Coated oil field operating assemblies and methods for protecting and extending the liferage
By applying a coating composition of trifunctional silane and silanol fluids to oilfield operating components, the wear problem caused by high flow rates and corrosive fluids was solved, resulting in improved wear resistance and extended service life of the components.
Patent Information
- Application Number
- CN202410987512.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-04-08
- Filing Date
- 2021-04-09
- Publication Date
- 2024-11-12
AI Technical Summary
Oilfield operating components experience high wear rates due to high flow rates, high pressures, and corrosive fluids, resulting in shortened service life and increased maintenance costs.
A coating composition comprising trifunctional silanes, silanol fluids, and fillers is used to form a coating layer with the primer layer through chemical bonding, thereby absorbing and dissipating energy in the fluid flow and protecting components from wear.
It significantly reduces the wear rate of oilfield operating components, extends their service life, and reduces maintenance frequency and costs.
Smart Images

Figure CN118926066A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application is a divisional application of the Chinese invention patent application with application number 202180040303.4, application date April 9, 2021, and invention name “Coated oilfield operating components and methods for protecting and extending the service life of oilfield operating components”. The original application is the national phase application PCT / US2021 / 070365, and the PCT application claims the following priority and rights: U.S. Provisional Application No. 63 / 008,035, entitled “COATING COMPOSITIONS, COATED OILFIELD OPERATIONAL COMPONENTS, AND RELATED METHODS FOR OILFIELD OPERATIONS” filed on April 10, 2020; U.S. Provisional Application No. 63 / 008,035, entitled “COATING COMPOSITIONS, COATED OILFIELD OPERATIONAL COMPONENTS, AND RELATED METHODS FOR OILFIELD OPERATIONS” filed on April 10, 2020; U.S. Provisional Application No. 63 / 008,035, entitled “METHODS FOR PROTECTING OILFIELD OPERATIONAL COMPONENTS, AND RELATED METHODS FOR OILFIELD OPERATIONS” filed on April 10, 2020 U.S. Provisional Application No. 63 / 008,038, filed on April 10, 2020, entitled “COATING AND METHODS FOR EXTENDING SERVICE LIFE OF OILFIELDOPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 008,042, filed on April 10, 2020, entitled “METHODS FOR PREPARING COATING COMPOSITIONS FOR PROTECTING OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 008,046, filed on April 10, 2020, entitled “METHODS FOR PROVIDING FLEXIBLE AND / OR ELASTIC COATINGS ON OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 008,050, filed on April 10, 2020, entitled “METHODS FOR PROVIDING FLEXIBLE AND / OR ELASTIC COATINGS ON OILFIELD OPERATIONAL COMPONENTS” ELASTIC COATINGS ONOILFIELD OPERATIONAL COMPONENTS);U.S. Provisional Application No. 63 / 065,542, filed on August 14, 2020, entitled “COATED OILFIELD OPERATIONAL COMPONENTS AND METHODS FOR PROTECTING AND EXTENDING THE SERVICE LIFE OF OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 065,545, filed on August 14, 2020, entitled “METHODS FOR PROTECTING OILFIELD OPERATIONAL COMPONENTS FROM DAMAGE FROM FLUID Flow”; U.S. Provisional Application No. 63 / 065,545, filed on August 14, 2020, entitled “COATING AND METHODS FOR EXTENDING SERVICE LIFE OF OILFIELD OPERATIONAL COMPONENTS U.S. Provisional Application No. 63 / 065,565, filed on August 14, 2020, entitled “METHODS FOR PREPARING COATING COMPOSITIONS FOR PROTECTING OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 065,577, filed on August 14, 2020, entitled “METHODS FOR PROVIDING FLEXIBLE AND / OR ELASTIC COATINGS ON OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 065,591, filed on August 14, 2020, entitled “METHODS FOR PROVIDING FLEXIBLE AND / OR ELASTIC COATINGS ON OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 065,592, filed on August 14, 2020, entitled “METHODS FOR PROVIDING FLEXIBLE AND / OR ELASTIC COATINGS ON OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 065,593, filed on September 25, 2020, entitled “COATED OILFIELD OPERATIONAL COMPONENTS AND METHODS FOR PROTECTING AND EXTENDING THE SERVICE OF OILFIELD OPERATIONAL COMPONENTS” METHODS FOR PROTECTING AND EXTENDING THE SERVICE LIFE OF OILFIELD OPERATIONAL COMPONENTS);and U.S. Non-Provisional Application No. 17 / 225,543, filed on April 8, 2021, entitled “COATED OILFIELDOPERATIONAL COMPONENTS AND METHODS FOR PROTECTING AND EXTENDING THE SERVICELIFE OF OILFIELD OPERATIONAL COMPONENTS,” the disclosures of all of which are incorporated herein by reference in their entirety. ; Technical Field
[0003] The present disclosure relates to coated oilfield operation components, methods for protecting oilfield operation components, and methods for extending the useful life of oilfield operation components. Background Art
[0004] Oilfield operations involve the use of many components that are subjected to harsh use. For example, many components are part of a system that supplies fluids at high flow rates, high pressures, and other uses and environmental conditions that will be understood by those skilled in the art. As an example, a fracturing operation involves providing a fracturing fluid at a high flow rate and high pressure sufficient to fracture an oil-bearing formation to allow hydrocarbons to flow more easily from the formation to the well for production. For example, a typical flow rate may be in the range of about 1,500 to about 4,000 gallons per minute, and a typical pressure may be in the range of about 7,500 to about 15,000 pounds per square inch. Such high flow rates and high pressures may cause significant wear of the components associated with the fluid flow. Further, current fracturing operations may involve up to two to three times the hydraulic horsepower of delivering the fracturing fluid to the formation compared to similar operations performed a decade ago. This increase generally results in a sharp reduction in the service life of the fluid handling components of the fracturing operation. In addition, the fracturing fluid may contain substances or particles with corrosive and abrasive properties, which may increase the wear rate of the components exposed to the fracturing fluid. In addition, components may contain internal passages and structures that increase the effect of fluid flow through the components, such as elbows, valves, seals, and pump impellers, which may be exposed to the effects of cavitation. Therefore, components associated with oilfield operations often experience high wear rates, resulting in the need for replacement, which results in significant expenses associated with replacement costs and downtime. Therefore, it may be desirable to develop systems and methods for extending the service life of oilfield components. At least some of the examples described herein can address one or more of the above-mentioned possible problems, as well as possible other problems. Summary of the invention
[0005] As mentioned above, components associated with oilfield operations often experience high wear rates, resulting in the need for replacement, which results in a large amount of expense associated with replacement costs and downtime. For example, many components are part of a system that supplies fluids at high flow rates, high pressures, and other use and environmental conditions that will be understood by those skilled in the art. High flow rates and high pressures may cause significant wear of components associated with fluid flow. In addition, the fracturing fluid may contain substances or particles with corrosive and abrasive properties, which may increase the wear rate of components exposed to the fracturing fluid. In addition, the components may contain internal passages and structures that increase the impact of fluid flow through the components and may be exposed to the impact of cavitation, such as elbows, valves, seals, and pump impellers.
[0006] The present disclosure generally relates to coatings, oilfield operation components, and related methods that can significantly reduce the wear rate associated with oilfield operation components. In some examples, the coatings and methods can protect oilfield operation components by absorbing and / or dissipating the energy of the fracturing fluid as it passes through the components. In some examples, the coatings and methods can protect oilfield operation components from kinetic energy associated with particles in the fracturing fluid and / or impact energy associated with cavitation of the fracturing fluid as it flows through the oilfield operation components.
[0007] In a first aspect, an oilfield operation component configured for use in oilfield operations may include a component body comprising a surface positioned to be exposed to a fluid stream during oilfield operations. The oilfield operation component may also include a coating that at least partially covers the surface of the component body to enhance the wear resistance of the component body, so that the oilfield operation component exhibits a comparison factor of greater than about 2 indicating increased wear resistance. The coating may include a primer applied to the surface of the component body and a coating composition that at least partially coats the primer. The coating composition may include a trifunctional silane, a silanol fluid, and a filler. The coating composition may be positioned to chemically bond with the primer.
[0008] In another aspect, a method for protecting an oilfield-operated component exposed to the flow of oilfield fluids may include applying a primer composition to the oilfield-operated component. The method further includes at least partially curing the primer composition to form a primer layer, such that the primer layer is at least partially mechanically bonded to the oilfield-operated component. The method further may include applying a coating composition to the primer layer and at least partially curing the coating composition to form a coating layer at least partially chemically bonded to the primer layer, thereby enhancing the wear resistance of the oilfield-operated component, such that the oilfield-operated component exhibits a comparison factor greater than about 2 indicating increased wear resistance.
[0009] In still other aspects, a method for increasing the service life of an oilfield operation component may include at least partially coating an oilfield operation component positioned for use in an oilfield operation to obtain a first coating layer on the oilfield operation component, thereby enhancing the wear resistance of the oilfield operation component, so that the oilfield operation component exhibits a comparison factor greater than about 2 indicating increased wear resistance, the oilfield operation component being positioned for use in an oilfield operation. The method may also include incorporating the oilfield operation component into the oilfield operation and exposing the oilfield operation component to a fluid flow in the oilfield operation for a first period of time. The method may further include at least partially removing at least a portion of the first coating layer from the oilfield operation component and at least partially coating the oilfield operation component to obtain a second coating layer on the oilfield operation component. One or more of the first coating layer or the second coating layer may include a trifunctional silane, a silanol fluid, and a filler. The one or more of the first coating layer or the second coating layer may be positioned to reduce the wear rate of the oilfield operation component when exposed to a fluid flow associated with an oilfield operation.
[0010] According to yet another aspect, a coating composition for application to a surface of an oilfield operation component configured to be exposed to an oilfield fluid may include a trifunctional silane, a silanol, and a filler. In some examples, the silicon in the coating composition may be configured to chemically bond with a cured primer composition comprising an epoxy resin.
[0011] On the other hand, the oilfield operation assembly configured for use in oilfield operations can include an oilfield operation assembly and a coating that at least partially covers the assembly. In some instances, the coating can include a coating composition that at least partially coats the assembly, and the coating composition can include a trifunctional silane, a silanol fluid, and a filler. In some instances, the coating composition can be configured to chemically bond to a cured epoxy primer.
[0012] On the other hand, a method for applying a coating composition to at least a portion of an oilfield operation assembly configured for oilfield operation can include applying a primer composition to the oilfield operation assembly and making the primer composition at least partially solidify to form a primer layer that is at least partially solidified on at least a portion of an assembly. The primer layer that is at least partially solidified can be configured to form a mechanical key with at least a portion of an assembly. The method can further include applying a coating composition to the primer layer that is at least partially solidified. In some instances, the coating composition can include trifunctional silane, silanol fluid and filler. The method can further include making the coating composition at least partially solidify so that the coating composition and the primer that is at least partially solidified are chemically bonded at least in part.
[0013] In yet another aspect, a method for protecting an oilfield operating component exposed to the flow of an oilfield fluid may include applying a primer composition to the component and at least partially curing the primer composition to form a primer layer, such that the primer layer is at least partially mechanically bonded to the component. The method may further include applying a coating composition to the primer layer and at least partially curing the coating composition to form a coating layer at least partially chemically bonded to the primer layer.
[0014] According to another aspect, a method for dissipating energy generated by cavitation associated with a fluid flow may include providing a coating on at least a portion of a component, the cavitation being associated with an oilfield operating component exposed to an oilfield fluid. In some examples, the providing may include applying a primer composition to the oilfield operating component and at least partially curing the primer composition to form a primer layer, such that the primer layer is at least partially mechanically bonded to the component. The method may further include applying a coating composition to the primer layer and at least partially curing the coating composition to form a coating layer that is at least partially chemically bonded to the primer layer.
[0015] In still other aspects, a method for dissipating kinetic energy associated with particles in an oilfield fluid that impacts an oilfield operation component can include providing a coating layer on at least a portion of the component. In some examples, the providing can include applying a primer composition to the oilfield operation component and at least partially curing the primer composition to form a primer layer such that the primer layer is at least partially mechanically bonded to the component. The method can further include applying a coating composition to the primer layer and at least partially curing the coating composition to form a coating layer that is at least partially chemically bonded to the primer layer.
[0016] On the other hand, a method for increasing the service life of an oilfield operation component can include at least partially coating an oilfield operation component to obtain a first coating layer on the component, the oilfield operation component being configured to be used in oilfield operations. In some instances, the method can further include incorporating the oilfield operation component into the oilfield operation and exposing the oilfield operation component to a fluid flow in the oilfield operation for a first time period. The method can further include at least partially removing at least a portion of the first coating layer from the oilfield operation component and at least partially coating the oilfield operation component to obtain a second coating layer on the component. In some instances, at least one of the first coating layer or the second coating layer can include a trifunctional silane, a silanol fluid, and a filler. The at least one of the first coating layer or the second coating layer can be configured to reduce the wear rate of the oilfield operation component when exposed to a fluid flow associated with an oilfield operation.
[0017] According to another aspect, a method for repairing paint damage on an oilfield operation component can include exposing at least a portion of a first primer layer associated with a damaged portion of the paint, the oilfield operation component being configured for use in an oilfield operation. The method can further include applying a primer composition to at least a portion of the first primer layer and at least partially curing the primer composition to obtain a second primer layer bonded to at least a portion of the first primer layer. The method can also include applying a coating composition to a second primer layer and at least partially curing the coating composition so that the coating composition is at least partially chemically bonded to the second primer layer.
[0018] In still another aspect, a method for repairing paint damage on an oilfield operation component can include exposing at least a portion of a first primer layer associated with a damaged portion of the paint and removing at least a portion of the first primer layer to expose a surface of the component, the oilfield operation component being configured for use in an oilfield operation. The method can further include applying a primer composition to the surface of the oilfield operation component and at least partially curing the primer composition to obtain a second primer layer bonded to the component surface. The method can also include applying a coating composition to the second primer layer and at least partially curing the coating composition so that the coating composition is at least partially chemically bonded to the second primer layer.
[0019] In yet another aspect, a method for replacing at least a portion of a first coating from an oilfield operation component can include removing at least a portion of the first coating from the oilfield operation component and exposing at least a portion of the component and cleaning at least a portion of the component, the oilfield operation component being configured for use in an oilfield operation. The method can further include applying a primer composition to at least a portion of the oilfield operation component and at least partially curing the primer composition to form a primer layer at least partially mechanically bonded to at least a portion of the component. The method can also include applying a coating composition to the primer layer and at least partially curing the coating composition to form a coating layer at least partially chemically bonded to the primer layer.
[0020] According to other aspects, a method for preparing a coating composition for at least a portion of being applied to an oilfield operation assembly to reduce the damage induced by oilfield fluid flow can include providing a trifunctional silane, providing a silanol fluid and providing a filler. The method may further include combining the trifunctional silane, the silanol fluid and the filler. The method may further include mixing the trifunctional silane, the silanol fluid and the filler to obtain a coating composition. In some instances, the coating composition may be configured to form a coating layer on at least a portion of the assembly, and the coating layer may be configured to reduce the damage induced by oilfield fluid flow.
[0021] In yet another aspect, a method for adjusting the hardness of a coating may include preparing a coating composition, the coating being configured to protect at least a portion of an oilfield operating component configured to be exposed to an oilfield fluid. The coating composition may include an amount of a trifunctional silane, an amount of a silanol fluid, and an amount of a filler. The method may further include at least one of the following: (1) increasing the amount of the silanol fluid relative to at least one of the amount of the trifunctional silane or the amount of the filler to reduce the hardness of the coating; (2) reducing the amount of the silanol fluid relative to at least one of the amount of the trifunctional silane or the amount of the filler to increase the hardness of the coating; (3) increasing the amount of the filler relative to at least one of the amount of the trifunctional silane or the amount of the silanol fluid to increase the hardness of the coating; or (4) reducing the amount of the filler relative to at least one of the amount of the trifunctional silane or the amount of the silanol fluid to reduce the hardness of the coating. In some examples, the coating composition can be configured to form a coating layer on the at least a portion of the component, and the coating layer can be configured to reduce damage induced by oilfield fluid flow.
[0022] In still another aspect, a method for adjusting the viscosity of a coating composition for application to at least a portion of an oilfield operation component may include preparing a coating composition, wherein the oilfield operation component is configured to be exposed to an oilfield fluid. The coating composition may include an amount of a trifunctional silane, an amount of a silanol fluid, an amount of a filler, and an amount of a solvent. The method may further include one of the following: (1) increasing the amount of solvent relative to at least one of the amount of the trifunctional silane, the amount of the silanol fluid, or the amount of the filler to reduce the viscosity of the coating composition; or (2) reducing the amount of solvent relative to at least one of the amount of the trifunctional silane, the amount of the silanol fluid, or the amount of the filler to increase the viscosity of the coating composition. In some instances, the coating composition may be configured to form a coating layer on at least a portion of the component, and the coating layer may be configured to reduce damage induced by the flow of oilfield fluids.
[0023] According to another aspect, a method for providing a flexible coating on the surface of an oilfield operation component may include applying a primer composition to the component, and the oilfield operation component is configured to be exposed to oilfield fluid flow. In some instances, the primer composition may include an epoxy resin. The method may further include at least partially curing the primer composition to obtain a primer layer with a dry film thickness range of about 20 microns to about 100 microns. The method may also include applying a first coating composition to the primer layer, and the first coating composition may include at least one of trifunctional silane, silanol or filler. The method may further include at least partially curing the first coating composition to obtain a first coating layer with a dry film thickness range of about 100 microns to about 250 microns. In some instances, the method may further include applying a second coating composition to the first coating layer, and the second coating composition may include at least one of trifunctional silane, silanol or filler. The method may further include at least partially curing the second coating composition to obtain a second coating layer with a dry film thickness range of about 100 microns to about 250 microns. In some examples, at least one of the primer layer, the first coating layer, or the second coating layer can be configured to reduce damage to oilfield operational components from oilfield fluid flow.
[0024] On the other hand, a method for providing an elastic coating on the surface of an oilfield operation component can include applying a primer composition to the component, and the oilfield operation component is configured to be exposed to oilfield fluid flow. In some instances, the primer composition can include epoxy resin. The method can further include making the primer composition at least partially solidify to obtain a primer layer with a dry film thickness range of about 20 microns to about 100 microns. The method can also include applying the first coating composition to the primer layer, and the first coating composition can include at least one of trifunctional silane, silanol or filler. The method can further include making the first coating composition at least partially solidify to obtain a first coating layer with a dry film thickness range of about 100 microns to about 250 microns. The method can also include applying at least one other coating composition to the first coating layer. The at least one other coating composition can include at least one of trifunctional silane, silanol or filler. The method can further include making at least one other coating composition at least partially solidify to obtain at least one other coating layer. In some examples, the total dry film thickness of the first coating layer and the at least one additional coating layer can be in the range of about 500 microns to about 1000 microns. In some examples, at least one of the primer layer, the first coating layer, or the at least one additional coating layer can be configured to reduce damage to oilfield operating components by oilfield fluid flow.
[0025] Still other aspects, examples and advantages of these exemplary aspects and embodiments are discussed in more detail below. It should be understood that the foregoing information and the following detailed description are only illustrative examples of various aspects and embodiments, and are intended to provide an overview or framework for understanding the nature and characteristics of the claimed aspects and embodiments. Therefore, by reference to the following description and the accompanying drawings, these and other purposes and the advantages and features of the present disclosure disclosed in this text will become apparent. In addition, it should be understood that the features of the various embodiments described herein are not mutually exclusive and can exist in various combinations and arrangements. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are included to provide a further understanding of the embodiments of the present disclosure, are incorporated into this specification and constitute a part thereof, illustrate embodiments of the present disclosure and are used together with the detailed description to explain the principles of the embodiments discussed herein. No attempt is made to show the structural details of the present disclosure in more detail and in various ways that may be practiced than may be required for a basic understanding of the exemplary embodiments discussed herein. As a matter of practice, the various features of the drawings discussed below are not necessarily drawn to scale. The sizes of the various features and elements in the drawings may be enlarged or reduced to more clearly illustrate the embodiments of the present disclosure.
[0027] Figure 1 is a schematic top view of an example oilfield operation including an example fracturing system, the schematic top view including a partial cross-sectional view of a schematically depicted example oilfield component having an interior surface at least partially coated with an example primer layer and an example coating layer according to the present disclosure.
[0028] Figure 2A is a schematic perspective view of an example fluid end that may be incorporated into a fracturing system according to the present disclosure.
[0029] Figure 2B is a schematic perspective view showing an example internal portion of a fluid end, as in accordance with the present disclosure Figure 2A Fluid end shown.
[0030] Figure 2C is a schematic perspective view of an example flow iron assembly that may be associated with a fluid transport portion of an oilfield operation, such as a fracturing system according to the present disclosure.
[0031] Figure 2D is a schematic perspective view of an example fracturing stack or frac stack that may be associated with a fluid transport portion of an oilfield operation, such as a fracturing system according to the present disclosure.
[0032] Figure 3is a partial cross-sectional schematic diagram of an example flow iron assembly having an interior surface at least partially coated with a primer layer and a paint layer and illustrating an example fluid passing through an oilfield operation assembly according to the present disclosure.
[0033] Figure 4 is a partial cross-sectional schematic diagram of an example flow iron assembly having an inner surface at least partially coated with a primer layer and a paint layer and illustrating example fluid flow directed toward and away from the inner surface of the flow iron assembly according to the present disclosure.
[0034] Figure 5 is a schematic perspective view showing an uncoated portion of an oilfield component, a primer layer, and a coating layer on the primer layer according to the present disclosure.
[0035] Figure 6 is a schematic perspective view of a primer layer, a first paint layer on the primer layer, a second paint layer on the first paint layer, and a third paint layer on the second paint layer according to the present disclosure.
[0036] Figure 7 is a schematic perspective view of an example particle in contact with an example coating layer according to the present disclosure.
[0037] Figure 8 is a schematic diagram of an example coating assembly configured to apply a coating composition to an oilfield operation component according to the present disclosure.
[0038] Fig.9A , 9B , 9C and 9D are schematic diagrams of a test arrangement according to the present disclosure, the test arrangement including a test sample exposed to a test fluid flow at an angle β relative to the test sample.
[0039] Fig.10 is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid stream for test results of uncoated (bare) test samples, coated test samples, and test samples coated with a chemically resistant coating according to the present disclosure, simulating a goathead assembly exposed to a fluid stream at different included angles.
[0040] Fig.11 is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid flow for test uncoated (bare) test samples and coated test samples tested in accordance with the present disclosure, simulating fluid end exposure to the fluid flow at different angles.
[0041] Fig.12is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid flow for test results of uncoated (bare) test samples and coated test samples tested in accordance with the present disclosure, simulating fracturing iron exposed to a fluid flow at different included angles.
[0042] Fig.13 is a graph of cumulative mass loss (grams (g)) versus time (hours (hr)) exposed to a test fluid flow for test results of uncoated (bare) test samples and coated test samples tested in accordance with the present disclosure, simulating a goat head, fluid end and frac iron exposed to a fluid flow at zero degrees.
[0043] Fig.14 is a graph of cumulative mass loss (grams (g)) versus time (hours (hr)) exposed to a test fluid flow for test results of uncoated (bare) test samples and coated test samples tested in accordance with the present disclosure, simulating a goat head, fluid end and frac iron exposed to a fluid flow at 30 degrees.
[0044] Fig.15 is a graph of cumulative mass loss in grams (g) versus time in hours (hr) of exposure to a test fluid flow, simulating a goat head, fluid end, and frac iron exposed to a fluid flow at 45 degrees, from test results for uncoated (bare) test samples and coated test samples in accordance with the present disclosure.
[0045] Fig.16 is a graph of cumulative mass loss in grams (g) versus time in hours (hr) of exposure to a test fluid flow, simulating a goat head, fluid end, and frac iron exposed to a fluid flow at 60 degrees, from test results for testing uncoated (bare) test samples and coated test samples in accordance with the present disclosure.
[0046] Fig.17 is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid flow for test results of uncoated (bare) test samples and coated test samples tested in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid flow at zero degrees.
[0047] Fig.18 is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid flow for test results of uncoated (bare) test samples and coated test samples tested in accordance with the present disclosure, simulating a goat head, fluid end and frac iron exposed to a fluid flow at 30 degrees.
[0048] Fig.19is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid flow from test results for uncoated (bare) and coated test samples in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid flow at 45 degrees.
[0049] Fig. 20 is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid flow from test results for uncoated (bare) and coated test samples in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid flow at 60 degrees.
[0050] Fig.21 is a bar graph showing estimated hours of wear depth of 0.014 inches relative to bare and coated samples, simulating goat heads, fluid ends, and frac irons exposed to fluid flow at different included angles and at each of two grit sizes (270 mesh and larger 100 mesh) in accordance with the present disclosure.
[0051] Fig. 22 is a bar graph showing estimated hours of wear depth relative to a bare sample, a sample with a coating depth of 0.014 inches (“Coated”), a sample with a coating depth of 0.028 inches (“Thick Coated”), and a sample coated with a chemically resistant coating (“Chemically Resistant”) in accordance with the present disclosure, simulating a goat's head exposed to fluid flow at zero degrees and 30 degrees and at each of two grit sizes (270 mesh and larger 100 mesh). DETAILED DESCRIPTION
[0052] Now with reference to the accompanying drawings in which the same numerals represent the same parts in several views, the following description is provided as an effective teaching of exemplary embodiments, and those skilled in the relevant art will recognize that many changes can be made to the described embodiments. It will also be apparent that some of the expected benefits of the embodiments described herein can be obtained by selecting some of the features of the embodiments without utilizing other features. Therefore, those skilled in the art will recognize that many modifications and adaptations to the embodiments described herein are possible, and in some cases can even be desirable and part of the present disclosure. Therefore, the following description is provided as an illustration of the principles of the embodiments rather than a limitation thereof.
[0053] The wording and terminology used herein are for the purpose of illustration and should not be considered to be restrictive. As used herein, the term "plurality" refers to two or more items or components. The terms "include", "comprising", "carrying", "having", "containing" and "involving", whether in written description or claims, are open terms, i.e., meaning "including but not limited to." Therefore, the use of these terms is intended to cover the items listed thereafter and their equivalents and additional items. With respect to any claim, only the transition phrases "consisting of..." and "consisting essentially of..." are closed or semi-closed transition phrases, respectively. Using sequential terms such as "first", "second", "third" in the claims to modify the claim element itself does not mean that any priority, priority, or order of a claim element is superior to the time sequence in which the action of another claim element or method is performed, but is only used as a label for distinguishing a claim element with a certain name from another element with the same name (but using sequential terms), thereby distinguishing these claim elements.
[0054] Generally, the present disclosure summarizes coating compositions, coated components and related methods, and is particularly used to protect components from the wear and tear associated with fluid flow in oilfield operations.Oilfield operations can include and are related to oil exploration, drilling, completion, production increase and / or production, such as any field activities associated with the oil industry.In some cases, for example, oilfield operations can also include the logistics activities of such operations, including pipelines and pipeline components, such as pipeline pumps, elbows and various pipeline sections.Fluid flow in oilfield operations can include any oilfield fluid flow, including any fluid or fluid-like material associated with any oilfield operation, including but not limited to fracturing fluid or any fluid, drilling fluid, production fluid and / or reservoir fluid associated with hydraulic fracturing operations.As an example, fracturing is an oilfield operation that stimulates hydrocarbon production, so that hydrocarbons can be more easily or more easily flow from underground formations to the borehole of the well.Although many examples discussed in the present disclosure are explained about fracturing equipment, fracturing components and related methods, other oilfield related operations, components and methods are also considered.
[0055] Figure 11 is a schematic top view of an example oilfield operation 10 including an example fracturing system 12 (e.g., a hydraulic fracturing system), and a partial cross-sectional view of a schematically depicted example oilfield assembly 14 is shown, the example oilfield assembly including an assembly body 16 having an inner surface coated at least partially by an example primer layer 18 and an example coating layer 20. In some instances, the fracturing system 12 can be configured to fractur e a formation by pumping a fracturing fluid into a well at high pressure and high flow rate. The fracturing fluid can include, for example, water, proppants and / or other additives, such as thickeners and / or gels. For example, the proppants can include sand, ceramic beads or balls, shells and / or other particles, and can be added to the fracturing fluid together with a gelling agent to produce a slurry. The slurry can be pressed from the surface into an underground formation by one or more pumps at a faster rate than the existing holes, cracks, faults or other spaces in the formation can accept. Therefore, the pressure rises rapidly to the extent that the formation breaks and begins to fracture. By continuing to pump the fracturing fluid into the formation, the existing fractures in the formation are enlarged and extended in a direction away from the wellbore, thereby forming a flow path to the well. When the pumping of the fracturing fluid stops, the proppant can be used to prevent the enlarged fractures from closing, or when the pumping of the fracturing fluid stops, the shrinkage degree of the enlarged fractures can be reduced. Once the well is fractured, a large amount of the injected fracturing fluid is made to flow out of the well, and the water and any proppant that is not left in the enlarged fracture can be separated from the hydrocarbons produced by the well to protect downstream equipment from damage and corrosion. In some cases, the production stream can be treated to neutralize the corrosive agents produced by the fracturing process in the production stream.
[0056] exist Figure 1 In the example shown, the fracturing system 12 includes a plurality of water tanks 22 for supplying water to the fracturing fluid, a chemical tank 24 for supplying a gel or agent for addition to the fracturing fluid, and a plurality of proppant tanks 26 (e.g., sand boxes) for supplying proppant to the fracturing fluid. The example fracturing system 12 shown also includes a hydration unit 28 for mixing water from the water tank 22 and gel and / or agent from the chemical tank 24 to form a mixture, such as gelled water. The example shown also includes a blender 30 that receives the mixture from the hydration unit 28 and the proppant from the proppant tank 26 via a conveyor 32. The blender 30 can mix the mixture and the proppant into a slurry for use as a fracturing fluid for the fracturing system 12. Once combined, the slurry can be discharged through a low-pressure hose 34, which conveys the slurry to two or more low-pressure pipelines 36 in a fracturing manifold 38. In the example shown, low-pressure lines 36 in a fracturing manifold 38 deliver slurry to a plurality of pumps 40 via low-pressure suction hoses 42 .
[0057] The pump 40 may be driven by a motor (e.g., an internal combustion engine and / or an electric motor) and discharges slurry (e.g., a fracturing fluid containing water, agents, gels, and / or proppants) at high pressure and / or high flow rate through separate high pressure discharge lines 44 into two or more high-pressure flow lines 46 on the fracturing manifold 38, sometimes referred to as "missiles." The flows from the flow lines 46 merge at the fracturing manifold 38, and one or more of the flow lines 46 provide flow communication with a manifold assembly 48, sometimes referred to as a "goat head." The manifold assembly 48 delivers the slurry to a wellhead manifold 50, sometimes referred to as a "zipper manifold" or "fracturing manifold." The wellhead manifold 50 may be configured to selectively divert the slurry to, for example, one or more wellheads 52 through the operation of one or more valves. Once the fracturing process is stopped or completed, the flow returning from the fractured formation is discharged into a return flow manifold 54, and the return flow may be collected in one or more return flow boxes 56.
[0058] As in Figure 1 As schematically depicted in , one or more components of the fracturing system 12 can be configured to be portable so that the fracturing system 12 can be transported to a well site, quickly assembled, operated for a relatively short period of time, at least partially disassembled, and transported to another location at another well site for use. For example, the components can be transported by a trailer and / or loaded into a truck so that the components can be easily transported between well sites.
[0059] At least some of the components of the fracturing system 12 may be collectively referred to as "frac irons". Such components may include, for example, straight sections of steel pipe and pipe joints, various fittings such as tees, cross fittings, transverse fittings, and Y-shaped fittings, which may provide joints for diverting or combining flows, and flow line assemblies including fittings configured to change the flow line route, such as elbows and swivels. In some instances, the fracturing iron may be configured to deliver fracturing fluids at high pressures and / or high flow rates. In some instances, the fracturing iron may incorporate instrumentation, other monitoring equipment, and / or control devices, such as stop valves, plug valves, check valves, throttle valves, pressure relief valves, butterfly valves, and / or throttle valves.
[0060] Because some components of the fracking system 12 may be subjected to high pressures and / or high flow rates, and because the fracking fluid may contain substances with abrasive and / or corrosive properties, such components of the fracking system 12 may exhibit high wear rates and / or high failure rates. At least some examples of coatings, coated components, and / or related methods may be directed to reducing such wear rates and / or failure rates.
[0061] like Figure 1As shown, the example oilfield component 14 has a component body 16 having an inner surface at least partially coated with an example primer layer 18 and an example paint layer 20 to protect the oilfield operation component 14 from wear induced by fluid flowing through the oilfield operation component 14, so that in at least some examples, the wear rate and / or failure rate of the oilfield operation component 14 can be reduced, and / or the service life of the oilfield operation component 14 can be extended, for example, as explained herein. In some examples, the primer layer 18 can be omitted or there can be more than one primer layer 18, and in some examples, there can be fewer or more paint layers 20 (e.g., one or two paint layers 20, or four or more paint layers 20). In examples with more than one primer layer 18, the primer layers 18 can be the same material or different materials, and / or the primer layers 18 can have the same thickness or different thicknesses. In examples having more than one paint layer 20 , the paint layers 20 may be the same material or different materials, and / or the paint layers 20 may have the same thickness or different thicknesses.
[0062] Figure 2A is a schematic perspective view of an assembly 14 in the form of an example fluid end 58, which may be incorporated into a fracturing system, such as Figure 1 An example fracturing system 12 is shown. Figure 2A In the example shown, the fluid end 58 includes a fluid end block 60, which may be generally formed of steel (e.g., stainless steel) and may be machined to provide internal passages and / or may be formed with internal passages (e.g., by casting). In some examples, the fluid end 58 may be connected to a power end of a reciprocating pump having a plurality of reciprocating plungers that cyclically at least partially extend into and at least partially retract from passages in the fluid end 58. During retraction, low-pressure fluid (e.g., fracturing fluid) is drawn into the fluid end 58, such as through a low-pressure suction hose 42 ( Figure 1 ), and during extension, high pressure fluid is discharged from the fluid end 58, for example, through the high pressure discharge line 44 ( Figure 1 ).
[0063] For example, Figure 2B is a schematic perspective view of an example interior portion 62 of the fluid end 58, as shown in Figure 2A The fluid end 58 is shown. Figure 2AA single portion 62 is shown, but the fluid end may include more internal portions. ) The example portion 62 includes an intake port 64 configured to facilitate the intake of fluid into the fluid end 58 and an exhaust port 66 configured to facilitate the discharge of fluid from the fluid end 58. The example portion 62 also includes a cylinder 68 configured to accommodate a reciprocating plunger of the power end of the pump. As the reciprocating plunger is at least partially retracted from the cylinder 68, fluid is sucked into the fluid end 58 through the intake port 64. As the plunger reciprocates, a valve (not shown) between the intake port 64 and the exhaust port 66 in the fluid end 58 operates cyclically to facilitate the intake and discharge of fluid from the fluid end 58. In this example manner, the fluid end 58 inhales fluid at low pressure and discharges fluid at high pressure. In some instances, the fluid end 58 may include multiple sets of intake ports, cylinders, and exhaust ports to pump fluid at higher pressures and / or flow rates. Due to the high pressures and large volumes to which the fluid end 58 is exposed, the fluid end block 60, valve, valve seat, and / or packaging of the fluid end 58 may be subject to high wear rates and / or high failure rates.
[0064] Figure 2C is a schematic perspective view of an example flow iron assembly 70 that may be associated with a fluid transport portion of an oilfield operation, such as a fracturing system. Figure 2C As shown, example flow iron assembly 70 includes a tubular portion 72 with an interior passage 74 defined by an interior surface 76 . Figure 2C The example tubular portion 72 shown in FIG. 7 is formed into a U-shape. Tubular portions having other shapes are contemplated, such as straight and ninety degree bends, obtuse bends, and acute bends. Figure 2C As shown, the example flow iron assembly 70 further includes a first coupler 78 at a first end of the tubular portion 72 and a second coupler 80 at a second, opposite end of the tubular portion 72. The first and second couplers 78 and 80 may be configured to couple the flow iron assembly 70 to other components of an oilfield operation (e.g., a fracturing system), for example, via complementary couplers of the other components.
[0065] Figure 2D is a schematic perspective view of an example frac stack 82 that may be associated with a fluid transport portion of an oilfield operation, such as the example frac system 12 . Figure 2D The example frac stack 82 shown in FIG. 8 includes an example goathead 84, an example upper master valve 86, an example lower master valve 88, and an example gate valve 90. The example frac stack 82 may generally correspond to Figure 1 In some examples, the goathead 84 can be configured to be used with one or more wellheads (e.g., similar to Figure 1In some examples, for example, as shown, the goat head 84 may include a plurality of connectors 92, which are configured to connect the flow iron to one or more wellheads so that the fracturing fluid can be supplied to one or more wellheads. In some examples, the upper main valve 86 and / or the lower main valve 88 may be configured to at least partially control the flow of the fracturing fluid to one or more wellheads during the fracturing operation. For example, during an emergency, one or more of the upper main valve 86 or the lower main valve 88 may be closed to close the wellhead. In some examples, the upper main valve 86 and / or the lower main valve 88 may be configured to be manually operated and / or remotely operated. In some examples, one or more gate valves in the gate valve 90 may be configured to at least partially control the flow of the fracturing fluid through the fracturing stack 82, such as controlling fluid backflow and / or during the cable evacuation operation.
[0066] Figure 3 is a partial cross-sectional schematic diagram of an example flow iron assembly 94 having an inner surface 96 at least partially coated with a primer layer 98 and one or more coating layers 100 (e.g., coating layers 100a, 100b, and 100c, as shown), and illustrating an example fluid 102 passing through the flow iron assembly 94. The example flow iron assembly 94 may correspond to any flow iron assembly used in oilfield operations, such as fracturing operations that may be performed by a fracturing system, such as Figure 1 The example fracturing system 12 is shown. Figure 3 The example flow iron assembly 94 shown in FIG. 9 includes an elbow, but other configurations of flow iron assemblies are contemplated, as are any fluid handling assemblies associated with oilfield operations.
[0067] Figure 3 The inner surface 96 of the illustrated example flow iron assembly 94 is at least partially coated with an example primer layer 98 and example coating layers 100a, 100b, and 100c to protect the flow iron assembly 94 from wear induced by the flow of the example fluid 102 through the flow iron assembly 94, so that, at least in some examples, the wear rate and / or failure rate of the flow iron assembly 94 can be reduced, and / or the useful life of the flow iron assembly 94 can be extended, for example, as explained herein. Figure 3In the schematically illustrated example of , fluid 102 is an example fracturing fluid, which includes, for example, water, one or more agents and / or gels, and proppant 104, which may include sand, ceramic beads or balls, shells, and / or other similar particles. In some examples, primer layer 98 may be omitted or there may be more than one primer layer 98. In examples with more than one primer layer 98, primer layers 98 may be the same material or different materials, and / or primer layers 98 may have the same thickness or different thicknesses. In some examples, there may be fewer or more coating layers 100. In examples with more than one coating layer 100, coating layers 100 may be the same material or different materials, and / or coating layers 100 may have the same thickness or different thicknesses.
[0068] As explained in more detail herein, in some instances, one or more in the coating layer 100 can be formed by coating composition, and coating composition can comprise trifunctional silane, silanol and / or filler.In the example comprising one or more primer layers 98, primer layer can be formed by primer composition, and described primer composition can comprise epoxy resin.In some instances, one or more in primer composition or coating composition can be solidified at least in part to form dry film layer.In some instances, primer layer can be solidified at least in part, and forms mechanical key with at least a portion of assembly.In some instances, described coating composition can be configured to be chemically bonded with the cured primer composition comprising epoxy resin.
[0069] Figure 4 1 is a partial cross-sectional schematic diagram of an example flow iron assembly 106 having an inner surface 108 at least partially coated with a primer layer 98 and one or more coating layers 100 (e.g., coating layers 100a, 100b, and 100c, as shown), and illustrating an example fluid flow 110 directed toward and away from the inner surface 108 of the flow iron assembly 106. Figure 4 In the schematically illustrated example of FIG. 1 , fluid stream 110 is an example fracturing fluid that includes, for example, water, one or more agents and / or gels, and proppant 112, which may include sand, ceramic beads or balls, shells, and / or other similar particles. Figure 4As schematically depicted in , one or more of the coating layers 100 can be configured to compress and / or bend in response to a fluid stream 110 impacting the coating layer 100. As explained in more detail herein, compression and / or bending of one or more of the coating layers can cause one or more of the coating layers 100 to absorb and / or dissipate energy associated with the fluid stream 110, which in at least some instances can be used to protect the inner surface 108 of the flow iron assembly 106. In some instances, the energy associated with the fluid stream 106 can include thermal energy and / or kinetic energy, which can be caused by, for example, the temperature of the fluid stream 110, the flow rate of the fluid stream 110, the impact of the proppant 104 on the one or more coating layers 100, and / or the impact caused by cavitation of the fluid stream 110 and other possible forms of energy associated with the fluid stream. In at least some instances, one or more coating layers 100 can also be used to reduce or eliminate any corrosive effects associated with the fluid stream 110.
[0070] Figure 5 is a schematic perspective view showing an uncoated portion of an oilfield operating component such as flow iron assembly 106 , a primer layer 98 covering a portion of flow iron assembly 106 , and a coating layer 100 covering primer layer 98 in accordance with the present disclosure.
[0071] Figure 6 is a schematic perspective view showing a primer layer 98 covering a portion of an oilfield operating component such as a flow iron assembly 106, a first paint layer 100a covering a portion of the primer layer 98, a second paint layer 100b covering a portion of the first paint layer 100a, and a third paint layer 100c covering a portion of the second paint layer 100b in accordance with the present disclosure.
[0072] For example, the primer composition may be applied to, for example, a flow iron assembly 106 as described herein, and may be at least partially cured (e.g., fully cured) to form a primer layer 98 bonded to the flow iron assembly 106 (e.g., forming a mechanical bond, a chemical bond, or a combination of mechanical and chemical bonds). Thereafter, the coating composition may be applied to, for example, the at least partially cured primer layer 98 as described herein, and may be at least partially cured (e.g., fully cured) to form a first coating layer 100a bonded to the primer layer 98 (e.g., forming a mechanical bond, a chemical bond, or a combination of mechanical and chemical bonds with the primer layer 98). Thereafter, the coating composition may be applied to, for example, the at least partially cured first coating layer 100a as described herein, and may be at least partially cured (e.g., fully cured) to form a second coating layer 100b (e.g., forming a mechanical bond, a chemical bond, or a combination of mechanical and chemical bonds with the first coating layer 100a). Thereafter, the coating composition may be applied to, for example, the at least partially cured second coating layer 100b as described herein, and may be at least partially cured (e.g., fully cured) to form a third coating layer 100c (e.g., forming a mechanical bond, a chemical bond, or a combination of mechanical and chemical bonds with the second coating layer 100b). It is contemplated that in some embodiments, primer layer 98 may be omitted, and in other embodiments, more than one primer layer may be applied and at least partially cured, as will be understood by those skilled in the art. It is contemplated that in some embodiments, less than three coating layers 100 may be applied and at least partially cured, and in other embodiments, more than three coating layers 100 may be applied and at least partially cured.
[0073] Figure 7 1 is a schematic perspective view of an example particle, such as a proppant 104, in contact with an example coating layer 100 according to the present disclosure. In some embodiments, one or more coating layers 100 (and / or one or more primer layers 98) can be at least partially elastically deformed, for example to form an elastic and / or resilient depression 114 under the impact of a particle, such as a proppant 104. For example, one or more primer layers 98 and / or one or more coating layers 100 can dissipate the kinetic energy associated with the impact of the particle as heat energy, and thereby suppress the particle before it reaches the substrate, so that the impacting particle can not cause erosion, crushing and / or deformation to the substrate (e.g., an oilfield operation component). Because the one or more coating layers 100 can absorb vibration energy as well as kinetic energy in at least some examples, secondary vibrations induced in the coating layer 100 by the impacting particle can be suppressed, which can prevent the secondary vibrations from being transmitted to the substrate. In addition, in at least some examples, the one or more coating layers 100 can be flexible, and thus the one or more coating layers can not hinder the bending of the component or apply additional mechanical stress to the bent component, as will be understood by those skilled in the art.
[0074] In at least some instances, the one or more coating layers 100 can be used to protect any fluid treatment component from degradation by the surrounding environment. For example, one or more coating layers can be configured to protect the fluid treatment component from erosion caused by particle impact, impact or cavitation. The erosion of particle impact may be caused by particles (e.g., proppant) entrained in a fluid flow, which may be a gas flow or a liquid flow. Impact can be a form of accelerated corrosion associated with bubbles entrained in the fluid flow. Cavitation may occur in incompressible fluids such as water, and cavitation may involve the formation of bubbles caused by boiling of the fluid under low pressure, and the sudden collapse of the bubbles. The formation and collapse of a single such bubble can be considered as a cavitation event. Therefore, in some cases, more than one mechanism in the particle impact, impact and / or cavitation mechanism can act on fluid treatment components such as flow iron components substantially simultaneously.
[0075] In at least some examples of coating composition, coating composition can comprise trifunctional silane.In at least some such examples, trifunctional silane can comprise ethoxysilane, ketoxime silane, alkenyloxy silane, amine silane, alkoxy silane and / or alkenyl silane.In at least some such examples, trifunctional silane can comprise ethyl triacetoxy silane and / or vinyl triacetoxy silane.In some such examples, trifunctional silane can comprise methyl tris (methyl-ethyl-ketoxime) silane and / or vinyl tris (methyl-ethyl-ketoxime) silane.
[0076] In at least some examples of coating compositions, coating compositions can include silanols such as silanol fluids. In at least some such examples, the silanol fluids can include polydialkylated siloxanes such as polydimethylsiloxanes. For example, the silanol fluids can include hydroxy-terminated polydimethylsiloxanes. In some such examples, the kinematic viscosity of the silanol fluids can range from about 90 centistokes to about 150,000 centistokes (e.g., from about 100 centistokes to about 130,000 centistokes, from about 200 centistokes to about 100,000 centistokes, from about 300 centistokes to about 90,000 centistokes, from about 400 centistokes to about 85,000 centistokes, or from about 500 centistokes to about 70,000 centistokes). For silanol fluids comprising linear chains and / or a monomodal molecular weight distribution, the silanol fluids can have a weight average molecular weight (MW) ranging from about 4,000 grams / mole (g / mol) to about 150,000 g / mol (e.g., from about 8,000 g / mol to about 140,000 g / mol, from about 12,000 g / mol to about 120,000 g / mol, or from about 10,000 g / mol to about 100,000 g / mol) and / or a hydroxyl content ranging from about 0.8 wt % to about 0.02 wt % (e.g., from about 0.7 wt % to about 0.05 wt %, from about 0.6 wt % to about 0.10 wt %, or from about 0.5 wt % to about 0.15 wt %). In some examples, the kinematic viscosity of the silanol fluid can range from about 700 centistokes to about 130,000 centistokes (e.g., with a linear chain and a monomodal distribution), a viscosity of about 700 centistokes (e.g., about 500 centistokes to about 900 centistokes or about 600 centistokes to about 800 centistokes), corresponding to a MW of about 18,000 g / mol and a hydroxyl content of about 0.2 wt.%. In some examples, the silanol fluid can have a kinematic viscosity ranging from about 2,000 centistokes to about 130,000 centistokes (e.g., with a linear chain and a monomodal distribution), a viscosity of about 2,000 centistokes (e.g., about 1,500 centistokes to about 2,500 centistokes or about 1,750 centistokes to about 2,250 centistokes), corresponding to a MW of about 35,000 g / mol and a hydroxyl content of approximately 0.09 wt.%. In some examples, the silanol fluid can have a kinematic viscosity ranging from about 40,000 centistokes to about 130,000 centistokes (e.g., with a linear chain and a monomodal distribution), a viscosity of 40,000 centistokes (e.g., about 35,000 centistokes to about 45,000 centistokes or about 37,500 centistokes to about 42,500 centistokes), a corresponding MW of about 85,000 g / mol and a hydroxyl content of about 0.04 wt.%.
[0077] In at least some examples, the coating composition may include one or more fillers. In at least some such examples, one or more fillers may include fumed silica and / or reinforcing agents, such as glass fiber, mica, wollastonite, kaolin and / or other phyllosilicates. In at least some examples comprising fumed silica, the fumed silica may be treated with an agent before or during addition to the remainder of the coating composition. Examples of treatment agents include hexamethylene disilazane, divinyl tetramethylene disilazane, chlorosilane and / or polydimethylsiloxane. In at least some examples, the one or more fillers may include particles with a relatively high aspect ratio and / or a relatively high shape factor. For example, a filler may include mica, and mica sheets with a high area-thickness ratio square root may be included in the coating composition. In at least some examples, a filler may include glass fiber, and glass fiber with a high aspect ratio may be included in the coating composition. In some examples, the aspect ratio of the filler is at least 2, and the shape factor is at least 2 or the aspect ratio is at least 2. In at least some examples, more than one type of filler can be included in the coating composition. For example, both fumed silica and mica can be included in the coating composition.
[0078] In at least some instances, the coating composition may include a catalyst, e.g., to accelerate the curing of the coating composition. In at least some such instances, more than one catalyst may be incorporated into the coating composition. In at least some instances that include a catalyst, the coating composition may include a tin catalyst, e.g., dibutyltin dilaurate.
[0079] At least some examples of the coating composition may include one or more pigments. Pigments may be used to improve the aesthetic appearance of the coated fluid treatment component and / or protect the fluid treatment component from visible light and / or ultraviolet light. In at least some examples, the coating composition may include one or more solvents, such as xylene and / or mineral spirits. The solvent may be used to adjust (e.g., reduce) the viscosity of the coating composition, such as to promote mixing the coating composition and / or applying it to the fluid treatment component. For example, one or more solvents may be included in the coating composition to promote the application of the coating composition to the fluid treatment component by spraying using a sprayer.
[0080] According to at least some examples, a relatively soft coating layer and / or a coating layer with a relatively low modulus can relatively more effectively protect fluid handling components such as flow iron components from damage and / or erosion from particle impact, collision and / or cavitation compared to a relatively hard coating layer and a coating layer with a relatively high modulus. In at least some examples, the coating composition can be adjusted and / or adjusted to form a coating layer adjusted for use in certain environments. For example, the relative hardness of the coating layer can be adjusted.
[0081] In at least some examples, a method for adjusting the hardness of a coating can include preparing a coating composition configured to protect at least a portion of a component configured to be exposed to a fluid, such as a fracturing fluid. The coating composition can include, for example, an amount of a trifunctional silane, an amount of a silanol fluid, and an amount of a filler. The method for adjusting the hardness of a coating layer can include at least one of the following: (1) increasing the amount of the silanol fluid relative to at least one of the amount of the trifunctional silane or the amount of the filler to reduce the hardness of the coating; (2) reducing the amount of the silanol fluid relative to at least one of the amount of the trifunctional silane or the amount of the filler to increase the hardness of the coating; (3) increasing the amount of the filler relative to at least one of the amount of the trifunctional silane or the amount of the silanol fluid to increase the hardness of the coating; or (4) reducing the amount of the filler relative to at least one of the amount of the trifunctional silane or the amount of the silanol fluid to reduce the hardness of the coating.
[0082] In at least some instances, the viscosity of the coating composition can be adjusted and / or regulated, for example, by changing the fraction of solvent (if any) contained in the coating composition. For example, when the coating composition is to be applied manually, for example, by applying the coating composition with a brush and / or spatula, a relatively high viscosity coating composition may be desirable. When the coating composition is to be applied, for example, by spraying onto a fluid handling component such as a flow iron assembly, a relatively low viscosity coating composition may be desirable.
[0083] In at least some examples, a method for adjusting the viscosity of a coating composition for application to at least a portion of an oilfield operation component can include preparing a coating composition, the oilfield operation component being configured to be exposed to a fluid such as a fracturing fluid. The coating composition can include an amount of a trifunctional silane, an amount of a silanol fluid, an amount of a filler, and an amount of a solvent. The method for adjusting the viscosity of the coating composition can include at least one of: (1) increasing the amount of solvent relative to at least one of the amount of the trifunctional silane, the amount of the silanol fluid, or the amount of the filler to reduce the viscosity of the coating composition; or (2) decreasing the amount of solvent relative to at least one of the amount of the trifunctional silane, the amount of the silanol fluid, or the amount of the filler to increase the viscosity of the coating composition.
[0084] In at least some examples of coating compositions comprising trifunctional silane, silanol fluid and filler, the trifunctional silane may account for about 0.01 wt% to about 20 wt% of the coating composition based on the non-solvent component; the silanol fluid may account for about 40 wt% to about 99 wt% of the coating composition based on the non-solvent component; and the filler (e.g., fumed silica) may account for about 0.01 wt% to about 25 wt% of the coating composition based on the non-solvent component. In some examples, the coating composition may also include one or more catalysts and / or one or more pigments, the one or more catalysts accounting for about 0.01 wt% to about 5 wt% of the coating composition based on the non-solvent component, and the one or more pigments accounting for about 0.01 wt% to about 10 wt% of the coating composition based on the non-solvent component.
[0085] In at least some instances, the coating composition may include one or more solvents. For example, per 100 weight portions of non-solvent components of the coating composition, the coating composition may include about 10 weight portions to about 300 weight portions of xylene to produce a coating composition comprising a solvent, and in some instances, the coating composition comprising a solvent may be applied by spraying onto a component. For example, about 100 weight portions (e.g., 108 weight portions) of xylene may be added to the non-solvent components of about 100 weight portions of the coating composition to produce a coating composition comprising a solvent.
[0086] In at least some examples of coating compositions comprising trifunctional silanes, silanol fluids, and fillers, the trifunctional silane may account for about 1.5 wt% to about 10 wt% of the coating composition based on the non-solvent component; the silanol fluid may account for about 60 wt% to about 95 wt% of the coating composition based on the non-solvent component; and the filler (e.g., fumed silica) may account for about 3 wt% to about 13 wt% of the coating composition based on the non-solvent component. In at least some such examples, the trifunctional silane may include acetoxysilane and / or ketoxime silane. In some examples, the coating composition may include one or more catalysts and / or one or more pigments, the one or more catalysts accounting for about 0.02 wt% to about 1 wt% of the coating composition based on the non-solvent component, and the one or more pigments accounting for about 0.02 wt% to about 5 wt.% of the coating composition based on the non-solvent component.
[0087] In at least some such coating compositions, the coating composition may include one or more solvents. For example, the coating composition may include about 20 to about 200 parts by weight of xylene per 100 parts by weight of the non-solvent component of the coating composition to produce a coating composition containing a solvent, which, in some instances, may be applied by spraying onto the component. For example, about 108 parts by weight of xylene may be added to about 100 parts by weight of the non-solvent component of the coating composition to produce a coating composition containing a solvent.
[0088] In at least some examples, the coating composition may include a trifunctional silane, a silanol fluid, and fumed silica. Based on the non-solvent component, the trifunctional silane may account for about 2wt% to about 7wt% of the coating composition; based on the non-solvent component, the silanol fluid may account for about 85wt% to about 92wt% of the coating composition; and based on the non-solvent component, the fumed silica may account for about 5wt% to about 10wt% of the coating composition. In at least some such examples, the trifunctional silane may include acetoxysilane and / or ketoxime silane. In at least some such examples, the coating composition may include one or more catalysts and / or one or more pigments, based on the non-solvent component, the one or more catalysts account for about 0.04wt% to about 0.4wt% of the coating composition, and based on the non-solvent component, the one or more pigments account for about 0.03wt% to about 1wt.% of the coating composition.
[0089] In at least some such coating compositions, the coating composition may include one or more solvents. For example, the coating composition may include from about 60 parts by weight to about 130 parts by weight of xylene per 100 parts by weight of the non-solvent component of the coating composition to produce a solvent-containing coating composition, which in some examples can be applied by spraying onto the component.
[0090] In at least some examples, the coating composition may include a trifunctional silane, a silanol fluid, and fumed silica. Based on the non-solvent component, the trifunctional silane may account for about 2wt% to about 7wt% of the coating composition; based on the non-solvent component, the silanol fluid may account for about 85wt% to about 92wt% of the coating composition; and based on the non-solvent component, fumed silica may account for about 5wt% to about 10wt% of the coating composition. In at least some such examples, the trifunctional silane may include ethyltriacetoxysilane, vinyltriacetoxysilane, methyltri(methyl-ethyl-ketoxime)silane and / or vinyltri(methyl-ethyl-ketoxime)silane.
[0091] In at least some examples, the coating composition may include a trifunctional silane, a silanol fluid, and fumed silica. In at least some such examples, the molar ratio of the trifunctional silane to the silanol fluid may be in the range of about 5:1 to about 1,000:1, and / or the molar ratio of the fumed silica to the silanol fluid may be in the range of about 10:1 to about 1,000:1, wherein for the purpose of ratio calculation, the molecular weight of the fumed silica is equal to the molecular weight of the silica. In at least some examples of coating compositions, the molar ratio of the trifunctional silane to the silanol fluid may be in the range of about 20:1 to about 300:1, and / or the molar ratio of the fumed silica to the silanol fluid may be in the range of about 100:1 to about 300:1, wherein for the purpose of ratio calculation, the molecular weight of the fumed silica is equal to the molecular weight of the silica.
[0092] A method for preparing a coating composition for applying to at least a portion of an oilfield operating component to reduce damage induced by fracturing fluid flow may include providing a trifunctional silane, a silanol fluid and a filler and combining the trifunctional silane, the silanol fluid and the filler. The method may further include mixing the trifunctional silane, the silanol fluid and the filler to obtain a coating composition. In some instances, the coating composition may be configured to form a coating layer on at least a portion of the component, and the coating layer may be configured to reduce damage induced by fracturing fluid flow. Mixing may include mixing the trifunctional silane, the silanol fluid and the filler to obtain a substantially uniform coating composition. The method may also include providing a solvent and mixing the solvent with the coating composition. The solvent may include xylene, mineral spirits and / or other petroleum distillates. In some instances, for every 100 parts by weight of non-solvent components, the solvent may account for about 10 parts by weight to about 300 parts by weight. In some instances, the method may include providing a catalyst and mixing the catalyst with the coating composition. The catalyst may be a tin catalyst.
[0093] A method for providing a flexible coating on the surface of an oilfield operation component may include applying a primer composition to an oilfield operation component configured to be exposed to a fracturing fluid flow, and the oilfield operation component is configured to be exposed to a fracturing fluid flow. In some examples, the primer composition may include an epoxy resin. The method may also include at least partially curing the primer composition to obtain a primer layer with a dry film thickness ranging from about 20 microns to about 100 microns. The method may further include applying a first coating composition to the primer layer. The first coating composition may include at least one of a trifunctional silane, a silanol, or a filler. The method may further include at least partially curing the first coating composition to obtain a first coating layer with a dry film thickness ranging from about 100 microns to about 250 microns. The method may also include applying a second coating composition to the first coating layer. The second coating composition may include a trifunctional silane, a silanol, and / or a filler. The method may also include at least partially curing the second coating composition to obtain a second coating layer with a dry film thickness ranging from about 100 microns to about 250 microns. The primer layer, the first coating layer and / or the second coating layer can be configured to reduce the damage of the fracturing fluid flow to the oilfield operation component. In some examples of the method, the first coating composition and the second coating composition can be substantially the same. The method can also include applying at least one additional coating composition to the second coating layer. The at least one additional coating composition can include trifunctional silane, silanol and / or filler. The method can further include at least one additional coating composition at least partially cured to obtain at least one additional coating layer. In some examples, the total dry film thickness of the first coating layer, the second coating layer and at least one additional coating layer can be in the range of about 500 microns to about 1,000 microns. In some examples, at least two of the first coating composition, the second coating composition or at least one additional coating composition are substantially the same. In some examples of the method, applying at least one additional coating composition can include applying a third coating composition, and at least one additional coating composition can include at least partially curing the third coating composition to obtain a third coating layer with a dry film thickness ranging from about 100 microns to about 250 microns.
[0094] A method for providing an elastic coating on the surface of an oilfield operation component can include applying a primer composition to an oilfield operation component configured to be exposed to the flow of a fracturing fluid, and the oilfield operation component is configured to be exposed to the flow of a fracturing fluid. The primer composition can include an epoxy resin. The method can also include making the primer composition at least partially solidify to obtain a primer layer with a dry film thickness range of about 20 microns to about 100 microns and applying the first coating composition to the primer layer. The first coating composition can include trifunctional silanes, silanols and / or fillers. The method can also include making the first coating composition at least partially solidify to obtain a first coating layer with a dry film thickness range of about 100 microns to about 250 microns. The method can further include applying at least one other coating composition to the first coating layer. The at least one other coating composition can include trifunctional silanes, silanols and / or fillers. The method can also include making at least one other coating composition at least partially solidify to obtain at least another coating layer. In some examples, the total dry film thickness of the first coating layer and the at least one additional coating layer can be in the range of about 500 microns to about 1,000 microns. In some examples, the primer layer, the first coating layer, and / or the at least one additional coating layer can be configured to reduce damage to oilfield operation components by the flow of fracking fluids.
[0095] It has been surprisingly found that at least some examples of primer layers and / or coating layers described herein are resistant to erosion by particle impact and / or cavitation, and therefore effectively protect fluid handling components such as oilfield components from such erosion by particle impact and / or cavitation. In at least some examples, as shown by the test results presented herein, the erosion resistance and erosion protection provided can be superior to many materials used in fluid handling components, such as steel, aluminum, tungsten carbide and nickel. At least some examples of primer layers and / or coating layers can be used to provide protection against the impact of impact and impact of particles such as proppants. For example, as described herein, silanol chains cross-linked by trifunctional silanes may result in coatings with unexpected useful properties, such as erosion resistance, and when used to protect fluid handling components from particle impact, impact and / or cavitation, the service life of the fluid handling components can be significantly extended.
[0096] Without wishing to be bound by theory, it is believed that for at least some examples, the primer layer and / or coating layer described herein can protect the substrate from erosion and cracking by at least one of several possible mechanisms. For example, the primer layer and / or coating layer can dissipate the vibration energy associated with cavitation on or near the substrate as heat energy. In at least some such cases, the vibration energy may not reach the substrate and may not induce the formation of microcracks, which may ultimately lead to failure of the substrate. In addition, the primer layer and / or coating layer can dissipate the kinetic energy associated with the impact of the particles as heat energy, and thereby suppress the particles before they reach the substrate, so that the impact particles can not cause erosion, crushing and / or deformation to the substrate. Because in at least some examples, the coating layer can absorb vibration energy as well as kinetic energy, the secondary vibration induced in the coating layer by the impact particles can be suppressed, which can prevent the secondary vibration from being transmitted to the substrate. In addition, in at least some examples, the coating layer can be flexible, and therefore the coating layer can not hinder the bending of the fluid treatment component or apply additional mechanical stress to the bent fluid treatment component.
[0097] For at least some examples, it is believed that the protection of the primer layer and / or coating layer to substrate, long operating life and flexibility can be enhanced by the relative viscoelastic properties of the primer layer and / or coating layer. This characteristic can help dissipate kinetic energy and / or vibration energy by converting kinetic energy and / or vibration energy into heat energy. The elastic properties of the primer layer and / or coating layer can make the primer layer and / or coating layer temporarily deformed by impact particles and basically return to its / their original shape in a relatively short period of time. The viscoelastic properties of the primer layer and / or coating layer can originate from the molecular structure of the primer layer and / or coating layer. For example, the silanol fluid can be a hydroxy-terminated polydialkylsiloxane, for example, with a hydroxy-terminated polydimethylsiloxane chain (PDMS-OH) at the end. When not subjected to stress, the silanol chain can be a random coil configuration. However, when subjected to stress, the chain may be extended, but after that, when releasing stress, it can be returned to its random coil configuration.
[0098] It is also believed that trifunctional silane can play the role of crosslinking agent.For example, trifunctional silane can react with the hydroxyl group on the coating composition component to form a covalent bond.When the total number of trifunctional silane exceeds the total number of hydroxyl groups on the coating composition component, all hydroxyl groups can be replaced by the functional group from trifunctional silane.For example, trifunctional silane can react with the hydroxyl group on the silanol chain, and after the silanol chain reacts with the trifunctional silane, the silanol chain can be referred to as a functionalized siloxane chain.For example, triacetoxylated silane can react with the hydroxyl group on the silanol chain to replace the hydroxyl group, release acetic acid and / or bond at the site where the previous hydroxyl group is located to form a siloxane chain with another silicon atom and two acetoxy groups.When using a hydroxyl-terminated silanol chain, an acetoxy-terminated siloxane chain can be formed.Trifunctional silane can also react with the hydroxyl group on other components of the coating composition, such as the hydroxyl group on the filler and the hydroxyl group on the pigment, to form a functionalized component.
[0099] It is believed that when the total number of trifunctional silane exceeds the total number of hydroxyl groups on the coating composition component, all hydroxyl groups are replaced by the functional group (e.g., acetoxy group) from the trifunctional silane and when there is no water, further reaction will not occur between the functionalized siloxane chain (e.g., other functionalized components such as functionalized fillers or functionalized pigments) and the trifunctional silane. Therefore, the coating composition can remain liquid as long as it is protected from moisture. However, when the coating composition is exposed to water, for example, when the coating composition is applied to the surface of the fluid treatment component and contacts with moisture in the air, further reaction may occur. For example, in the case of acetoxylated siloxane chains, it is believed that water reacts with acetoxy groups to form acetic acid and replaces acetoxy groups with hydroxyl groups. The hydroxyl groups on the siloxane chain can react with the remaining acetoxy groups on the siloxane chain to release acetic acid and form a bond between the siloxane chains afterwards. Similarly, a bond can be formed between other components (e.g., filler and / or pigment) of the functionalized composition and the siloxane chain. In at least some instances, there is no need to apply artificially generated heat to cure the coating layer. Because the trifunctional silane used to form the crosslinking has three functional sites to which the hydroxyl groups on the siloxane chain can be bonded, a chain network can be formed. In at least some instances, it can be expected that the siloxane chain is bonded to fillers and / or pigments by the reaction of hydroxyl groups and functional groups (e.g., acetoxy groups). Fillers and / or pigments can be used as additional crosslinking sites, and many siloxane chains can be connected to the crosslinking sites. In at least some instances, siloxanes (e.g., siloxane chains) can be UV-resistant, antioxidant, hydrophobic, nontoxic, chemically inert and / or can exhibit anti-valence properties. In at least some instances, the siloxanes can perform well in a relatively wide temperature range and / or can exhibit relatively high vapor permeability.
[0100] According to at least one hypothesis, the coating layer may have viscoelastic properties, and when particles impact the surface of the coating layer, the stress generated temporarily deforms the coating layer and stretches the siloxane chains. During the deformation process, the chains rub against each other, and through friction, a portion of the impact energy is converted into heat energy. This conversion into heat energy through interchain friction can explain the viscous nature of the coating layer. After the impact, the siloxane chains can recoil, and during the recoil, the chains can rub against each other so that the residual energy imparted to the coating layer by the particle impact can be converted into heat energy. During the stretching and recoil, crosslinking can play a role in maintaining the topological structure of the siloxane chains connected in the coating layer, so that the coating layer returns to its original shape before the particle impact. It is believed that this chain stretching and / or recoil action can explain the elastic properties of the coating layer. The process of chain stretching, recoil and interchain friction is also believed to be the reason for the conversion of vibration energy into heat energy (e.g., vibration energy associated with cavitation events). According to this hypothesis, the viscoelastic properties of the coating layer can improve the ability of the coating layer to resist the effects of particle impact, impact and / or cavitation and protect the substrate from particle impact, impact and / or cavitation.
[0101] In at least some examples described herein, the coating composition may include any trifunctional silane and silanol fluid. In at least some examples, specific components may be selected to control the physical and chemical properties of the coating layer formed by the coating composition, and the coating composition may be adjusted for a specific purpose or desired result. For example, in some uses, it may be desirable that the coating layer be able to prevent or protect the substrate from the influence of particles with high kinetic energy. In at least some such cases, for example, silanol chains with relatively low molecular weight may be used so that high crosslinking density may be obtained. A large amount of crosslinking per unit volume may be used to prevent the material from being too deformed when particles impact, and the energy of particle impact is allowed to be effectively distributed in a large amount of chains to reduce the possibility that a chain is stretched to a breaking point. Other uses may make it desirable to transmit relatively less vibration to the coating layer on the surface of the fluid treatment component or to adapt the coating layer to the bending of the fluid treatment component. It is believed that such uses may sometimes make it desirable to use silanol chains with relatively high molecular weight so that a material with relatively low crosslinking density and / or relatively low modulus may be formed. Thus, for at least some examples, a relative balance between hardness and elasticity of the coating layer can be achieved for a particular application, for example, by adjusting the molecular weight of at least some of the silanol chains.
[0102] A method for adjusting the hardness of a coating may include preparing a coating composition comprising an amount of a trifunctional silane, an amount of a silanol fluid, and an amount of a filler, the coating being configured to protect at least a portion of a component configured to be exposed to a fracturing fluid. The method may further include at least one of the following: (1) increasing the amount of the silanol fluid relative to at least one of the amount of the trifunctional silane or the amount of the filler to reduce the hardness of the coating; (2) reducing the amount of the silanol fluid relative to at least one of the amount of the trifunctional silane or the amount of the filler to increase the hardness of the coating; (3) increasing the amount of the filler relative to at least one of the amount of the trifunctional silane or the amount of the silanol fluid to increase the hardness of the coating; or (4) reducing the amount of the filler relative to at least one of the amount of the trifunctional silane or the amount of the silanol fluid to reduce the hardness of the coating.
[0103] A method for adjusting the viscosity of a coating composition for application to at least a portion of an oilfield operation component configured to be exposed to a fracturing fluid may include preparing a coating composition comprising an amount of a trifunctional silane, an amount of a silanol fluid, an amount of a filler, and an amount of a solvent. The method may also include at least one of: (1) increasing the amount of solvent relative to at least one of the amount of the trifunctional silane, the amount of the silanol fluid, or the amount of the filler to reduce the viscosity of the coating composition; or (2) decreasing the amount of solvent relative to at least one of the amount of the trifunctional silane, the amount of the silanol fluid, or the amount of the filler to increase the viscosity of the coating composition.
[0104] In some examples, the coating composition can be applied directly to the surface of a substrate such as a fluid handling component. In some examples, a primer layer can be applied to the surface of a substrate to improve the adhesion of one or more coating layers to the substrate. Such a primer layer can be an epoxy resin primer. For example, an epoxy resin primer composition can be applied to the surface of a substrate and partially and / or at least substantially cured to form a primer layer. Thereafter, the coating composition can be applied to the primer layer. In some examples, the primer composition can include an epoxy resin blend and / or an aliphatic amine. In some examples, the epoxy resin blend can include epichlorohydrin and a bisphenol (e.g., bisphenol F, such as Resin 862, manufactured by Resolution Performance Products LLC, may be a suitable epoxy resin blend). Examples of suitable aliphatic amines are, for example, EPIKURE TMCuring agent 3218. In some examples, the primer composition may also include a silane adhesion promoter, such as trimethoxysilane, triethoxysilane and / or 3-glycidoxypropyltrimethoxysilane. In at least some examples, the adhesion promoter is believed to enhance the chemical bonding of the coating layer containing silicone to the primer layer. In some examples, the primer composition may also include other components, such as to control viscosity and / or facilitate application of the primer composition to the substrate. For example, the primer composition may include a leveling agent, a solvent and / or a pigment. The leveling agent can be a modified urea-formaldehyde in butanol (e.g., manufactured by Cytec Industries Inc.). U-216-8 resin). The solvent may comprise a mixture of 2-ethoxyethanol and xylene.
[0105] In some examples, the primer composition may include an epoxy resin blend ranging from about 20 wt % to about 95 wt %, an adhesion promoter ranging from about 0.5 wt % to about 10 wt %, an aliphatic amine ranging from about 1 wt % to about 20 wt %, and a leveling agent, a solvent, and / or a pigment ranging from about 0.01 wt % to about 70 wt %. In some examples, the primer composition may include about 26 wt % of Resin 862, about 3.7 wt% 3-glycidoxypropyltrimethoxysilane, about 6.8 wt% EPIKURE TM Curing agent 3218, about 0.78wt% U-216-8 resin, about 42 wt% of 2-ethoxyethanol, about 13.2 wt% of xylene, and about 7.8 wt.% of pigment.
[0106] In some instances, before the primer composition is applied to the surface of the fluid handling component, the surface is prepared according to at least one of several steps. For example, the surface can be cleared of all foreign matter, such as dust, lint, oil, wax, corrosion products, oxidation and / or water. The surface can be prepared by sandblasting, which can remove foreign matter and provide a mechanical profile that can promote adhesion. Residual dust can be removed by forced air (e.g., an air blow gun). In some instances, after sandblasting, wiping the surface with a cloth or the like can be avoided, for example, to avoid lint contaminating the surface. In some instances, the primer composition can be applied within eight hours of preparing the surface, for example, to prevent oxidation of the prepared surface.
[0107] In some instances, before the primer composition is applied to the component surface, the components of the primer composition can be mixed and its reaction range is about 20 minutes to about 30 minutes. The primer composition can be applied to the surface of the oilfield operation component (or its fluid handling component) by spraying the primer composition on the surface, brushing the primer composition and / or applying it on the surface, and / or dipping the oilfield operation component into the primer composition. In some instances, when applying the primer composition by spraying, conventional spraying equipment can be used. In some instances, the spraying equipment can be a large volume low pressure (HVLP) type. The cup pressure can be arranged in the range of about 10 pounds per square inch (psi) to about 20psi, and the air pressure can be arranged in the range of about 30psi to about 40psi, for example to enhance atomization.
[0108] After the primer composition is applied to the fluid handling component, the primer composition can be cured for a period of time to form a primer layer. In some instances, the primer composition can be cured at least substantially. In some instances, the primer composition can be cured for eight hours or longer. In some instances, the primer composition can be cured for twelve hours or longer. In some instances, it is possible to test whether the primer layer is fully cured, for example, by wiping the primer layer with a cloth soaked with a solvent. When fully cured, the appearance of the primer layer can be generally unaffected by the solvent, and the cloth can generally not be stained with any color of the primer layer. In some instances, the primer composition can be applied to have a dry film thickness (for example, thickness after solvent evaporation and / or after curing) ranging from about 20 microns (μm) to about 80 μm. In at least some instances, it is believed that when the coating composition is applied on the primer layer, the unreacted functional groups in the coating composition can react with the unreacted functional groups in the primer layer, thereby causing chemical bonding between the functional groups.
[0109] Example techniques for applying the coating composition to the surface of the fluid handling component may include, for example, spraying the coating composition onto the surface, brushing and / or smearing the coating composition on the surface and / or dipping the surface into a batch of coating compositions. In some instances, the thickness of the coating layer (i.e., dry film thickness) that has evaporated the solvent and has at least partially solidified can be in the range of about 200 μm to about 3,000 μm. In some instances, the total dry film thickness of the coating layer can be in the range of about 500 μm to about 1,000 μm. In some instances, the coating composition can be applied by spraying using HVLP spray equipment. In some instances, the cup pressure can be set in the range of about 15 psi to about 30 psi, and the air pressure can be set in the range of about 35 psi to about 50 psi. In some instances, the coating composition can be diluted by including xylene and / or mineral spirits. In some instances, the coating composition can be applied using airless spray equipment. In some such instances, the pressure setting of the equipment can be in the range of about 2,000 psi to about 3,300 psi. For example, the pressure may be in the range of about 3,000 psi to about 3,300 psi. Airless spray techniques may reduce the required solvent fraction compared to the solvent fraction required for spraying using HVLP spray equipment.
[0110] In some examples, a dry film thickness of less than about 200 μm can be obtained by transferring the coating composition to the surface in a single pass. The term "transfer" is used to represent the deposition of a single-layer coating composition on the surface of a substrate such as an oilfield component. For complex and / or vertical surfaces, or in order to obtain a dry film thickness greater than about 200 μm, the coating composition can be applied in multiple thin layers. In some examples, the coating composition can be applied to an inner surface, such as the inner surface of other components through which a pipe or fluid can flow. In some examples, an initial layer of the coating composition can be applied to achieve a dry film thickness ranging from about 70 μm to about 100 μm. The initial layer can be made to be substantially completely dried and at least substantially cured throughout the entire thickness of the coating layer. In some examples, substantially fully cured may require about two hours to about three hours. In some examples, it is important not to apply another layer of the coating composition before substantially curing, because insufficient curing may induce the previously applied coating layer to separate from the surface and / or primer layer, which may affect the adhesion of one or more layers in the coating layer to the substrate. In some examples, a subsequent layer may be applied, and the dry film thickness of the subsequent layer may be up to about 500 μm. In some examples, after checking the separation of this subsequent coating layer from the surface or another coating layer, an additional subsequent coating layer may be applied at intervals of about one hour. In some examples, additional subsequent coating layers may be applied to obtain a coating layer dry film thickness of up to about 500 μm. In some examples, an initial coating layer with a dry film thickness ranging from about 70 μm to about 100 μm may be sprayed onto the surface of the component. This initial coating layer may be at least substantially cured. Thereafter, a subsequent coating layer may be sprayed onto the surface of the oilfield operation component and at least substantially cured to obtain a total dry film thickness of the coating layer ranging from about 200 μm to about 600 μm. In some examples, additional subsequent layers may be sprayed onto the surface of the oilfield operation component and at least substantially cured to obtain a total dry film thickness of the coating layer ranging from about 200 μm to about 3,000 μm.
[0111] In some instances, a method for maintaining the protection of oilfield operation components from particle impact, impact and / or cavitation erosion can include repairing and / or replacing one or more coating layers. The one or more coating layers may eventually wear out after a long period of time, and in some cases, may be damaged due to large and / or sharp objects impacting the coating layer or other situations. In some instances, a new coating layer can be directly applied to the coating layer that is worn or damaged, and can usually show a strong adhesion to the coating layer previously applied. In some instances, the damaged coating layer on the oilfield operation component can be repaired by applying a coating composition on the coating layer that is worn or damaged and making the applied coating composition basically dry and at least basically solidify. In some instances, one or more coating layers that are worn or damaged can be peeled off from the oilfield operation component before applying and curing the coating composition. In some instances, the coating layer that is worn or damaged can be removed by soaking at least the affected part of the oilfield operation component in, for example, mineral spirits for a period of two or more hours (this may cause the coating layer to swell) and thereafter scraping off or otherwise removing the damaged coating layer from the component surface. In some examples, the damaged coating layer can be removed by cutting through the coating layer and lifting the coating layer from the component through a concentrated water jet. In some such examples, the water jet can be discharged at a pressure of about 2,000 psi or more.
[0112] For the coated assembly with the primer layer exposed by the worn or damaged coating layer below the worn or damaged coating layer, in some instances, before applying the coating composition for the new coating layer, the old primer layer can be at least partially removed. Although the coating composition can be firmly adhered to the coating layer previously applied, in some instances, the new coating layer may not be firmly adhered to the old primer layer. Therefore, in some instances, before applying the new coating layer, at least partially removing the old primer layer may be advantageous. In some instances, the old primer layer can be removed by sandblasting, and therefore in some instances, the coating composition can be directly applied to the surface of the assembly, or in some instances, the primer composition can be applied to the exposed surface of the oil field operation assembly to form a new primer layer before applying the coating composition. In some instances, the surface of the original primer layer (for example, the primer layer below the worn or damaged coating layer) can be prepared (for example, by slightly sandblasting the original primer layer to expose the previously unexposed part of the primer layer), and thereafter the primer composition can be applied to the surface of the preparation of the original primer layer.
[0113] For coated components with one or more coating layers that are damaged in a relatively small area, in some instances, in at least some cases, it may be more economical to repair the one or more coating layers in a small area than to apply the coating composition to the entire surface of the component. In some instances, when damage is only present in a relatively small area (e.g., damage is limited to a wide area of more than or below 6 mm), and when the primer layer of the oilfield operation component is not exposed, the damaged area can be cleaned, for example, to remove foreign matter, a layer of coating composition can be applied, and the coating composition can be at least substantially cured. For examples where the surface of the primer layer and / or the oilfield operation component is exposed, a primer composition can be applied and it can be at least substantially cured before applying the coating composition. In some instances, when damage extends into a relatively large area (e.g., damage (e.g., holes) is present in a wide area of 6 mm or more), the damaged area can be treated or filled with, for example, an epoxy resin adhesive. In some such examples, epoxy resin adhesive can be processed to the damaged area and made flat with a putty knife, so that the surface of epoxy resin adhesive is in the range of about 0.5 millimeter to about 1 millimeter below the desired final surface. After this, epoxy resin adhesive can be cured at least substantially. In some examples, epoxy resin adhesive can be selected to include the silane that promotes bonding, so that once epoxy resin adhesive solidifies, coating composition can be directly applied to the surface of epoxy resin adhesive, without the need to apply primer layer in advance. In some examples, primer composition can be applied to cured epoxy resin adhesive. After primer composition is dried and solidified to form primer layer, coating composition can be applied. When repairing the damage of small areas, coating composition can be prepared as paste, for example, by not comprising solvent (or not comprising as much solvent as possible). In such examples, coating composition paste can be applied by using caulking gun, putty knife and / or brush, and coating composition paste can be made flat with putty knife. In some instances where damage over relatively large areas is being repaired, the coating composition may include a solvent and may be applied by spraying.
[0114] A method for repairing paint damage on an oilfield operation component may include exposing at least a portion of a first primer layer associated with a damaged portion of the coating and removing at least a portion of the first primer layer to expose the surface of the component, the oilfield operation component being configured for use in oilfield operations. In some instances, the method may further include applying a primer composition to the surface of the oilfield operation component and at least partially curing the primer composition to obtain a second primer layer bonded to the component surface. The method may also include applying a coating composition to the second primer layer and at least partially curing the coating composition so that the coating composition is at least partially chemically bonded to the second primer layer. In some instances, exposing at least a portion of the first primer layer may include applying mineral spirits to the coating and scraping off at least a portion of the coating to expose a portion of the first primer layer. In some instances, removing at least a portion of the first primer layer may include sandblasting the first primer layer.
[0115] A method for replacing at least a portion of a first coating from an oilfield operation component may include removing at least a portion of the first coating from the oilfield operation component and exposing at least a portion of the component, the oilfield operation component being configured for use in oilfield operations. The method may also include cleaning a portion of the oilfield operation component and applying a primer composition to a portion of the component. The method may further include at least partially curing the primer composition to form a primer layer that is at least partially mechanically bonded to a portion of the component and applying the coating composition to the primer layer. The method may also include at least partially curing the coating composition to form a coating layer that is at least partially chemically bonded to the primer layer. In some instances, cleaning a portion of the oilfield operation component may include heating a portion of the oilfield operation component at a temperature of at least about 650°F for at least about five hours. Some instances of the method may also include sandblasting a portion of the oilfield operation component before applying the primer composition. The method may also include drying the primer composition for at least twelve hours, at least eighteen hours, or at least twenty-four hours before applying the coating composition to the primer layer. In some examples, the method may include drying the coating composition for at least six hours, at least nine hours, or at least twelve hours and applying a second layer of the coating composition to the coating layer. The method may further include at least partially curing the second layer of the coating composition to form a second coating layer. In some such examples, the method may also include drying the second coating layer for a period of at least one hour. Thereafter, some examples of the method may also include applying a third layer of the coating composition to the second coating layer and at least partially curing the third layer of the coating composition for at least twelve hours, at least twenty-four hours, or at least thirty-six hours to form a third coating layer.
[0116] In some instances, one or more primer layers and / or one or more coating layers can be used to protect the surface of the assembly formed by various materials. For example, primer layers and / or coating layers can effectively protect the surface of metal, ceramic and / or polymer. For example, the surface of steel alloy, stainless steel alloy, aluminum alloy, nickel alloy, titanium alloy, lead alloy and / or other similar materials can be protected. In some instances, the surface of polyurethane, epoxy resin, polycarbonate, acrylic acid, polyester composite material, epoxy resin composite material and / or other similar materials can be protected. These materials are only examples, and it is considered that the surface of other materials known to those skilled in the art can be protected. In some instances, primer layers and / or coating layers can show effective resistance to high temperature degradation.
[0117] In some examples, for example, the component fractions in the primer composition and / or coating composition can be adjusted so that the primer composition and / or coating composition can be suitable for any of a variety of application methods, such as spraying, and methods such as brushing and / or painting that are usually associated with one-time production. In some examples, no special heat treatment is required to cure the primer composition and / or coating composition. Once applied to the component, the primer composition and / or coating composition may only need to be exposed to air (e.g., at a temperature close to room temperature).
[0118] In some examples, a method for increasing the service life of an oilfield operation component may include at least partially coating an oilfield operation component to obtain a first coating layer on the component, the oilfield operation component being configured to be used in oilfield operations. The method may also include incorporating the oilfield operation component into the oilfield operation and exposing the oilfield operation component to a fluid flow in the oilfield operation for a first time period. The method may further include at least partially removing at least a portion of the first coating layer from the component and at least partially coating the oilfield operation component to obtain a second coating layer on the component. In at least some examples, the first coating layer and / or the second coating layer may include a trifunctional silane, a silanol fluid, and a filler. In some examples, the first coating layer and / or the second coating layer may be configured to reduce the wear rate of the oilfield operation component, the oilfield operation component being exposed to a fluid flow associated with the oilfield operation. In some examples, the first time period may range from about 500 hours to about 2,000 hours. In some examples, the method may further include exposing the oilfield operation component to a fluid flow in an oilfield operation for a second time period after at least partially coating the oilfield operation component to obtain a second coating layer on the component. The second time period may range from about 500 hours to about 2,000 hours. The ratio of the first time period to the second time period may range from about 1.0 to about 1.5.
[0119] In some examples, the method may further include applying a primer composition to at least a portion of the oilfield operation component prior to at least partially coating the component. In some such examples, the method may further include at least partially curing the primer composition to form a bond between the primer composition and the component prior to at least partially coating the oilfield operation component. Some examples may also include at least partially curing the coating composition to form a chemical bond between the coating composition and the primer composition.
[0120] In some examples of the method, the method may further include at least partially removing at least a portion of the second coating layer from the component and at least partially coating the oilfield operation component to obtain a third coating layer on the component. In some examples, the third coating layer may include trifunctional silane, silanol fluid and filler, and the third coating layer may be configured to reduce the wear rate of the oilfield operation component when exposed to a fluid flow associated with oilfield operations. In some examples, the method may further include at least partially coating the oilfield operation component to obtain the third coating layer on the component, exposing the oilfield operation component to the fluid flow in the oilfield operation for a third time period. The scope of the third time period can be about 500 hours to about 2,000 hours. The scope of the ratio of the first time period and / or the second time period to the third time period can be about 1.0 to about 1.5.
[0121] This application also provides examples described below.
[0122] Example 1. An oilfield operation component configured to be used in oilfield operations, the oilfield operation component comprising:
[0123] an assembly body including a surface positioned to be exposed to fluid flow during oilfield operations; and
[0124] A coating at least partially covering the surface of the component body to enhance the wear resistance of the component body such that the oilfield operations component exhibits a comparison factor indicative of increased wear resistance of greater than about 2, the coating comprising:
[0125] a primer applied to the surface of the component body; and
[0126] A coating composition at least partially coats the primer, the coating composition comprising a trifunctional silane, a silanol fluid, and a filler, and the coating composition is positioned to chemically bond with the primer.
[0127] Example 2. An oilfield operation component according to Example 1, wherein the comparison factor indicates a first amount of time for a portion of the coating to wear to a first depth divided by a second amount of time for a portion of the component body to wear to a second depth equal to the first depth in the absence of the coating.
[0128] Example 3. The oilfield operation component of Example 1, wherein one of the following:
[0129] The oilfield operation component includes at least a portion of a goat head, and the comparison factor ranges from about 5 to about 30;
[0130] The oilfield operations component includes at least a portion of a fluid end, and the comparison factor ranges from about 3 to about 12; or
[0131] The oilfield operation component includes at least a portion of a fracturing iron component, and the comparison factor ranges from about 2 to about 20.
[0132] Example 4. The oilfield operation component of Example 1, wherein the coating composition further comprises titanium dioxide in an amount ranging from about 0.50 wt % to about 0.90 wt %.
[0133] Example 5. The oilfield operation component of example 1, wherein the coating composition comprises a blue pigment in an amount ranging from about 1.0 wt % to about 5.0 wt %.
[0134] Example 6. The oilfield operation component of Example 1, wherein the primer comprises an epoxy resin primer applied to the surface of the component body, the coating composition being at least partially chemically bonded to the epoxy resin primer.
[0135] Example 7. An oilfield operation component according to Example 6, wherein the oilfield operation component includes one or more of the following: a flow iron positioned to receive a portion of the fracturing fluid passing through it, a manifold positioned to receive at least a portion of the fracturing fluid passing through it, a single-line system positioned to receive at least a portion of the fracturing fluid passing through it, or a fracturing pump positioned to increase the pressure of the fracturing fluid.
[0136] Example 8. An oilfield operation component according to Example 1, wherein one or more of the trifunctional silane, the silanol fluid, or the filler is configured to cure and form ethyl T-resin units, each of which forms two or more bonds with one or more of the other ethyl T-resin units, silanol fluid, filler, or pigment.
[0137] Example 9. The oilfield operation component of example 1, wherein the silanol comprises one or more of a polydialkyl siloxane, a polydimethyl siloxane, or a hydroxyl terminated polydimethyl siloxane.
[0138] Example 10. The oilfield operation component of example 1, wherein the filler comprises fumed silica.
[0139] Example 11. The oilfield operation component of example 1, wherein the coating composition further comprises a reinforcing agent comprising one or more of glass fiber, mica, wollastonite, kaolin, or layered silicate.
[0140] Example 12. The oilfield operation component of Example 1, wherein the coating composition further comprises a silica treating agent comprising one or more of hexamethylenedisilazane, divinyltetramethylenedisilazane, chlorosilane, or polydimethylsiloxane.
[0141] Example 13. The oilfield operation component of example 1, wherein the packing has one or more of: an aspect ratio of at least 2, a shape factor of at least 2, or a length to diameter ratio of at least 2.
[0142] Example 14. The oilfield operation component of example 1, wherein the primer comprises one or more of an aliphatic amine, epichlorohydrin, bisphenol, a silane adhesion promoter, trimethoxysilane, triethoxysilane, or 3-glycidoxypropyltrimethoxysilane.
[0143] Example 15. A method for protecting an oilfield operation component exposed to oilfield fluid flow, the method comprising:
[0144] applying a primer composition to the oilfield operation component;
[0145] at least partially curing the primer composition to form a primer layer such that the primer layer is at least partially mechanically bonded to the oilfield operation component;
[0146] applying a coating composition to the primer layer; and
[0147] The coating composition is at least partially cured to form a coating layer that is at least partially chemically bonded to the primer layer, thereby enhancing the wear resistance of the oilfield operation component such that the oilfield operation component exhibits a comparison factor greater than about 2 indicative of increased wear resistance.
[0148] Example 16. The method of Example 15, wherein the comparison factor indicates a first amount of time for a portion of the coating to wear to a first depth divided by a second amount of time for a portion of the oilfield operation component to wear to a second depth equal to the first depth in the absence of the coating.
[0149] Example 17. The method according to Example 15, wherein one of the following:
[0150] The oilfield operation component includes at least a portion of a goat head, and the comparison factor ranges from about 5 to about 30;
[0151] The oilfield operations component includes at least a portion of a fluid end, and the comparison factor ranges from about 3 to about 12; or
[0152] The oilfield operation component includes at least a portion of a fracturing iron component, and the comparison factor ranges from about 2 to about 20.
[0153] Example 18. The method according to Example 15, wherein one or more of the following:
[0154] The coating composition includes a trifunctional silane, a silanol fluid and a filler;
[0155] The primer composition comprises one or more of aliphatic amine, epichlorohydrin, bisphenol, silane adhesion promoter, trimethoxysilane, triethoxysilane or 3-glycidoxypropyltrimethoxysilane; or
[0156] The oilfield fluid includes one or more of water, proppant or thickener.
[0157] Example 19. The method of Example 15, wherein applying the coating composition comprises spraying the coating composition onto the oilfield operation component through a spray head, the spray head being configured to atomize the coating composition when the coating composition is applied to the oilfield operation component.
[0158] Example 20. The method of Example 19, wherein spraying the coating composition onto the oilfield operation component through the spray head comprises:
[0159] pumping the coating composition via an airless pump at an output ratio ranging from about 40:1 to about 80:1 to a spray head configured to rotate and atomize the coating composition; and
[0160] While the coating composition is atomized and sprayed from the spray head, air is supplied to the spray head to rotate the spray head.
[0161] Example 21. The method according to Example 15, further comprising one or more of the following:
[0162] applying the coating composition to the coating layer to form a second coating layer and at least partially drying the second coating layer; or
[0163] The coating composition is applied to the second coating layer to form a third coating layer and the third coating layer is at least partially dried.
[0164] Example 22. A method for increasing the useful life of an oilfield operation component, the oilfield operation component being positioned for use in an oilfield operation, the method comprising:
[0165] at least partially coating an oilfield operation component to obtain a first coating layer on the oilfield operation component to enhance wear resistance of the oilfield operation component such that the oilfield operation component exhibits a comparison factor indicative of increased wear resistance of greater than about 2, the oilfield operation component being positioned for use in oilfield operations;
[0166] incorporating the oilfield operations assembly into an oilfield operation;
[0167] exposing the oilfield operation component to a fluid flow in the oilfield operation for a first period of time;
[0168] at least partially removing at least a portion of the first coating layer from the oilfield operation component; and
[0169] at least partially coating the oilfield operation component to obtain a second coating layer on the oilfield operation component, one or more of the first coating layer or the second coating layer comprising a trifunctional silane, a silanol fluid, and a filler,
[0170] The one or more of the first coating layer or the second coating layer are positioned to reduce a wear rate of the oilfield operation component when exposed to a fluid flow associated with the oilfield operation.
[0171] Example 23. The method of Example 22, wherein the comparison factor indicates a first amount of time for a portion of the coating to wear to a first depth divided by a second amount of time for a portion of the oilfield operation component to wear to a second depth equal to the first depth in the absence of the coating.
[0172] Example 24. The method according to Example 22, wherein one of the following:
[0173] The oilfield operation component includes at least a portion of a goat head, and the comparison factor ranges from about 5 to about 30;
[0174] The oilfield operations component includes at least a portion of a fluid end, and the comparison factor ranges from about 3 to about 12; or
[0175] The oilfield operation component includes at least a portion of a fracturing iron component, and the comparison factor ranges from about 2 to about 20.
[0176] Example 25. The method of Example 22, wherein the first time period ranges from about 500 hours to about 2000 hours.
[0177] Example 26. The method of Example 22, further comprising, after at least partially coating the oilfield operation component to obtain the second coating layer on the oilfield operation component, exposing the oilfield operation component to a fluid flow in the oilfield operation for a second period of time; and one or more of the following:
[0178] The second period of time ranges from about 500 hours to about 2000 hours; or
[0179] A ratio of the first time period to the second time period ranges from about 1.0 to about 1.5.
[0180] Example 27. The method according to Example 22, further comprising:
[0181] applying a primer composition to at least a portion of the oilfield operation component prior to at least partially coating the oilfield operation component;
[0182] prior to at least partially coating the oilfield operation component, at least partially curing the primer composition to form a bond between the primer composition and the oilfield operation component; and
[0183] The coating composition is at least partially cured to form a chemical bond between the coating composition and the primer composition.
[0184] Example 28. The method according to Example 22, further comprising:
[0185] at least partially removing at least a portion of the second coating layer from the oilfield operation component; and
[0186] The oilfield operation component is at least partially coated to obtain a third coating layer on the oilfield operation component, the third coating layer including a trifunctional silane, a silanol fluid, and a filler, the third coating layer being positioned to reduce a wear rate of the oilfield operation component when exposed to a fluid flow associated with the oilfield operation.
[0187] Example 29. The method of Example 28, further comprising exposing the oilfield operations component to a fluid flow in the oilfield operation for a third period of time after at least partially coating the oilfield operations component to obtain the third coating layer on the oilfield operations component.
[0188] Example 30. The method of Example 29, wherein one or more of the first coating layer or the second coating layer is formed from a coating composition comprising a pigment and titanium dioxide and one or more of a trifunctional silane, a silanol fluid, or a filler,
[0189] The coating composition comprises a pigment in an amount of about 1.0 wt % to about 5.0 wt % of the coating composition based on non-solvent components and titanium dioxide in an amount of about 0.50 wt % to about 0.90 wt % of the coating composition based on non-solvent components.
[0190] Example 1
[0191] Examples of coating compositions for protecting fluid handling components are presented in Table 1 below. The exemplary coating compositions include trifunctional silanes, silanol fluids, fillers, pigments, catalysts, and crosslinking agents. Dow Corning 3-0134 polymer manufactured by Dow Corning Corp. is used for the silanol fluid. Dow Corning 3-0134 polymer contains 400 ppm of hydroxyl groups and has a viscosity of 50,000 centistokes. Surface-treated Cabot TS-530 manufactured by Cabot Corp. is used for fumed silica. Transition metal ferrite spinel powder F-6331-2 Black Ferro manufactured by Ferro Corporation with a median particle size of less than 1 μm is used as a pigment. The catalyst for all examples is dibutyltin dilaurate. Four different crosslinking agents are used for the compositions presented in Table 1. Coating composition examples 1-13 include ethyl triacetoxy silane as a crosslinking agent. Coating composition Example 14 includes vinyl triacetoxy silane as a crosslinking agent. Coating composition Example 15 includes methyl tris(methyl-ethyl-ketoximino) silane as a crosslinking agent. Coating composition Example 16 includes vinyl tris(methyl-ethyl-ketoximino) silane as a crosslinking agent.
[0192] Table 1
[0193]
[0194] Table 2 below shows test data, which includes particle impact erosion rate of cured coating layer formed by each of the sixteen example coating compositions listed in Table 1. The particle impact erosion rate data is expressed in micrograms of cured coating layer wear per gram of sandblasting on the coating layer. The erosion rate test was performed by sandblasting at an impact angle of 30 degrees relative to the coating layer surface with a speed of 600 feet per second using aluminum oxide of 120 grit size. Particle impact erosion rate data of uncoated 1100 aluminum, uncoated 1008 low carbon steel, tungsten carbide and nickel are also shown for comparison. The particle impact erosion rate data corresponds to the metal mass of wear of each example in the example. Tungsten carbide is a high-speed oxygen fuel (HVOF) spray coating containing 17wt.% cobalt. Table 2 also shows the loss rate data of each coating layer in the coating layer associated with cavitation. The cavitation loss rate data is expressed in milligrams of cured coating layer exposed to cavitation wear per hour. Cavitation testing was conducted with the coating layer immersed in water and an ultrasonic horn vibrating at 20 kHz in the water, the ultrasonic horn being spaced 0.5 mm from the respective coating layer surface. Cavitation loss rate data for uncoated 1100 aluminum and uncoated 1008 mild steel are also shown for comparison. The cavitation loss rate data corresponds to the worn metal mass for these examples.
[0195] Table 2
[0196] Examples / Materials <![CDATA[Particle impact erosion rate μg 表面 / g 砂粒 > <![CDATA[Cavitation loss rate mg 表面 / hour]]> 1 4.2 -- 2 4.3 2.3 3 4.3 -- 4 4.6 2.1 5 4.7 -- 6 5.2 2.5 7 3.6 2.7 8 5.4 2.4 9 6.4 -- 10 7.4 3.6 11 5.6 2.4 12 5.1 1.7 13 5 2.4 14 4.6 3.5 15 5.5 3.5 16 5.8 3.5 Aluminum 1100 58.6 39 Steel 1008 99.3 10 Tungsten Carbide 69.9 -- nickel 129.2 --
[0197] For the cured coating layer formed from coating composition Example 10, a maximum particle impact erosion rate of 7.4 m / s was observed for the coating layer. 表面 / g 砂粒 The particle impact erosion rate of Example 10 was only about 13% of the particle impact erosion rate of uncoated 1100 aluminum and only about 7% of the particle impact erosion rate of uncoated 1008 mild steel. Thus, the coating layer produced by the example coating composition exhibited better corrosion resistance than both uncoated metals tested. For the cured coating layer formed from coating composition Example 10, a maximum cavitation loss rate of 3.6 mg / cm2 was observed for the coating layer. 表面 / hour. This cavitation loss rate is only about 9% of the cavitation loss rate of uncoated 1100 aluminum and only about 36% of the cavitation loss rate of uncoated 1008 mild steel. Thus, the coating layer produced by the example coating composition exhibits better cavitation resistance than both uncoated metals tested.
[0198] Example 2
[0199] Table 3 below shows six exemplary coating compositions, including silanol, filler, pigment, catalyst and crosslinker. The filler is fumed silica, the pigment is transition metal ferrite spinel powder F-6331-2 Black Ferro manufactured by Flow Corporation with a median particle size of less than 1 μm, the catalyst is dibutyltin dilaurate, and the crosslinker is ethyltriacetoxysilane.
[0200] Table 3
[0201]
[0202] When the example coating compositions C, D, E or F are applied to a fluid handling component and cured thereon, the particle impact erosion rate of the resulting coating layer is expected to be similar to the erosion rate of the coating layer exhibited by the example coating compositions 1-16 shown in Table 2 under similar conditions of sandblasting with 120 grit aluminum oxide at a speed of 600 feet per second and an impact angle of 30 degrees. The cavitation loss rate of the example coating layer formed by the example coating composition C, D, E or F is expected to be similar to the cavitation loss rate of the coating layer formed by the example composition 1-16 shown in Table 2 under similar ultrasonic treatment conditions with the coating layer immersed in water and an ultrasonic horn vibrating at 20 kHz in the water, the ultrasonic horn being spaced 0.5 mm from the surface of the corresponding coating layer. The example coating compositions A and B have different weight percentages of components than the example coating compositions 1-16 shown in Table 1. The particle impact erosion rate and cavitation loss rate of the coating layer formed by the example coating compositions A and B can be different from the results of the coating layer formed by the example coating compositions 1-16. However, coating compositions A and B, when cured on a fluid treatment component, are expected to produce useful respective coating layers that will effectively protect the fluid treatment component from erosion caused by particle impact, impingement, and / or cavitation.
[0203] The use of pigments other than Black Ferro F-6331-2 in the coating composition is expected to form a coating layer after curing that exhibits properties similar to the properties of a coating layer formed from a coating composition using Black Ferro F-6331-2 (e.g., similar erosion resistance and protection of fluid handling components from particle impact, impact, and / or cavitation). The use of a tin catalyst other than dibutyltin dilaurate and / or one of a number of other catalysts that are not tin-based and the use of a crosslinker other than ethyltriacetoxysilane, such as vinyltriacetoxysilane, methyltri(methyl-ethyl-ketoximo)silane, or vinyltri(methyl-ethyl-ketoximo)silane is expected to produce a corresponding coating layer after curing that exhibits properties similar to the properties of a coating layer formed from a composition using dibutyltin dilaurate and ethyltriacetoxysilane (e.g., similar erosion resistance and protection of fluid handling components from particle impact, impact, and / or cavitation).
[0204] Example Method
[0205] An example method for forming one or more primer layers and one or more coating layers according to at least some of the examples described herein will now be described. Unless otherwise indicated herein, the order of the steps described is not required for performing a method consistent with the methods described herein, some steps may be optional, and other steps are inconsistent with the methods described herein.
[0206] In some examples of the method, before the primer composition or coating composition is applied to the oilfield operation component to be treated, the damage or surface irregularities of the oilfield operation component can be visually inspected before treatment. Before the component is surface prepared, any surface irregularities in the component, such as hard surface layer, sharp fillet, corner and weld, can be removed by appropriate methods. In some examples, for example, for previously used components, the oilfield operation component can be solvent-cleaned (e.g., MEK) and / or vapor degreased (e.g., according to ASTM D4126). In some examples, the oilfield operation component can be cleaned, degreased and / or thermally degreased by baking the oilfield operation component in an oven to reach a component temperature of about 700°F for about eight hours, thereby substantially or completely removing potential contaminants. In some examples, the machined surface and / or any other part of the oilfield operation component that may be damaged by sandblasting can be covered before sandblasting to protect those parts of the oilfield operation component from sandblasting.
[0207] In some examples of the method, the environmental conditions of the processing area can be checked, and in some examples, a blotter test (e.g., according to ASTM 4285-83) can be performed. If the environmental conditions are suitable, the oilfield operation component can be sandblasted or white metal blasted using a 100 mesh aluminum oxide abrasive media according to NACENO.1 / SSPC-SP5 (e.g., white metal blasting). In some examples, the surface temperature of the oilfield operation component can be maintained at a temperature at least 5°F above the dew point.
[0208] In some examples of the method, the oilfield operation component can be sandblasted to form an anchor pattern of about 20 μm to about 30 μm. In some examples, the Testex Press-O-Film replica tape method can be used to verify the anchor profile. The tape profile can be measured using a spring micrometer (e.g., according to ASTM D4417).
[0209] In some examples of the method, after sandblasting, the method may further include applying a primer composition consistent with at least some examples of the primer composition described herein. In some examples, the primer composition can be applied relatively quickly after cleaning, such as within about four hours after sandblasting. If formed by steel, any humidity may cause flash rust of the oilfield operation component, and if such flash rust is observed, the method may include sandblasting again. In some examples of the method, the primer composition may be applied to the oilfield operation component only when the ambient temperature is higher than about 40 ° F and the relative humidity is less than about 85%, or when the oilfield operation component temperature is higher than about 5 ° F of the dew point. The primer composition can be applied by a sprayer that atomizes the primer composition.
[0210] In some examples of the method, a 2.5 gallon pressure paint can can be used with a dual regulator. The pressure can can be set at an air pressure ranging from about 40 psi to about 60 psi and a fluid pressure ranging from about 15 psi to about 20 psi. In some examples, before applying the primer composition, the surface of the oilfield operation component receiving the primer composition can be sandblasted with compressed air to reduce the chance of any surface contamination.
[0211] Some examples of the method may include applying the primer composition to achieve a dry film thickness ranging from about 20 μm to about 50 μm. In some examples, the method may include drying or curing the primer composition at about 70°F (e.g., under ambient conditions) for forty-eight hours, or in some examples, if the temperature is below 70°F, for seventy-two hours.
[0212] Some examples of the method may also include testing the primer layer to determine whether the primer layer has been sufficiently cured, such as by wiping the primer layer surface with a cotton swab dipped in xylene. If the tip of the cotton swab turns black, it may indicate that the primer composition should be further cured.
[0213] In some examples of the method, before applying the coating composition to the dried or cured primer layer, the method may include wiping the primer layer surface clean, for example, using a lint-free cloth to avoid contaminating the primer layer surface, as such contamination may result in insufficient adhesion of the coating composition to the primer layer.
[0214] In some examples of the method, an airless spray pump can be used to apply the coating composition. The coating composition can be applied by a sprayer that atomizes the coating composition. In some examples, a spin coating tool can be used with a pump so that the coating composition can be applied to the inner surface of the fluid handling component. In some examples, the coating composition can be applied by continuous application about every ten minutes to achieve a coating thickness of about 50 μm or thicker. In some examples, the air pressure of the airless pump can be set to a pressure ranging from about 15 psi to about 20 psi.
[0215] In some examples, the coating composition can be applied to an oilfield operating component to achieve a dry film thickness ranging from about 150 μm to about 200 μm. Once applied, the coating composition can be cured at a temperature of about 70°F (e.g., under ambient conditions) for a period of time ranging from about ten hours to about twenty-four hours. Thereafter, an additional layer of the coating composition can be applied to the at least partially cured layer of the coating composition to achieve an additional coating layer dry film thickness ranging from about 150 μm to about 200 μm. In some examples, this additional coating composition layer can be cured at a temperature of about 70°F for a period of time ranging from about one hour to about three hours.
[0216] Thereafter, in some instances, a second additional layer of the coating composition may be applied to the at least partially cured additional layer of the coating composition to achieve a second additional coating layer dry film thickness in the range of about 150 μm to about 200 μm. In some instances, this second additional coating composition layer may be cured for a time period in the range of about thirty-six hours to about eighty-four hours (e.g., about seventy-two hours) at a temperature of about 70 ° F, for example in a well-ventilated area with a relative humidity range of about 30% to about 70%. In some instances, the method may be included in curing the final coating composition layer for a minimum of seven days before using the assembly. Additional layers of the coating composition may be applied and / or cured, for example, in a manner at least similar to that described above. After applying and / or curing the last layer of the coating composition, the at least partially coated oilfield operation assembly may be inspected before being put into use.
[0217] Figure 8 is a schematic diagram of an example coating assembly 116 configured to apply a coating composition to an oilfield operation component according to the present disclosure. Figure 8 As shown, in some embodiments, the coating assembly 116 can include an airless pump 118 configured to pump a batch of the coating composition (or primer composition) from a reservoir 120 through a fluid line 124 (e.g., an airless fluid hose) to a spray gun 122 via a fluid line 119. As shown, some embodiments of the spray gun 122 can include a wand 126, which in some examples can include a back pressure hole 128. In some embodiments, the spray gun 122 can include an activation trigger 130 configured to cause the coating composition to be delivered to a coating tool 134 via a second fluid line 132. In some embodiments, for example, as shown, the coating tool 134 can include a spray head 136 configured to rotate as the spray head 136 rotates and discharge the coating composition from a plurality of spray holes 138. For example, the spray head 136 can include an air motor configured to rotate the spray head 136 by air pressure supplied from an air source 142 (e.g., a pressurized air box and / or an air compressor) via an air line 140. For example, the spray head 136 can be inserted into an interior 144 of a component 146 having an interior surface 148, to which the coating composition will be applied. Air can be supplied to the spray head 136 to rotate the air motor 136, and the airless pump 118 can supply the coating composition to the coating tool 134 and the spray head 136 under pressure, thereby atomizing the coating composition when the coating composition is passed through the orifice 138. In some examples, the rod 126 (i.e., instead of the spray head 136) can be inserted into the interior 144 of the component 146 to which the coating composition is to be applied, and the activation trigger 130 of the spray gun 122 can be engaged to manually apply the coating composition to the interior surface 148 of the component 146, as will be understood by those skilled in the art.
[0218] In some embodiments, the airless pump 118 can be configured to have an output ratio ranging from about 10:1 to about 100:1, such as about 20:1 to about 90:1, about 30:1 to about 80:1, about 40:1 to about 70:1, or about 50:1 to about 65:1 (e.g., about 60:1). For example, if the air from the air source 142 is supplied at about 100 pounds per square inch (psi) and the airless pump 118 has an output ratio of about 60:1, the coating composition can be passed through the spray holes 138 at about 6,000 psi, which may result in the coating composition being atomized into fine particles as the coating composition passes through the spray holes 138. In some embodiments, atomizing the coating composition in such a manner may result in a relatively smoother surface finish when the coating composition is applied to a surface, which may result in a more damage-resistant surface in some embodiments, as will be appreciated by those skilled in the art.
[0219] test
[0220] Steel samples coated with coating compositions consistent with the example coating compositions described herein were subjected to erosion testing. The purpose of the test was to measure and record the erosion resistance of a slurry containing fluid representing a fracturing fluid, wherein the coating layer was formed by a coating composition applied to the inner surface of a common fracturing system component (e.g., through which the fracturing fluid flows), including a goat head, a fluid end, and a fracturing iron component. Unless otherwise specified below, the coating layer on the test sample was 0.014 inches thick and formed by the same coating composition, which is consistent with at least some of the coating compositions described herein. Several base materials commonly used to form goat heads, fluid ends, and fracturing iron components were used to form the following test samples: alloy steel AISI 4130API-spec steel commonly used to form goat heads; stainless steel 17-4PH commonly used to form fluid ends; and alloy steel AISI 4715 commonly used to form fracturing iron components. The test comprises direct impingement flow of silica (SiO2) sand coated with a test sample of a cured coating composition consistent with at least some examples of the coating composition described herein and a bare test sample (i.e., an uncoated test sample) with a constant pressure difference. The test is usually continued for four hours with a constant slurry flow rate after the coating layer penetrates, wherein the test is paused every four hours to record the condition of the test sample after each flow interval. Typically, the total test time of the bare test sample matches the total test time of the corresponding test sample with the test coating layer. For each test sample tested, four impact angles are tested for comparison: 0 °, 30 °, 45 ° and 60 °. A constant nozzle outlet velocity is used in all tests.
[0221] Fig.9A , 9B, 9C and 9D are schematic diagrams of a test arrangement 150 including a test sample 152 exposed to a test fluid stream 154 discharged from a nozzle outlet 156, wherein the test sample 152 is at an impingement angle β relative to a horizontal plane (as depicted), the impingement angle comprising 0° ( Fig.9A )、30°( Fig. 9B )、45°( Fig. 9C ) and 60°( Fig.9D ). The size of each test sample 152 is three inches in diameter and one-half inch thick. Each test sample 152 is machined with two quarter-inch threaded holes on the back side to enable the test sample 152 to be mounted in a holder (not shown). For the test sample 152 with a coating layer, the surface of the test sample 152 is shot peened before applying the coating composition. After shot peening, a primer composition consistent with at least some of the example primer compositions described herein is applied to the test sample 152 so that a primer layer with a dry film thickness of about 25 μm is formed on the test sample. Thereafter, a coating composition consistent with at least some of the coating compositions described herein is applied to form a coating layer with a dry film thickness of about 30 μm to about 36 μm. All metal surfaces are prepared in the same manner so that the test sample substrate material properties are consistent.
[0222] The AISI 4715 material used to make the test specimens was carburized and exhibited a surface hardness of 62 HRC. This material was also case hardened to 44 HRC at a depth of about 1,780 μm. The core hardness of the test specimens was about 35 HRC. The AISI 4130 material used to make the test specimens is a standard API 75-ksi material. The hardness requirement per API is about 207 to about 35 HBW. The MTR for this material lists a hardness of about 212 to about 227 HBW.
[0223] Regarding the fluid flow for testing, all test samples and impact angles use a jet velocity of about 100 feet per second. This jet velocity is selected to increase the erosion rate and reduce the overall test time, so that it is expected that significant changes will occur within the four-hour test interval. A single, substantially constant jet velocity is used to reduce the number of test variables and minimize the number of changes required for the test fixture and related equipment. Regarding the composition of the fluid flow, the test slurry consists of tap water, to which erosion particles with a concentration of 20,000 parts by weight are added. At the flow rate selected for testing, this concentration means that about 200 pounds of gravel erosion agent is consumed every four hours of testing. The concentration of 20,000 parts by weight is the oil industry standard value and is specified in several American Petroleum Institute (API) standards. It is believed that concentrations exceeding 20,000 parts by weight may cause interactions between particles, which transform specific erosion (i.e., the total mass of the eroded material is normalized by dividing it by the total mass of the erosion agent) from a linear relationship to a nonlinear relationship.
[0224] The erosion material selected for the small grit test was "270 mesh" silica powder, and the erosion material selected for the large grit test was "100 mesh" silica powder. The relatively small 270 mesh grit has a D 10 , D of about 51μm 50 and D of about 130 μm 90 The relatively large 100 mesh gravel has a D of about 118 μm. 10 , D of about 194μm 50 and D of about 332 μm 90 The silica material is produced by processing round Midwest gravel into a finer particle size to achieve the desired particle size distribution. This results in a representation of solids in fracturing fluids that is accepted by the petroleum industry and is recommended for erosive flow testing in API standards, which include API 19ICD (inflow control device) and API 19ICV (interval control valve). The Mohs hardness of silica ranges from 6 to 7.
[0225] The sand particles mixed in the slurry passed through the test setup once and were discarded thereafter (i.e., the sand particles were not recycled back through the test arrangement). This procedure was used because silica particles have sharp corners or edges after grinding, and after multiple passes through the test arrangement, the sharp corners or edges may be smoothed / rounded by interaction with other particles and the test sample. The single-pass design more consistently affects the test samples with the most abrasive erosives. This single-pass approach is also considered to be the most representative of field conditions during fracturing operations.
[0226] The general test procedure used is as follows:
[0227] 1. Weigh the test sample in grams before testing, with a resolution of 0.01 grams;
[0228] 2. Install the test sample into the test sample holder;
[0229] 3. Obtain slurry samples and measure particle concentration to verify target particle loading;
[0230] 4. Start the flow test while maintaining the flow parameters constant within their respective defined ranges. After every two hours of erosion flow, obtain a new slurry sample to confirm that the particle concentration remains within the defined range;
[0231] 5. After each four-hour test interval (corresponding to a total grit flow of approximately 200 pounds), pause the test and remove the test sample from the holder. Clean the test sample and weigh it to record the weight of the material lost, and photograph the worn area to record its current condition;
[0232] 6. Measure the maximum wear depth in the test sample using a depth gauge; and
[0233] 7. Repeat steps 1 to 6 at additional four-hour intervals and continue to repeat flow intervals for a cumulative flow period of at least sixteen hours. After the sixteen-hour test is complete, decide whether the test should be continued further, for example, if the coating layer has not cracked or is only slightly damaged. Continue testing until a trend in the results is apparent and record it.
[0234] Test Results
[0235] For AISI 4130 alloy steel commonly used in goat heads, twelve tests were conducted on twelve test samples, including four test samples (i.e., samples B, F, J, and L) coated with a coating composition consistent with at least some examples described herein to form a 0.014-inch thick coating layer and four uncoated (bare) test samples (i.e., samples A, E, I, and K). In addition, two test samples were coated with a coating composition consistent with at least some examples described herein to form a 0.028-inch thick ("thick coating") layer instead of 0.014 inches thick (i.e., samples C and G), and two test samples were coated with a modified coating composition consistent with at least some examples described herein ("chemical resistant coating") to form a 0.014-inch thick coating layer (i.e., samples D and H).
[0236] Relative to at least some of the example coating compositions previously described herein, the modified coating compositions are modified to be chemically resistant to fluids such as fracturing fluids and / or petroleum that are commonly found in oilfield environments (or at least relatively more chemically resistant than unmodified coating compositions). For example, some embodiments of the coating compositions previously described herein may include a silanol fluid in an amount ranging from about 40 wt% to about 90 wt%, a fumed silica in an amount ranging from about 0.01 wt% to about 25 wt%, and / or a catalyst (dibutyltin dilaurate) in an amount ranging from about 0.01 wt% to about 10 wt%. In some embodiments of the modified coating compositions, the amount (or amounts) of one or more (or combination) of the silanol fluid, the fumed silica, or the catalyst may be reduced by an amount in the following ranges: about 1 wt% to about 10 wt%, about 2 wt% to about 9 wt%, about 3 wt% to about 8 wt%, about 4 wt% to about 7 wt%, or about 4 wt% to about 6 wt% (e.g., about 5 wt%, e.g., about 5.2 wt%), relative to the coating compositions previously described herein. In some embodiments, the wt % given may be for a cured coating, for example after solvents and / or volatiles have been lost and / or eliminated.
[0237] In some embodiments, the modified coating composition may include a silanol fluid in an amount ranging from about 75.0 wt% to about 85.0 wt%, about 76.0 wt% to about 84.0 wt%, about 77.0 wt% to about 83.0 wt%, about 78.0 wt% to about 82.0 wt%, about 79.0 wt% to about 82.0 wt%, about 80.0 wt% to about 82.0 wt%, or about 80.0 wt% to about 81.0 wt% (e.g., about 80.7 wt%). In some embodiments, the modified coating composition may include fumed silica in an amount ranging from about 13.0 wt% to about 17.0 wt%, about 14.0 wt% to about 16.0 wt%, about 14.5 wt% to about 15.5 wt%, or about 15.0 wt% to about 15.5 wt% (e.g., about 15.1 wt%). In some embodiments, the modified coating composition may include a catalyst (e.g., dibutyltin dilaurate) in an amount ranging from about 0.15 wt% to about 0.21 wt%, from about 0.16 wt% to about 0.20 wt%, or from about 0.17 wt% to about 0.19 wt% (e.g., about 0.18 wt%). In some embodiments, the cured and dried coating composition may include, for example, substantially all functional types of silanols, which are combined together and include silane chains and T-resins.
[0238] Some embodiments of the coating compositions previously described herein may include one or more crosslinking agents (e.g., trifunctional silanes such as ethyltriacetoxysilane) in an amount ranging from about 1 wt% to about 20 wt% (e.g., about 2 wt% to about 7 wt%). In some embodiments of the modified coating compositions, the amount of the crosslinking agent (e.g., ethyltriacetoxysilane) may be increased in an amount ranging from about 1 wt% to about 10 wt%, from about 2 wt% to about 9 wt%, from about 3 wt% to about 8 wt%, from about 4 wt% to about 7 wt%, or from about 4 wt% to about 6 wt% (e.g., about 5 wt%, such as about 5.2 wt%) relative to the coating compositions previously described herein. In some embodiments, the crosslinking agent (e.g., ethyltriacetoxysilane) may react with other silanols, fumed silica, and / or moisture in the air. In some such embodiments, the coating composition can be cured to form polymers, copolymers, and block polymers that can be collectively referred to as "ethyl T-resins," with each unit forming three links and / or bonds, each of which is to another unit of the ethyl T-resin, a silanol, a fumed silica surface, and / or a surface of another ingredient such as a pigment.
[0239] In some such embodiments, the coating composition may include an amount of ethyl T-resin in the following range: about 2.0 wt% to about 3.5 wt%, about 2.2 wt% to about 3.3 wt%, about 2.4 wt% to about 3.1 wt%, about 2.5 wt% to about 3.0 wt%, or about 2.6 wt% to about 2.9 wt% (e.g., about 2.8 wt%). In some embodiments, the modified coating composition (e.g., a chemically resistant coating composition) may include an amount of ethyl T-resin in the following range: about 2.0 wt% to about 3.5 wt%, about 2.2 wt% to about 3.3 wt%, about 2.4 wt% to about 3.1 wt%, about 2.5 wt% to about 3.0 wt%, or about 2.6 wt% to about 2.9 wt% (e.g., about 2.7 wt%). Applicants believe that the level of ethyl T-resin in the cured coating can improve the performance and / or durability of the coating. In some embodiments, the amount of ethyl T-resin in the modified coating composition may be less than about 5 wt % and / or greater than about 1.5 wt % (e.g., an amount ranging from about 1.9 wt % to about 3.3 wt % (e.g., about 2.6 wt % to about 2.9 wt %)).
[0240] Some embodiments of the coating compositions previously described herein may include one or more pigments (e.g., one or more black pigments, such as transition-metal ferrite spinel powder) in an amount ranging from about 0.01 wt% to about 15 wt%. In some embodiments of the modified coating compositions, relative to the coating compositions previously described herein, the amount of pigment (e.g., black pigment) may be replaced with one or more blue pigments in an amount ranging from about one to about fifteen times the amount of black pigment, from about three times to about fifteen times the amount of black pigment, from about five times to about fifteen times the amount of black pigment, from about eight times to about fourteen times the amount of black pigment, or from about ten times to about twelve times the amount of black pigment. In some embodiments, the blue pigment may be included in an amount ranging from about 1.0 wt% to about 5.0 wt%, from about 1.5 wt% to about 4.5 wt%, from about 2.0 wt% to about 4.5 wt%, from about 2.5 wt% to about 4.0 wt%, from about 3.0 wt% to about 4.0 wt%, from about 3.5 wt% to about 4.0 wt%, or from about 3.5 wt% to about 3.8 wt% (e.g., about 3.6 wt%). In some embodiments, the blue pigment may include cobalt aluminate blue spinel, Cas# 1345-16-0. Other blue pigments and / or pigments of other colors are contemplated.
[0241] Some embodiments of the coating compositions previously described herein may not contain titanium dioxide or may contain only a relatively small amount (trace amount) of titanium dioxide. In some embodiments of the modified coating composition, titanium dioxide may be included in an amount in the following range: about 0.01 wt% to about 15 wt%, about 1 wt% to about 14 wt%, about 3 wt% to about 12 wt%, about 5 wt% to about 10 wt%, about 6 wt% to about 9 wt%, or about 7 wt% to about 8 wt%. For example, titanium dioxide may be included in an amount in the following range: about 0.50 wt% to about 0.90 wt%, about 0.60 wt% to about 0.85 wt%, about 0.65 wt% to about 0.80 wt%, about 0.70 wt% to about 0.80 wt%, or about 0.70 wt% to about 0.75 wt% (e.g., about 0.72 wt%).
[0242] Relative to some embodiments of the unmodified coating composition previously described herein, applicants believe that for some embodiments of the modified coating composition, the addition of titanium dioxide can increase the durability of the cured coating layer. Applicants also believe that for some embodiments of the modified coating composition, adding additional crosslinking agents (e.g., trifunctional silanes) to the coating composition and / or removing some polymers (e.g., silanol fluids) from the coating composition can promote relatively tighter bonds between the crosslinking agent and the polymer and / or promote additional crosslinking between the blue pigment and the titanium dioxide. For some embodiments, applicants also believe that relatively tighter bonds may reduce the permeability of the coating layer, which may reduce the sensitivity of the coating layer to attack by solvents and / or other chemicals to which oilfield operating components may be exposed.
[0243] Samples A to D were tested at an impact angle of 0°. Samples E to H were tested at an impact angle of 30°. Samples I and J were tested at an impact angle of 45°, and samples K and L were tested at an impact angle of 60°. The test results are provided in Table 4 below, showing the cumulative mass loss (grams (g)) and cumulative wear depth (inches (in)) as a function of the time the samples were subjected to the test. Fig.10 is a graph of cumulative wear depth (inches (in)) versus test time (hours (hr)) during which the samples were subjected to the test results shown in Table 4.
[0244] Table 4
[0245]
[0246]
[0247]
[0248] like Fig.10 As shown, for AISI 4130 alloy steel, which is consistent with the material commonly used in goat heads, the cumulative wear depth of each of the bare test samples is significantly greater (regardless of the impact angle) compared to the cumulative wear depth of the coated test samples, regardless of the coating thickness or whether the coating is a modified coating (i.e., a chemically resistant coating). In addition, as Figure 4As shown, the cumulative mass loss of each bare test sample in the bare test samples was significantly greater (regardless of the impact angle) compared to the cumulative mass loss of the coated test samples, regardless of the coating thickness or whether the coating was a modified coating. In addition, the coated test samples did not show any significant wear depth or mass loss before two hours of testing (i.e., about 400 pounds of sand grains passed through), and for the 60° angle, no significant mass loss occurred until four hours of testing (i.e., about 800 pounds of sand grains had passed through). (For each four hours of testing, the test samples were subjected to approximately 200 pounds of sand grain erosive agent.) As would be generally expected, the amount of mass loss decreases with increasing impact angle, such as making the mass loss at 60° significantly less than the mass loss at 0° for a given test time or sand grain passing through. The test results indicate that the tested primer and coating layers can significantly increase the service life of fluid handling components used in oilfield operations, such as goat heads associated with fracturing systems.
[0249] In addition, if Fig.10 As shown, the bare samples (samples A, E, I and K) all reached a wear depth of 0.014 inches within two hours of testing or less. In contrast, coated sample F, which exhibited the fastest wear rate of the coated samples, only reached a wear depth of 0.014 inches after eight hours of testing, a four-fold decrease in wear rate. In addition, samples C and G, which contained thick coatings (0.028 inches), did not reach a wear depth of 0.014 inches until sixteen and twenty hours of testing, respectively. Comparing coated samples B and F containing a 0.014-inch thick coating layer with coated samples C and G containing a 0.028-inch thick coating layer, samples C and G reached a wear depth of 0.140 inches twice as long as samples B and F. Regarding samples D and H containing a chemically resistant coating layer (0.014 inches thick), samples D and H did not reach a wear depth of 0.014 inches until sixteen hours of testing. Sample B, tested at an impact angle of 0 degrees and having a coating thickness of .014 inches, exhibited a wear depth of 0.014 inches in a little more than half the time (ten hours) of Sample D (seventeen hours), which was tested at an impact angle of 0 degrees and had a 0.014 inch thick chemical resistant coating. Sample F, tested at an impact angle of 30 degrees and having a coating thickness of .014 inches, exhibited a wear depth of 0.014 inches in about half the time (slightly more than eight hours) of Sample H, which was tested at an impact angle of 30 degrees and had a 0.014 inch thick chemical resistant coating.
[0250] For stainless steel 17-4PH, which is commonly used for flow ends, fifteen tests were performed with test samples, which included eight test samples (i.e., samples O, P, S, T, W, X, AA, and BB) coated with a coating composition consistent with at least some examples described herein and seven uncoated (bare) test samples. In addition, four of the test samples were subjected to relatively large 100-mesh sand grains (i.e., samples P, T, X, and BB), and four test samples were subjected to relatively small 270-mesh sand grains (i.e., samples O, S, W, and AA). Samples M to P were tested at an impact angle of 0 °. Samples Q to T were tested at an impact angle of 30 °. Samples U and X were tested at an impact angle of 45 °, and samples Y and BB were tested at an impact angle of 60 °. Test results are provided in Table 5 below, showing the cumulative mass loss (grams (g)) and cumulative wear depth (inches (in)) as the sample was subjected to the time variation of the test. Fig.11 is a graph of cumulative wear depth (inches (in)) versus test time (hours (hr)) during which the samples were subjected to the test results shown in Table 5.
[0251] Table 5
[0252]
[0253]
[0254]
[0255] like Fig.11 As shown, for stainless steel 17-4PH, which is consistent with materials commonly used in fluid ends, the cumulative wear depth of each of the uncoated (bare) test samples was significantly greater (regardless of the impact angle) compared to the cumulative wear depth of the coated test samples, regardless of the grit size (i.e., relatively large 100 mesh grit or relatively small 270 mesh grit). For example, the worst performing coated sample (Sample W) took three times longer to reach a wear depth of 0.014 inches compared to the best performing uncoated sample (Sample V). The best performing coated samples (Samples R, T, and X) took ten to eleven times longer to reach a wear depth of 0.014 inches. Fig.11 It was also shown that when exposed to relatively larger grit (100 mesh grit), generally all samples (uncoated and coated) exhibited better wear (i.e., slower wear rates) than relatively smaller grit (270 mesh grit). Fig.11 The thicker line in the figure shows data for relatively smaller sand particles).
[0256] In addition, if Figure 5As shown, the cumulative mass loss of each bare test sample in the uncoated test samples was significantly greater (regardless of the impact angle) compared to the cumulative mass loss of the coated test samples, regardless of the grit size. The coated test samples did not show any significant wear depth or mass loss before two hours of testing (i.e., about 400 pounds of grit had passed through), and for the 60° angle, no significant mass loss occurred until four hours of testing (i.e., about 800 pounds of grit had passed through). (For each four hours of testing, the test samples were subjected to approximately 200 pounds of grit erosive agent.) As would be generally expected, the amount of mass loss decreases with increasing impact angle, such that for a given test time or grit pass through, the mass loss at 60° is significantly less than the mass loss at 0°. Additionally, as Fig.11 As shown, the bare samples (Samples M, N, Q, R, U, V, and Z) all reached a wear depth of 0.014 inches in two hours or less of testing time. In contrast, coated sample W, which exhibited the fastest wear rate of the coated samples, only reached a wear depth of 0.014 inches after six hours of testing, a three-fold decrease in wear rate. The test results show that the tested primer and coating layers can significantly increase the service life of fluid handling components used in oilfield operations, such as fluid ends associated with fracturing systems.
[0257] For AISI 4715 alloy steel, which is commonly used in fracturing iron, eight tests were conducted with test samples comprising four test samples (i.e., samples DD, FF, HH, and JJ) coated with a 0.014 inch thick coating layer and four bare (uncoated) test samples, wherein the coating layer comprises a coating composition consistent with at least some examples described herein. Samples CC and DD were tested at an impact angle of 0°. Samples EE and FF were tested at an impact angle of 30°. Samples GG and HH were tested at an impact angle of 45°, and samples II and JJ were tested at an impact angle of 60°. The test results are provided in Table 6 below, showing the cumulative mass loss (grams (g)) and cumulative wear depth (inches (in)) as a function of the time the samples were subjected to the test. Fig.12 is a graph of cumulative wear depth (inches (in)) versus test time (hours (hr)) during which the samples were subjected to the test results shown in Table 6.
[0258] Table 6
[0259]
[0260]
[0261] like Fig.12As shown, for AISI 4715 alloy steel, which is consistent with materials commonly used in fracturing iron, the cumulative wear depth of each of the uncoated (bare) test samples was significantly greater than the cumulative wear depth of the coated test samples (regardless of the impact angle). For example, the worst performing coated sample (sample DD with an impact angle of 0 degrees) took three times longer to reach a wear depth of 0.014 inches compared to the uncoated sample CC with an impact angle of 0 degrees. The best performing coated samples (samples FF, HH, and JJ) took four to eight times longer to reach a wear depth of 0.014 inches compared to the uncoated sample.
[0262] In addition, if Figure 6 As shown, the cumulative mass loss of each bare test sample in the uncoated test samples is significantly greater (regardless of the impact angle) than the cumulative mass loss of the coated test samples. Fig.12 As shown, the coated test sample did not show any significant wear depth (or mass loss) before two hours of testing (i.e., about 400 pounds of grit had penetrated), and for the 60° angle, no significant mass loss occurred until after sixteen hours of testing (i.e., about 800 pounds of grit had penetrated). (For every four hours of testing, the test sample was subjected to approximately 200 pounds of grit erosive.) In addition, as Figure 8 As shown, the bare samples (samples CC, EE, GG, and II) all reached a wear depth of 0.014 inches within two to four hours of testing. In contrast, coated sample DD, which exhibited the fastest wear rate of the coated samples, only reached a wear depth of 0.014 inches after six hours of testing. The test results indicate that the tested primer and coating layers can significantly increase the service life of fluid handling components used in oilfield operations, such as frac iron components associated with fracturing systems.
[0263] Fig.13 is a graph of cumulative mass loss (grams (g)) versus time (hours (hr)) exposed to a test fluid stream for uncoated (bare) test samples and coated test samples tested in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid stream at an impingement angle of zero degrees. Fig.13 As shown, while the uncoated (bare) samples (Samples A, M, and C corresponding to goat head, fluid end, and frac iron, respectively) began to lose mass almost immediately during the test, the coated samples (Samples B, O, and DD corresponding to goat head, fluid end, and frac iron, respectively) did not begin to lose mass until after four hours of testing, and Sample B did not begin to lose mass until after eight hours of testing.
[0264] Fig.14is a graph of cumulative mass loss (grams (g)) versus time (hours (hr)) exposed to a test fluid stream for uncoated (bare) and coated test samples tested in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid stream at an impingement angle of thirty degrees. Fig.14 As shown, the uncoated (bare) samples (samples E, Q, and EE corresponding to the goat head, fluid end, and frac iron, respectively) began to lose mass almost immediately during the test. In contrast, the coated samples (samples F, S, and FF corresponding to the goat head, fluid end, and frac iron, respectively) did not begin to lose mass until eight hours into the test.
[0265] Fig.15 is a graph of cumulative mass loss (grams (g)) versus time (hours (hr)) exposed to a test fluid stream for uncoated (bare) and coated test samples tested in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid stream at an impingement angle of 45 degrees. Fig.15 As shown, the uncoated (bare) samples (Samples I, U, and GG corresponding to the goat head, fluid end, and frac iron, respectively) began to lose mass almost immediately during the test. In contrast, the coated samples (Samples J, W, and HH corresponding to the goat head, fluid end, and frac iron, respectively) did not begin to lose mass until after eight hours, four hours, and sixteen hours of testing, respectively.
[0266] Fig.16 is a graph of cumulative mass loss (grams (g)) versus time (hours (hr)) exposed to a test fluid stream for uncoated (bare) and coated test samples tested in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid stream at an impingement angle of sixty degrees. Fig.16 As shown, the uncoated (bare) samples (Samples K, Y, and II corresponding to the goat head, fluid end, and frac iron, respectively) began to lose mass almost immediately during the test. In contrast, the coated samples (Samples L, AA, and JJ corresponding to the goat head, fluid end, and frac iron, respectively) did not begin to lose mass until sixteen hours, eight hours, and sixteen hours of testing, respectively.
[0267] Fig.17 is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid stream for test results of uncoated (bare) test specimens and coated test specimens tested in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid stream at an impingement angle of zero degrees. Fig.17As shown, the uncoated (bare) samples (Samples A, M, and CC corresponding to the goat head, fluid end, and frac iron, respectively) reached a wear depth of 0.014 inches within two hours or less of the start of the test. In contrast, the coated samples (Samples BB, O, and DD corresponding to the goat head, fluid end, and frac iron, respectively) did not reach a wear depth of 0.014 inches until ten hours, eight and a half hours, and six and a half hours of testing, respectively.
[0268] Fig.18 is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid stream for test results of uncoated (bare) test specimens and coated test specimens tested in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid stream at a thirty degree angle of impact. Fig.18 As shown, the uncoated (bare) samples (Samples E, Q, and EE corresponding to the goat head, fluid end, and frac iron, respectively) reached a wear depth of 0.014 inches within two hours or less of the start of the test. In contrast, the coated samples (Samples F, S, and FF corresponding to the goat head, fluid end, and frac iron, respectively) did not reach a wear depth of 0.014 inches until about nine hours into the test, representing a more than four-fold reduction in wear rate.
[0269] Fig.19 is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid stream for test results of uncoated (bare) test specimens and coated test specimens tested in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid stream at a forty-five degree angle of impact. Fig.19 As shown, the uncoated (bare) samples (Samples I, U, and GG corresponding to the goat head, fluid end, and frac iron, respectively) reached a wear depth of 0.014 inches within about two hours or less of the start of the test. In contrast, the coated samples (Samples J, W, and HH corresponding to the goat head, fluid end, and frac iron, respectively) did not reach a wear depth of 0.014 inches until about six hours, nine and a half hours, and about seventeen hours after testing, respectively.
[0270] Fig. 20 is a graph of cumulative wear depth (inches (in)) versus time (hours (hr)) exposed to a test fluid stream for test results of uncoated (bare) test specimens and coated test specimens tested in accordance with the present disclosure, simulating a goat head, fluid end, and frac iron exposed to a fluid stream at a sixty degree angle of impact. Fig. 20As shown, the uncoated (bare) samples (Samples K, Y, and II corresponding to the goat head, fluid end, and frac iron, respectively) reached a wear depth of 0.014 inches within about one and a half hours (Samples K and Y) or about four hours (Sample II) of the start of the test. In contrast, the coated samples (Samples L, AA, and JJ corresponding to the goat head, fluid end, and frac iron, respectively) did not reach a wear depth of 0.014 inches until about seventeen hours, about nine and a half hours, and about sixteen and a half hours of testing, respectively.
[0271] Fig.21 is a bar graph showing estimated hours of wear depth relative to an uncoated (bare) sample and a coated sample of 0.014 inches, simulating a goat head, fluid end, and frac iron exposed to fluid flow at different impact angles and each of two grit sizes (relatively small 270 mesh grit and relatively large 100 mesh grit) in accordance with the present disclosure. Additionally, Fig.21 An example comparison factor is also shown. For example, the comparison factor can indicate a first amount of time for the coating to wear to a first depth divided by a second amount of time for the fluid treatment component to wear to the first depth without the coating. For example, the comparison factor can indicate a level of wear improvement provided to each of the test samples by a 0.014 inch thick layer of coating comprising a coating composition consistent with at least some examples described herein relative to the uncoated test sample.
[0272] like Figure 10-20 As shown, a plot of the wear depth and mass loss of the test samples shows very similar slopes after the paint layer is penetrated and the sand particles begin to impact the bare metal underneath. In order to compare the relative wear resistance of the uncoated and coated test samples, the time to penetrate the paint layer was estimated in one of two ways. First, the mass loss data was used to estimate the estimated time to penetration. For the uncoated metal, the mass loss slope for the initial four-hour window was determined. For the coated samples, the measurable mass loss was negligible until penetration occurred. After this time point, the next mass measurement at the four-hour interval was significantly larger, and penetration was observed visually during inspection. The uncoated test sample slope was used to extrapolate backward from the first point after penetration to find the x intercept point on the graph, and the time corresponding to the x intercept point was identified as representing the approximate penetration time based on mass loss. Secondly, the wear depth data was used to estimate the estimated time to penetration. The wear depth of the test samples was measured. Before the paint penetrated, the wear depth indicated the loss in paint thickness (0.014 inches), which was Figure 10-12 The slope of the uncoated test sample graph is used to extrapolate backward from the wear depth measured on the graph after penetrating the coating layer to estimate the intercept point where the wear depth is equal to 0.014 inches (see, for example, Figure 10-12and 17-20). The time corresponding to the intercept point is used as the estimated time to penetrate the coating layer based on the wear depth. If, for a given test sample, the estimated penetration time calculated based on mass loss is different from the estimated penetration time calculated based on the wear depth, the two values are averaged to determine a single penetration time for the test sample.
[0273] After calculating the penetration time for each of the coated samples, the relative erosion resistance between the coated and uncoated samples was calculated. Linear interpolation was performed along the uncoated test sample wear depth line to calculate the wear time through the 0.014-inch uncoated metal test sample. To determine the comparison factor for the coating, the penetration time of the coating layer was divided by the time for the corresponding uncoated test sample to reach a wear depth of 0.014 inches. Fig.21 As shown, the comparison factor ranges from about 3.0 to about 17.5, which indicates the level of improvement in abrasion resistance provided by the coating layer.
[0274] For example, Fig.21 As shown, for a simulated goat head material at a zero impact angle and 270 grit, the coated test sample required 7.1 times longer to reach a wear depth of 0.014 inches (e.g., corresponding to a comparison factor of 7.1) than the uncoated test sample. In another example, Fig.21 As shown, for a simulated goat head material at a forty-five degree impact angle and 100 grit grit, the coated test sample required 17.0 times longer to reach a wear depth of 0.014 inches compared to the uncoated test sample (e.g., corresponding to a comparison factor of 17.0). For a simulated fluid end material at a zero degree impact angle and 270 grit grit, the coated test sample required 5.5 times longer to reach a wear depth of 0.014 inches compared to the uncoated test sample (e.g., corresponding to a comparison factor of 5.5). In another example, Fig.21 As shown, for the fluid end material simulated at a sixty degree impact angle and 100 mesh grit, the coated test sample required 11.8 times longer to reach a wear depth of 0.014 inches compared to the uncoated test sample (e.g., corresponding to a comparison factor of 11.8). For the fractured iron material simulated at a forty-five degree impact angle and 100 mesh grit, the coated test sample required 17.2 times longer to reach a wear depth of 0.014 inches compared to the uncoated test sample (e.g., corresponding to a comparison factor of 17.2). With an example comparison factor ranging from a minimum of about 3.0 to a maximum of about 17.5, the coating layer exhibited a significant improvement in the wear resistance of the test sample.
[0275] Fig. 22is a bar graph showing estimated hours of wear depth of 0.014 inches for simulated goat head material according to the present disclosure relative to a bare sample, a sample with a coating depth of 0.014 inches (“Coated”), a sample with a coating depth of 0.028 inches (“Thick Coated”), and a sample coated with a chemically resistant coating (“Chemically Resistant”), simulating a goat head exposed to fluid flow at zero degrees and thirty degrees and at each of two grit sizes (270 mesh and larger 100 mesh). Fig. 22 Also similar to Fig.21 The comparison factor for each of the test samples is shown in a manner. For example, at a zero-degree impact angle and 270-mesh grit, the coated test sample takes 7.1 times longer to reach a wear depth of 0.014 inches compared to the uncoated test sample (e.g., corresponding to a comparison factor of 7.1). At a zero-degree impact angle and 270-mesh grit, the thick-coated test sample takes 8.8 times longer to reach a wear depth of 0.014 inches compared to the uncoated test sample (e.g., corresponding to a comparison factor of 8.8). At a zero-degree impact angle and 270-mesh grit, the chemically resistant coated test sample takes 12.3 times longer to reach a wear depth of 0.014 inches compared to the uncoated test sample (e.g., corresponding to a comparison factor of 12.3). At a zero-degree impact angle and 100-mesh grit, the chemically resistant coated test sample takes 10.6 times longer to reach a wear depth of 0.014 inches compared to the uncoated test sample (e.g., corresponding to a comparison factor of 10.6). At a thirty degree impact angle and 100 grit, the chemically resistant coated test sample required 28.2 times longer to reach a wear depth of 0.014 inches compared to the uncoated test sample (e.g., corresponding to a comparison factor of 28.2). Fig. 22 As shown, the comparison factor ranges from a minimum of about 6.0 to a maximum of about 28.5, and the coating layer exhibits a significant improvement in the abrasion resistance of the test samples.
[0276] Oilfield components such as fluid ends are sometimes formed of carbon steel, and recently some fluid end manufacturers have switched to stainless steel, which in some cases can provide a longer service life compared to fluid ends formed of carbon steel. Sometimes, a fluid end formed of stainless steel can have up to twice the service life compared to a similar fluid end formed of carbon steel. Historically, stainless steel tends to be more expensive than carbon steel, sometimes twice as expensive. Coating compositions, coating layers, and / or related methods consistent with at least some of those described herein can be used with oilfield components (e.g., fluid ends) formed of carbon steel to achieve a service life approaching or exceeding that of similar oilfield components formed of stainless steel. Therefore, at least some of the examples described herein can be able to reduce the costs associated with purchase, maintenance, production downtime, and / or replacement costs associated with oilfield components and oilfield operations.
[0277] Having now described some illustrative embodiments of the present disclosure, it should be apparent to those skilled in the art that the foregoing is merely illustrative and not restrictive, and is presented only by way of example. Many modifications and other embodiments are within the scope of those of ordinary skill in the art and are considered to fall within the scope of the present disclosure. Specifically, although many of the examples presented herein relate to specific combinations of method actions or system elements, it should be understood that those actions and those elements can be combined in other ways to achieve the same goals. It should be understood by those skilled in the art that the parameters and configurations described herein are exemplary, and that actual parameters and / or configurations will depend on the specific application of the system, method and / or aspect or technology of the present disclosure. It should also be recognized by those skilled in the art or can be determined using only routine experiments, the equivalent forms of the specific embodiments of the present disclosure. Therefore, it should be understood that the embodiments described herein are introduced only by way of example, and within the scope of any appended claims and their equivalents, the present disclosure can be practiced in a manner different from the specific description.
[0278] This PCT application claims priority to and the benefit of U.S. Provisional Application No. 63 / 008,035, filed on April 10, 2020, entitled “COATING COMPOSITIONS, COATED OILFIELD OPERATIONAL COMPONENTS, AND RELATED METHODS FOR OILFIELD OPERATIONS”; U.S. Provisional Application No. 63 / 008,038, filed on April 10, 2020, entitled “METHODS FOR PROTECTING OILFIELD OPERATIONAL COMPONENTS FROM DAMAGE FROM FLUID Flow”; and U.S. Provisional Application No. 63 / 008,039, filed on April 10, 2020, entitled “COATING AND METHODS FOR EXTENDING SERVICE LIFE OF OILFIELD OPERATIONAL COMPONENTS”. U.S. Provisional Application No. 63 / 008,042, filed on April 10, 2020, entitled “METHODS FOR PREPARING COATING COMPOSITIONS FOR PROTECTING OILFIELDOPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 008,046, filed on April 10, 2020, entitled “METHODS FOR PROVIDING FLEXIBLE AND / OR ELASTIC COATINGS ON OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 008,049, filed on April 10, 2020, entitled “METHODS FOR PROVIDING FLEXIBLE AND / OR ELASTIC COATINGS ON OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 008,050, filed on August 14, 2020, entitled “COATED OILFIELD OPERATIONAL COMPONENTS AND METHODS FOR PROTECTING AND EXTENDING THE SERVICE OF OILFIELD OPERATIONAL COMPONENTS AND METHODS FOR PROTECTING AND EXTENDING THE SERVICE LIFE OF OILFIELD OPERATIONAL COMPONENTS);U.S. Provisional Application No. 63 / 065,545, filed on August 14, 2020, entitled “METHODS FOR PROTECTING OILFIELD OPERATIONAL COMPONENTS FROM DAMAGE FROM FLUID Flow”; U.S. Provisional Application No. 63 / 065,565, filed on August 14, 2020, entitled “COATING AND METHODS FOR EXTENDING SERVICE LIFE OF OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 065,565, filed on August 14, 2020, entitled “METHODS FOR PREPARING COATING COMPOSITIONS FOR PROTECTING OILFIELD OPERATIONAL COMPONENTS U.S. Provisional Application No. 63 / 065,577, filed on August 14, 2020, entitled “METHODS FOR PROVIDING FLEXIBLE AND / OR ELASTIC COATINGS ON OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 065,591, filed on August 14, 2020, entitled “METHODS FOR PROVIDING FLEXIBLE AND / OR ELASTIC COATINGS ON OILFIELD OPERATIONAL COMPONENTS”; U.S. Provisional Application No. 63 / 198,044, filed on September 25, 2020, entitled “COATED OILFIELDOPERATIONAL COMPONENTS AND METHODS FOR PROTECTING AND EXTENDING THE SERVICELIFE OF OILFIELD OPERATIONAL COMPONENTS”;and U.S. Non-Provisional Application No. 17 / 225,543, filed on April 8, 2021, entitled “COATED OILFIELD OPERATIONAL COMPONENTS AND METHODS FOR PROTECTING AND EXTENDING THE SERVICE LIFE OF OILFIELD OPERATIONAL COMPONENTS,” the disclosures of all of which are incorporated herein by reference in their entirety. ;
[0279] Furthermore, the scope of the present disclosure should be interpreted to cover various modifications, combinations, additions, variations, etc. of the above-described and previously described embodiments, which should be considered within the scope of the present disclosure. Therefore, the various features and characteristics as discussed herein may be selectively interchanged and applied to other illustrated and unillustrated embodiments, and many further changes, modifications, and additions may be made thereto without departing from the spirit or scope of the present disclosure as set forth in the appended claims.
Claims
1. A method for protecting an operating component exposed to a fluid flow, the method comprising: applying a primer composition to the operating component; at least partially curing the primer composition to form a primer layer such that the primer layer is at least partially mechanically bonded to the operating component; applying a coating composition to the primer layer, the coating composition comprising a trifunctional silane, a silanol fluid, a filler, and titanium dioxide; as well as The coating composition is at least partially cured to form a coating layer such that the coating layer at least partially chemically bonds with the primer layer to enhance the wear resistance of the operating component, the coating composition comprising T-resin units, each of the T-resin units forming one or more bonds with one or more of the other T-resin units, the silanol fluid, the filler, or the titanium dioxide, such that the operating component exhibits a comparison factor indicative of increased wear resistance of greater than about 2, the comparison factor indicating a first amount of time for a portion of the one or more coating layers or the primer layers to be worn to a first depth divided by a second amount of time for a portion of the operating component to be worn to a second depth equal to the first depth in the absence of the one or more coating layers or the primer layers.
2. The method of claim 1, wherein the coating composition further comprises one or more pigments, and the T-resin unit forms two or more bonds with the one or more pigments and one or more of other T-resin units, silanol fluid, titanium dioxide, or fillers.
3. The method of claim 1, wherein applying the primer composition to the operational component comprises applying the primer composition to at least a portion of an oilfield operational component, and wherein the comparison factor ranges from about 5 to about 30.
4. A method for protecting an operating component exposed to a fluid flow, the method comprising: spraying the primer composition onto the operating component via a spray head, the spray head being configured to atomize the primer composition when the primer composition is applied to the operating component; at least partially curing the primer composition to form a primer layer such that the primer layer is at least partially mechanically bonded to the operating component; spraying a coating composition onto the primer layer, the coating composition comprising a trifunctional silane, a silanol fluid, a filler and titanium dioxide; as well as The coating composition is at least partially cured to form a coating layer such that the coating layer at least partially chemically bonds with the primer layer to enhance the wear resistance of the operating component, the coating composition comprising T-resin units, each of the T-resin units forming one or more bonds with one or more of the other T-resin units, the silanol fluid, the filler, or the titanium dioxide such that the operating component exhibits a comparison factor indicative of increased wear resistance, the comparison factor being indicative of a first amount of time for a portion of the one or more coating layers or the primer layers to be worn to a first depth divided by a second amount of time for a portion of the operating component to be worn to a second depth equal to the first depth in the absence of the one or more coating layers or the primer layers.
5. The method according to claim 4, wherein spraying the coating composition onto the operating component through the spray head comprises: pumping the coating composition via an airless pump at an output ratio ranging from about 40:1 to about 80:1 to a spray head configured to rotate and atomize the coating composition; as well as While the coating composition is atomized and sprayed from the spray head, air is supplied to the spray head to rotate the spray head.
6. The method of claim 4, further comprising spraying the coating composition onto the coating layer to form a second coating layer and at least partially drying the second coating layer.
7. A method for protecting a component, the method comprising: applying a primer composition to the component; at least partially curing the primer composition to form a primer layer such that the primer layer is at least partially mechanically bonded to the component; applying a coating composition to the primer layer, the coating composition comprising a trifunctional silane, a silanol fluid, a filler, and titanium dioxide; as well as The coating composition is at least partially cured to form a coating layer and to at least partially chemically bond the coating layer to the primer layer to enhance the wear resistance of the component, the coating composition comprising T-resin units, each of the T-resin units forming one or more bonds with one or more of other T-resin units, silanol fluid, filler, or the titanium dioxide, such that the component exhibits a comparison factor indicative of increased wear resistance of greater than about 2, the comparison factor indicating a first amount of time for a portion of the one or more coating layers or the primer layers to be worn to a first depth divided by a second amount of time for a portion of the component to be worn to a second depth equal to the first depth in the absence of the one or more coating layers or the primer layers.
8. The method of claim 7, wherein the T-resin unit forms two or more bonds with one or more of other T-resin units, silanol fluid, titanium dioxide, or filler.
9. The method of claim 7, wherein applying the primer composition to the component comprises applying the primer composition to at least a portion of the component, and wherein the comparison factor ranges from about 5 to about 30.
10. A method for protecting a component, the method comprising: spraying a primer composition onto the component via a spray head, the spray head being configured to atomize the primer composition as it is applied to the component; at least partially curing the primer composition to form a primer layer such that the primer layer is at least partially mechanically bonded to the component; spraying a coating composition onto the primer layer, the coating composition comprising a trifunctional silane, a silanol fluid, a filler and titanium dioxide; as well as The coating composition is at least partially cured to form a coating layer, such that the coating layer at least partially chemically bonds with the primer layer to enhance the wear resistance of the component, the coating composition comprising T-resin units, each of the T-resin units forming one or more bonds with one or more of other T-resin units, silanol fluid, filler, or the titanium dioxide, and such that the component exhibits a comparison factor indicative of increased wear resistance, the comparison factor indicating a first amount of time for a portion of the one or more coating layers or primer layers to be worn to a first depth divided by a second amount of time for a portion of the component to be worn to a second depth equal to the first depth in the absence of the one or more coating layers or primer layers.
11. The method of claim 10, wherein spraying the coating composition onto the component through the spray head comprises: pumping the coating composition via an airless pump at an output ratio ranging from about 40:1 to about 80:1 to a spray head configured to rotate and atomize the coating composition; as well as While the coating composition is atomized and sprayed from the spray head, air is supplied to the spray head to rotate the spray head.
12. The method of claim 10, further comprising spraying the coating composition onto the coating layer to form a second coating layer and at least partially drying the second coating layer.
13. A method of coating a component, the method comprising: applying a primer composition to the component; at least partially curing the primer composition to form a primer layer such that the primer layer is at least partially mechanically bonded to the component; applying a coating composition to the primer layer, the coating composition comprising a trifunctional silane, a silanol fluid, a filler, and titanium dioxide; as well as The coating composition is at least partially cured to form a coating layer and to at least partially bond the coating layer to the primer layer to enhance the wear resistance of the component, the coating composition comprising T-resin units, each of the T-resin units being bonded to one or more of other T-resin units, silanol fluid, filler, or the titanium dioxide, such that the component exhibits a comparison factor indicative of increased wear resistance of greater than about 2, the comparison factor indicating a first amount of time for a portion of the one or more (a) the coating layer or (b) the primer layer to be worn to a first depth divided by a second amount of time for a portion of the component to be worn to a second depth equal to the first depth in the absence of the one or more (a) the coating layer or (b) the primer layer.
14. The method of claim 13, wherein the T-resin unit comprises two or more bonds to one or more of other T-resin units, silanol fluid, or titanium dioxide.
15. The method of claim 13, wherein applying the primer composition to the component comprises applying the primer composition to at least a portion of the component, and wherein the comparison factor ranges from about 5 to about 30.
16. A method of coating a component, the method comprising: spraying a primer composition onto the component via a spray head, the spray head being configured to atomize the primer composition as it is applied to the component; at least partially curing the primer composition to form a primer layer such that the primer layer is at least partially mechanically bonded to the component; spraying a coating composition onto the primer layer, the coating composition comprising a trifunctional silane, a silanol fluid and titanium dioxide; as well as The coating composition is at least partially cured to form a coating layer, such that the coating layer is at least partially chemically bonded to the primer layer to enhance the wear resistance of the component, the coating composition comprising T-resin units, each of the T-resin units being bonded to one or more of other T-resin units, silanol fluid, filler, or the titanium dioxide, and such that the component exhibits a comparison factor indicative of increased wear resistance, the comparison factor being indicative of a first amount of time for a portion of one or more of the coating layers or the primer layers to be worn to a first depth divided by a second amount of time for a portion of the component to be worn to a second depth equal to the first depth in the absence of the one or more of the coating layers or the primer layers.
17. The method of claim 16, wherein spraying the coating composition onto the component through the spray head comprises: pumping the coating composition via an airless pump at an output ratio ranging from about 40:1 to about 80:1 to a spray head configured to rotate and atomize the coating composition; as well as While the coating composition is atomized and sprayed from the spray head, air is supplied to the spray head to rotate the spray head.
18. The method of claim 16, further comprising spraying the coating composition onto the coating layer to form a second coating layer and at least partially drying the second coating layer.
19. A method of coating a component, the method comprising: applying a primer composition to the component; at least partially curing the primer composition to form a primer layer such that the primer layer is at least partially mechanically bonded to the component; applying a coating composition to the primer layer, the coating composition comprising a trifunctional silane, a silanol fluid, or a filler; as well as The coating composition is at least partially cured to form a coating layer, such that the coating layer is at least partially bonded to the primer layer to enhance the wear resistance of the component, the coating composition comprising T-resin units, each of the T-resin units being bonded to one or more of other T-resin units, silanol fluid, filler, or the one or more pigments, and such that the component exhibits a comparison factor indicative of increased wear resistance of greater than about 2, the comparison factor indicating a first amount of time for a portion of the one or more coating layers or primer layers to be worn to a first depth divided by a second amount of time for a portion of the component to be worn to a second depth equal to the first depth in the absence of the one or more coating layers or primer layers.
20. A method of coating a component, the method comprising: spraying a primer composition onto the component via a spray head, the spray head being configured to atomize the primer composition as it is applied to the component; at least partially curing the primer composition to form a primer layer such that the primer layer is at least partially mechanically bonded to the component; Spraying a coating composition onto the primer layer, the coating composition comprising a trifunctional silane, a silanol fluid, and a filler, the coating composition being sprayed onto the component comprising: (a) pumping the coating composition to a spray head at an output ratio ranging from about 40:1 to about 80:1 via an airless pump, the spray head being configured to rotate and atomize the coating composition; and (b) supplying air to the spray head to rotate the spray head while the coating composition is atomized and sprayed from the spray head; and The coating composition is at least partially cured to form a coating layer, such that the coating layer is at least partially bonded to the primer layer to enhance the wear resistance of the component, the coating composition comprising T-resin units, each of the T-resin units being bonded to one or more of the other T-resin units, the silanol fluid, or the filler, and such that the component exhibits a comparison factor indicative of increased wear resistance, the comparison factor being indicative of a first amount of time for a portion of one or more of the coating layers or the primer layers to be worn to a first depth divided by a second amount of time for a portion of the component to be worn to a second depth equal to the first depth in the absence of the one or more of the coating layers or the primer layers.