chamber, wherein the electrodes are titanium electrodes coated with ruthenium oxide. The polarization chamber is filled with a 0.3M sodium sulfate solution, and the desalination chamber is filled with a Li+ solution with a metal ion concentration of 0.1M. + and Mg 2+ The concentration chamber is a 0.01 M KCl solution; the electrodialysis membrane group consists of CEM (AMX, purchased from Asahi Kasei Corporation, Japan), the sample membrane to be tested, and CEM. The volume of the solution in each compartment is 100 mL, the pump flow rate is 20 mL / min, and the constant current mode is adopted to determine the Li in the concentration chamber by ICP-OES. + Mg 2+The concentration of ions was calculated and the ion flux J and lithium ion selectivity P were calculated according to the following formula:
[0170]
[0171] Where J is the ion flux (mol·h -1 ·m -2 ), C0 and C t are the ion concentrations in the concentration chamber at time 0 and time t (mol / L), V is the liquid volume in the concentration chamber of the device (L), and A is the effective area of the membrane (m 2 ).
[0172]
[0173] Where P is the lithium ion selectivity, J Li and J Mg are the ion fluxes of lithium ions and magnesium ions at time t, respectively, Mg and C Li are the concentrations of lithium ions and magnesium ions in the desalination chamber at time t, respectively.
[0174] Table 1 shows the lithium ion flux (J) after the first operation for 1 h (i.e., t = 1 h). Li ) and lithium ion permselectivity (P) as well as the lithium ion flux after 24 h of continuous operation (i.e., t = 24 h) relative to J after the first operation for 1 h Li Retention rate.
[0175] Table 1
[0176]
[0177] As can be seen from Table 1, the separation membrane based on the metal organic framework prepared in the embodiment of the present invention has better long-term use performance and lithium selective permeability than the comparative example. Specifically, comparative example 1 uses tannic acid as the complexing ligand. Since tannic acid has a small molecular weight and cannot undergo bulk cross-linking, it has almost no adhesion and will dissolve into the water body during use, causing water pollution, so its long-term use performance is poor; By comparing Examples 1 to 3 and Comparative Examples 3 to 4, it can be seen that the grafting ratio of catechol groups in the polymer has a significant effect on the performance of the separation membrane. As the grafting ratio increases, the J of the separation membrane increases. LiThe retention rate and P both increase first and then decrease. The reasons are as follows: on the one hand, the more the grafting ratio of catechol groups is, the more active sites are coordinated with zinc ions, and thus the more amount is subsequently converted into metal organic frameworks, resulting in a decrease in ion permeability; on the other hand, the catechol groups are grafted to the PEI side chains through the acylation reaction between catechol monomers and the amino groups on the PEI chain. Therefore, the more the grafting ratio of catechol groups is, the fewer the remaining amino groups are; the ratio of catechol groups to amino groups affects the degree of bulk cross-linking reaction between the two. The higher the degree of cross-linking reaction, the greater the bonding strength. The long-term performance shows a trend of increasing first and then decreasing. The reason for the decrease is that the excessive degree of cross-linking leads to a lower pore size, which is easy to cause blockage; similarly, the pore size decreases with the increase of the degree of cross-linking of the polymer bulk, so the selective permeability to lithium increases first and then decreases. Too low a pore size leads to too low a lithium ion flux, so the selective permeability to lithium deteriorates. Comparative Example 2 has a higher lithium ion flux than Example 1, but its long-term performance is poor and the lithium ion selectivity is low. The reason is that there is no cross-linked polymer as a bonding medium between the metal organic framework and the base membrane on the membrane prepared in Comparative Example 2, resulting in low bonding strength of the metal organic framework, which is easy to fall off during use, resulting in poor long-term performance. In addition, due to the metal organic framework cannot be evenly dispersed and fully covered on the surface of the base membrane under this preparation method, the local pore size is too large, resulting in low lithium selectivity.
[0178] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A separation membrane based on a metal organic framework, characterized in that: The metal organic framework-based separation membrane comprises a base membrane and a functional coating on the surface of the base membrane; the functional coating comprises a bulk cross-linked polymer and a metal organic framework.
2. The metal organic framework-based separation membrane according to claim 1, characterized in that: The metal organic framework-based separation membrane comprises at least one of the following features: Feature 1: The bulk cross-linked polymer is obtained by bulk cross-linking a polymer under oxygen-containing conditions, and the polymer is polyethyleneimine grafted with catechol; Feature 2: The base film includes one of polysulfone, polyethersulfone, polyvinylidene fluoride, polypropylene, polyethylene, polyacrylonitrile, polyimide or polytetrafluoroethylene; Feature 3: The metal ion of the metal organic framework is a zinc ion, and the ligand is an imidazole compound; Feature 4: The functional coating covers both sides of the base film, and the thickness of the functional coating on one side is 80 to 150 nm; Feature 5: The thickness of the base film is 90 to 150 μm; Feature 6: The average pore size of the base membrane is 100 to 1000 nm.
3. The metal organic framework-based separation membrane according to claim 2, characterized in that: The metal organic framework-based separation membrane further comprises at least one of the following features: Feature 7: The polymer is prepared by acylation reaction of polyethyleneimine and catechol monomer; the catechol monomer includes at least one of 3,4-dihydroxyphenylpropionic acid, 3,4-dihydroxyphenylbutyric acid, 3-(2,3-dihydroxyphenyl)propionic acid, α-methyl-3,4-dihydroxyphenylpropionic acid, and 5-(3,4-dihydroxyphenyl)pentanoic acid; Feature 8: The number average molecular weight of the polyethyleneimine is 600 to 10000 g / mol; Feature 9: The amine value of the polyethyleneimine is 18 to 22 mmol / g; Feature 10: The molar ratio of the amino group to the catechol group in the polymer is (2:3) to (5:1); Feature 11: The imidazole compound includes at least one of benzimidazole, 2-methylimidazole, 4-methylimidazole, and 2-aminobenzimidazole.
4. The metal organic framework-based separation membrane according to any one of claims 1 to 3, characterized in that: The metal organic framework-based separation membrane further comprises at least one of the following features: Feature 12: The lithium ion flux of the metal organic framework-based separation membrane during the first operation of 1 hour is not less than 0.3 mol·h -1 ·m -2 ; Feature 13: The lithium ion permselectivity of the metal organic framework-based separation membrane is not less than 8.4; Feature 14: The metal organic framework-based separation membrane has a lithium ion flux retention rate of not less than 95.4% after continuous operation for 24 hours.
5. A method for preparing a separation membrane based on a metal organic framework according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: Polyethyleneimine and catechol monomer undergo acylation reaction to prepare a polymer; Step 2: preparing a polymer solution and a zinc salt solution respectively, and applying the polymer solution and the zinc salt solution to the surface of the base film in sequence to form a complex coating modified base film; Step 3: prepare a ligand solution, apply it to the surface of the complex coating-modified base membrane, and heat and dry it under oxygen-containing conditions to obtain a metal organic framework-based separation membrane.
6. The preparation method according to claim 5, characterized in that: The step 1 includes at least one of the following features: Feature 1: The acylation reaction is added with a catalyst 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride; Feature 2: The acylation reaction uses water and / or alcohol as solvent; Feature 3: The acylation reaction is carried out in an acidic environment; Feature 4: The ratio of the molar amount of the catechol monomer to the total molar amount of the primary amine and the secondary amine in the polyethyleneimine is 0.2 to 0.6:
1.
7. The preparation method according to claim 5, characterized in that: The step 2 includes at least one of the following features: Feature 5: The mass percentage concentration of the polymer solution is 2% to 6%; Feature 6: The mass percentage concentration of the zinc salt solution is 0.5% to 1.5%; Feature 7: The zinc salt includes at least one of zinc acetate, zinc chloride and zinc nitrate; Feature 8: The complex coating covers both sides of the base film, and the thickness of the complex coating on one side of the base film modified by the complex coating is 80 to 160 nm.
8. The preparation method according to claim 5, characterized in that: The step three includes at least one of the following features: Feature 9: The ligand includes at least one of benzimidazole, 2-methylimidazole, 4-methylimidazole, and 2-aminobenzimidazole; Feature 10: The molar concentration of the ligand solution is 2 to 4 M; Feature 11: The solvent of the ligand solution includes one of ethanol, methanol and water.
9. The preparation method according to claim 5, characterized in that: The heating and drying under oxygen-containing conditions is heating and drying under air purge.
10. A lithium extraction device, characterized in that: The invention comprises a metal organic framework-based separation membrane as claimed in any one of claims 1 to 4 or a metal organic framework-based separation membrane prepared by the preparation method as claimed in any one of claims 5 to 9.
Citation Information
Patent Citations
Charged nanofiltration membrane based on polymer nanoparticles and preparation method thereof
CN113908703A
Metal-organic framework material separation membrane as well as preparation method and application thereof
CN116474573A
Organic / inorganic MOF (Metal Organic Framework) hybrid mixed matrix membrane with high separation performance as well as preparation method and application of organic / inorganic MOF hybrid mixed matrix membrane
CN116808848A
Modified metal organic framework, gas separation membrane as well as preparation method and application of modified metal organic framework and gas separation membrane
CN118001947A