A method for preparing high-purity trimanganese tetraoxide by water vapor calcination after precipitation and oxidation using manganese chloride as raw material
By using manganese chloride as raw material, combined with the precipitation oxidation and segmented calcination methods of surfactants and catalysts, and using a mixture of air and water vapor for calcination, the problems of low purity and high cost of manganese tetroxide have been solved, and the preparation and industrial production of high-purity manganese tetroxide have been realized.
Patent Information
- Application Number
- CN202411311575.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-09-20
AI Technical Summary
Existing technologies are insufficient to effectively improve the purity of manganese tetroxide, reduce the dependence of raw material purity on price, and suffer from problems such as impurity encapsulation and high costs.
Manganese chloride is used as raw material. After precipitation and oxidation, it is mixed with surfactant and catalyst and then added to react with alkaline solution. Oxidizing gas is then introduced, and after filtration and drying, it is calcined in stages using a mixture of air and water vapor. The calcination temperature and time are controlled.
The preparation of high-purity manganese tetroxide was achieved, with a manganese content of over 71% and low impurity content. The process is simple, suitable for industrial production, and reduces costs.
Smart Images

Figure CN118929761B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of chemical materials technology, specifically to a method for preparing high-purity manganese tetroxide. Background Technology
[0002] Manganese tetroxide (Mn3O4), also known as black manganese ore in nature, has a theoretical manganese content of 72.03%. It is primarily used as a basic raw material in industries such as electronics and new energy power batteries. Mn3O4 products can be divided into electronic grade and battery grade. Electronic grade Mn3O4 is a key raw material for the production of manganese-zinc ferrite, mainly used in transformers, filters, and inductors. Battery grade Mn3O4 is mainly used in manganese-based cathode materials for lithium batteries, including lithium manganese oxide, lithium manganese iron phosphate, and layered oxides for sodium-ion batteries. Besides these main applications, Mn3O4 can also be used in many other fields such as petroleum weighting agents, pigments, and resistors.
[0003] CN109052480A discloses a method for preparing manganese tetroxide. The method involves mixing electrolytic manganese powder with water to form a manganese slurry; adding an ammonium salt solution to the manganese slurry; stirring; and introducing an oxidizing gas to react and prepare manganese tetroxide. This method results in the high cost of manganese tetroxide due to the high price and difficulty in obtaining electrolytic manganese powder, and the significant impact of the purity of the manganese powder on manganese tetroxide. Furthermore, some impurities may be incorporated during the mixed oxidation stage to form manganese tetroxide, and there is no subsequent purification process.
[0004] Therefore, how to further improve the purity of manganese tetroxide, increase the manganese content, reduce impurities, and reduce dependence on the purity of raw materials and price fluctuations, thereby developing a low-cost, simple, readily available, and high-purity synthesis method for manganese tetroxide, is a problem that needs to be solved. Summary of the Invention
[0005] To address the problems existing in the prior art, this invention provides a method for preparing high-purity manganese tetroxide by precipitating and oxidizing manganese chloride and then calcining it with steam. The specific scheme is as follows:
[0006] A method for preparing high-purity manganese tetroxide by precipitating and oxidizing manganese chloride and then calcining it with steam includes the following steps:
[0007] Step 1: Dissolve and mix manganese chloride with the surfactant and catalyst together;
[0008] Step 2: Mix the solution obtained in Step 1 with the alkaline solution in parallel flow and introduce oxidizing gas to carry out the reaction;
[0009] Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide.
[0010] Step 4: Grind the initial product obtained in Step 3 and then perform segmented calcination to obtain purified manganese tetroxide.
[0011] The surfactant used in step one is EDTA-2Na; the catalyst is ammonium chloride; the alkaline solution used in step two is sodium hydroxide solution; the oxidizing gas used in step two is air; and the atmosphere used for calcination in step four is a mixture of air and water vapor.
[0012] In step two, the amount of alkali solution added is 200-300 mL. Preferably, the amount of alkali solution added in step two is 210-250 mL.
[0013] The reaction temperature in step two is 50-100℃. Preferably, the reaction temperature in step two is 70-90℃.
[0014] In step two, air is used as the oxidizing gas.
[0015] The oxidation time in step two is 2-10 hours. Preferably, the oxidation time in step two is 4-8 hours.
[0016] The calcination process in step four consists of two stages: first stage calcination at 500-600℃ for 6-10 hours; and second stage calcination at 900-1000℃ for 4-8 hours.
[0017] In step four, a mixture of air and water vapor is continuously introduced during the calcination process.
[0018] The high-purity manganese tetroxide prepared after purification contains more than 71% Mn.
[0019] This invention features simple operation steps. Manganese chloride is mixed with a surfactant and catalyst, then stirred and mixed concurrently with liquid alkali, and oxidized by introducing air to obtain the initial product, manganese tetroxide. Subsequently, high-purity manganese tetroxide is obtained by high-temperature calcination while maintaining a continuous flow of a mixture of water vapor and air. This method yields high-purity manganese tetroxide with high purity, low impurity content, and good dispersibility.
[0020] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0021] (1) In the precipitation oxidation stage, the present invention adds surfactants and catalysts. When the alkaline solution reacts with the manganese chloride solution, the morphology of the precipitated manganese hydroxide can be controlled, the agglomeration phenomenon can be reduced, the manganese hydroxide precipitate can be oxidized more fully, the particle size of the prepared manganese tetroxide is uniform, and the reaction is promoted, the reaction rate is increased, and the reaction time is reduced.
[0022] (2) In the purification stage, the present invention uses two high-temperature calcination stages to convert unreacted raw materials such as manganese chloride and manganese hydroxide in the initial product into manganese oxides during the first low-temperature calcination stage, thereby avoiding the melting of unreacted raw materials, which could lead to incomplete reaction and potential danger. The second high-temperature calcination stage can further form manganese tetroxide and remove some impurities while shaping the manganese tetroxide.
[0023] (3) In this invention, a mixture of water vapor and air is continuously introduced during the calcination process. The oxygen in the air can help substances that have not yet been converted into manganese tetroxide to be converted into manganese tetroxide. The water vapor can help remove some impurities and reduce the occurrence of sublimation, thereby reducing the impurity content in manganese tetroxide and reducing the loss of manganese tetroxide. The addition of water vapor can reduce the oxygen content in the mixed gas, which can prevent the excessive oxidation of manganese tetroxide during the calcination process to form manganese oxides such as manganese dioxide, resulting in a decrease in manganese content and a decrease in the purity of manganese tetroxide.
[0024] (4) The preparation process of the present invention is simple and easy to operate, and all conditions during the reaction process can be controlled, making it suitable for large-scale industrial production.
[0025] (5) The Mn content in the high-purity manganese tetroxide prepared by this invention is all higher than 71%. Attached Figure Description
[0026] Figure 1 The diagram shows a schematic of the process flow for preparing manganese tetroxide by stepwise precipitation and oxidation using manganese chloride as a raw material according to the present invention. Detailed Implementation
[0027] To illustrate the invention more clearly, the following description, in conjunction with embodiments, further clarifies the invention. However, the scope of protection is not limited to the description provided.
[0028] Comparative Example 1
[0029] Step 1: Add 214g of manganese chloride tetrahydrate, 3.72g of EDTA-2Na, and 2g of ammonium chloride to 1L of water and stir thoroughly until completely dissolved.
[0030] Step 2: Dilute 200ml of 32% alkali solution to 1L and add it to the 2L water base solution at a flow rate of 10mL / min. Stir and mix at 50℃ and 300rpm. Then, oxidize by introducing air at a flow rate of 10L / min for 2 hours.
[0031] Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide.
[0032] Comparative Example 2
[0033] Step 1: Add 214g of manganese chloride tetrahydrate, 3.72g of EDTA-2Na, and 2g of ammonium chloride to 1L of water and stir thoroughly until completely dissolved.
[0034] Step 2: Dilute 220ml of 32% alkali solution to 1L and add it to the bottom solution of 2L water at a flow rate of 10mL / min. Stir and mix at 50℃ and 300rpm. Then, oxidize by passing air through at a flow rate of 10L / min for 2 hours.
[0035] Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide.
[0036] Comparative Example 3
[0037] Step 1: Add 214g of manganese chloride tetrahydrate, 3.72g of EDTA-2Na, and 2g of ammonium chloride to 1L of water and stir thoroughly until completely dissolved.
[0038] Step 2: Dilute 220ml of 32% alkali solution to 1L and add it to the bottom solution of 2L water at a flow rate of 10mL / min. Stir and mix at 50℃ and 300rpm. Then, oxidize by introducing air at a flow rate of 10L / min for 6 hours.
[0039] Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide.
[0040] Comparative Example 4
[0041] Step 1: Add 214g of manganese chloride tetrahydrate, 3.72g of EDTA-2Na, and 2g of ammonium chloride to 1L of water and stir thoroughly until completely dissolved.
[0042] Step 2: Dilute 220ml of 32% alkali solution to 1L and add it to the bottom solution of 2L water at a flow rate of 10mL / min. Stir and mix at 80℃ and 300rpm. Then, oxidize by introducing air at a flow rate of 10L / min for 6 hours.
[0043] Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide.
[0044] Comparative Example 5
[0045] Step 1: Add 214g of manganese chloride tetrahydrate, 3.72g of EDTA-2Na, and 2g of ammonium chloride to 1L of water and stir thoroughly until completely dissolved.
[0046] Step 2: Dilute 220ml of 32% alkali solution to 1L and add it to the bottom solution of 2L water at a flow rate of 10mL / min. Stir and mix at 80℃ and 300rpm. Then, oxidize by introducing air at a flow rate of 10L / min for 6 hours.
[0047] Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide.
[0048] Step 4: Grind the initial product obtained in Step 3 and calcine it. Heat it to 550℃ at a heating rate of 5℃ / min and hold for 8 hours. Then continue heating it to 950℃ at a heating rate of 5℃ / min and hold for 6 hours. Air is continuously introduced throughout the process. Then cool it naturally to room temperature to obtain purified manganese tetroxide.
[0049] Example 1
[0050] Step 1: Add 214g of manganese chloride tetrahydrate, 3.72g of EDTA-2Na, and 2g of ammonium chloride to 1L of water and stir thoroughly until completely dissolved.
[0051] Step 2: Dilute 220ml of 32% alkali solution to 1L and add it to the bottom solution of 2L water at a flow rate of 10mL / min. Stir and mix at 80℃ and 300rpm. Then, oxidize by introducing air at a flow rate of 10L / min for 6 hours.
[0052] Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide.
[0053] Step 4: Grind the initial product obtained in Step 3 and calcine it. Heat it to 500℃ at a heating rate of 5℃ / min and hold for 6 hours. Then continue heating it to 900℃ at a heating rate of 5℃ / min and hold for 4 hours. A mixture of water vapor and air is continuously introduced throughout the process. Then cool it naturally to room temperature to obtain purified manganese tetroxide.
[0054] Example 2
[0055] Step 1: Add 214g of manganese chloride tetrahydrate, 3.72g of EDTA-2Na, and 2g of ammonium chloride to 1L of water and stir thoroughly until completely dissolved.
[0056] Step 2: Dilute 220ml of 32% alkali solution to 1L and add it to the bottom solution of 2L water at a flow rate of 10mL / min. Stir and mix at 80℃ and 300rpm. Then, oxidize by introducing air at a flow rate of 10L / min for 6 hours.
[0057] Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide.
[0058] Step 4: Grind the initial product obtained in Step 3 and calcine it. Heat it to 550℃ at a heating rate of 5℃ / min and hold for 6 hours. Then continue heating it to 950℃ at a heating rate of 5℃ / min and hold for 4 hours. A mixture of water vapor and air is continuously introduced throughout the process. Then cool it naturally to room temperature to obtain purified manganese tetroxide.
[0059] Example 3
[0060] Step 1: Add 214g of manganese chloride tetrahydrate, 3.72g of EDTA-2Na, and 2g of ammonium chloride to 1L of water and stir thoroughly until completely dissolved.
[0061] Step 2: Dilute 220ml of 32% alkali solution to 1L and add it to the bottom solution of 2L water at a flow rate of 10mL / min. Stir and mix at 80℃ and 300rpm. Then, oxidize by introducing air at a flow rate of 10L / min for 6 hours.
[0062] Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide.
[0063] Step 4: Grind the initial product obtained in Step 3 and calcine it. Heat it to 550℃ at a heating rate of 5℃ / min and hold for 8 hours. Then continue heating it to 950℃ at a heating rate of 5℃ / min and hold for 6 hours. A mixture of water vapor and air is continuously introduced throughout the process. Then cool it naturally to room temperature to obtain purified manganese tetroxide.
[0064] Example 4
[0065] Step 1: Add 214g of manganese chloride tetrahydrate, 3.72g of EDTA-2Na, and 2g of ammonium chloride to 1L of water and stir thoroughly until completely dissolved.
[0066] Step 2: Dilute 220ml of 32% alkali solution to 1L and add it to the bottom solution of 2L water at a flow rate of 10mL / min. Stir and mix at 80℃ and 300rpm. Then, oxidize by introducing air at a flow rate of 10L / min for 6 hours.
[0067] Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide.
[0068] Step 4: Grind the initial product obtained in Step 3 and calcine it. Heat it to 600℃ at a heating rate of 5℃ / min and hold for 10 hours. Then continue heating it to 1000℃ at a heating rate of 5℃ / min and hold for 8 hours. A mixture of water vapor and air is continuously introduced throughout the process. Then cool it naturally to room temperature to obtain purified manganese tetroxide.
[0069] The comparative analysis of different experimental results is shown in Table 1.
[0070] Table 1 Comparison of different experimental results
[0071] experiment Mn / % Si / % Mg / % Cl / % <![CDATA[Apparent density / (g / cm 3 )]]> Comparative Example 1 68.72 0.0071 0.0052 0.091 0.77 Comparative Example 2 69.36 0.0068 0.0045 0.085 0.75 Comparative Example 3 70.11 0.0066 0.0046 0.080 0.71 Comparative Example 4 70.54 0.0065 0.0041 0.079 0.73 Comparative Example 5 70.92 0.0051 0.0032 0.067 0.68 Example 1 71.30 0.0037 0.0022 0.022 0.64 Example 2 71.48 0.0031 0.0018 0.016 0.63 Example 3 71.62 0.0026 0.0017 0.013 0.64 Example 4 71.41 0.0024 0.0017 0.011 0.62
[0072] The results in the table above show that in Comparative Examples 1, 2, 3, and 4, the amount of alkali added, the reaction temperature, and the oxidation time all affect the formation of manganese tetroxide. Sufficient alkali ensures sufficient reaction with the raw materials and maintains the system's pH in an alkaline state. Increasing the reaction temperature and extending the oxidation time allows for complete oxidation of manganese hydroxide, thereby increasing the manganese content of the product. In Comparative Examples 4 and 5, the manganese content of the calcined manganese tetroxide further increased, while the impurity content slightly decreased, indicating that calcination has a purifying and impurity-removing effect on the product.
[0073] Compared with Comparative Example 1, water vapor was added as a mixed gas for calcination in Examples 1, 2, 3, and 4, and the calcination temperature and time were increased and extended. It can be found that the addition of water vapor further removed impurities and increased the manganese content, resulting in higher purity of manganese tetroxide. Appropriately extending the calcination time and increasing the calcination temperature is beneficial to the formation of manganese tetroxide. Excessive temperature and calcination time may lead to over-oxidation of manganese tetroxide, thereby reducing the manganese content. Therefore, the calcination process should be within 500-600℃ for 6-10h; or 900-1000℃ for 4-8h.
[0074] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing high-purity manganese tetroxide by precipitating and oxidizing manganese chloride and then calcining it with steam, characterized in that, Includes the following steps: Step 1: Dissolve and mix manganese chloride with the surfactant and catalyst together; Step 2: Mix the solution obtained in Step 1 with the alkaline solution in parallel flow and introduce oxidizing gas to carry out the reaction; Step 3: Filter the solution obtained in Step 2, and dry the filter residue to obtain the initial product, manganese tetroxide. Step 4: Grind the initial product obtained in Step 3 and then perform segmented calcination to obtain purified manganese tetroxide. The surfactant used in step one is EDTA-2Na; the catalyst is ammonium chloride. The alkaline solution used in step two is a sodium hydroxide solution; the atmosphere used in the segmented calcination in step four is a mixture of air and water vapor. The reaction temperature in step two is 70-90℃; Step two uses air as the oxidizing gas; In step two, an oxidizing gas is introduced for oxidation for 4-8 hours; The segmented calcination process in step four consists of: a first-stage calcination at 500-600℃ for 6-10 hours, and a second-stage calcination at 900-1000℃ for 4-8 hours. During the segmented calcination process in step four, a mixture of air and water vapor is continuously introduced.
Citation Information
Patent Citations
High-purity manganous-manganic oxide and preparation method thereof
CN109052480A
Technology for preparing high-purity manganous-manganic oxide with manganese sulfate solution
CN103466720A
Method for refining iron oxide, iron oxide thus obtained and use thereof
CN118369293A