Optical glass, optical element and optical instrument
By reasonably preparing components such as SiO2, B2O3, La2O3, ZnO, Nb2O5+WO3 in optical glass, the crystallization resistance is improved, and the problem of poor crystallization resistance in precision molding of existing optical glass is solved, and the problem of poor crystallization resistance in precision molding is achieved. Efficient production and use of optical glass.
Patent Information
- Application Number
- CN202411128070.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-12
AI Technical Summary
The existing optical glass with a refractive index of 1.71 to 1.79 and an ABE number of 42 to 49 has poor crystallization resistance during precision molding, resulting in a decrease in the quality of the optical glass or scrapping.
Optical glass with specific component ratios, including SiO2, B2O3, La2O3, ZnO, Nb2O5+WO3, etc., improve the crystallization resistance through reasonable component design, with the refractive index and Abbe number in the range of 1.71~1.79, 42~49 Within, the upper limit temperature of crystallization is reduced to below 1080°C.
It significantly improves the crystallization resistance of optical glass, is suitable for precision molding, extends the service life of optical components, and reduces production costs and environmental pollution.
Smart Images

Figure BDA0004997048550000121 
Figure BDA0004997048550000151 
Figure BDA0004997048550000161
Abstract
Description
Technical Field
[0001] The invention relates to optical glass, in particular to optical glass with excellent anti-crystallization performance. Background Art
[0002] In recent years, with the advancement of science and technology, the continuous updating of optoelectronic information products, the demand for optical glass has gradually increased, and at the same time, higher requirements have been put forward for the performance of optical glass. Under the same radius of curvature, the higher the refractive index of the glass, the larger the imaging field of view. With the development trend of miniaturization of optical devices, the demand trend of high refractive index glass is becoming more and more obvious. Optical glass with a refractive index of 1.71 to 1.79 and an Abbe number of 42 to 49 is easier to achieve miniaturization, ultra-thinness and wide angle due to its high refractive index, and its application scenarios are relatively wide. At present, the mainstream method of manufacturing optical glass into optical components is precision molding (including direct molding and secondary molding). The use of precision molding technology to manufacture optical components reduces the consumption of raw materials, reduces the cost of manpower and material resources, and reduces environmental pollution. This technology can produce optical components in large quantities at low cost. The so-called precision molding is to mold a glass preform with a high-precision mold with a predetermined product shape under a certain temperature and pressure, so as to obtain a glass product with the shape and optical function of the final product. Various optical glass products can be manufactured by precision molding technology, such as spherical lenses, aspherical lenses, prisms and diffraction gratings, etc. In the prior art, optical glass with a refractive index of 1.71-1.79 and an Abbe number of 42-49 generally has a poor anti-crystallization performance when pressed. In the process of manufacturing optical components by precision molding, crystallization is easy to occur in the optical glass, resulting in a decline in the quality of the optical glass or even scrapping. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide an optical glass with excellent anti-crystallization performance.
[0004] The technical solution adopted by the present invention to solve the technical problem is:
[0005] (1) Optical glass, the components of which, expressed in weight percentage, contain: SiO2: 1-10%; B2O3: 18-31%; La2O3: 20-35%; ZnO: 19-32%; Nb2O5+WO3: 0.5-12%, wherein (Nb2O5+WO3) / ZnO is 0.05-0.5.
[0006] (2) The optical glass according to (1), wherein the components, expressed in weight percentage, further contain: ZrO2: 0-10%; and / or Gd2O3: 0-10%; and / or Y2O3: 0-10%; and / or Li2O: 0-8%; and / or Na2O: 0-6%; and / or K2O: 0-6%; and / or RO: 0-4%; and / or TiO2: 0-4%; and / or Ta2O5: 0-4%; and / or Al2O3: 0-4%; and / or Yb2O3: 0-10%; and / or F: 0-3%; and / or a clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
[0007] (3) Optical glass, which contains SiO2, B2O3, La2O and ZnO. The composition, expressed in weight percentage, contains Nb2O5+WO3: 0.5-12%, wherein (Nb2O5+WO3) / ZnO is 0.05-0.5, and the refractive index of the optical glass is n d is 1.71~1.79, Abbe number v d The maximum crystallization temperature is 1080°C or lower.
[0008] (4) The optical glass according to (3), wherein the components, expressed in weight percentage, include: SiO2: 1-10%; and / or B2O3: 18-31%; and / or La2O3: 20-35%; and / or ZnO: 19-32%; and / or ZrO2: 0-10%; and / or Gd2O3: 0-10%; and / or Y2O3: 0-10%; and / or Li2O: 0-8%; and / or Na2O: 0-6%; and / or Or K2O: 0-6%; and / or RO: 0-4%; and / or TiO2: 0-4%; and / or Ta2O5: 0-4%; and / or Al2O3: 0-4%; and / or Yb2O3: 0-10%; and / or F: 0-3%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
[0009] (5) The optical glass according to any one of (1) to (4), wherein the components thereof, expressed in weight percentage, satisfy one or more of the following 11 conditions:
[0010] 1) Gd2O3+Y2O3: 1-14%, preferably Gd2O3+Y2O3: 2-12%, more preferably Gd2O3+Y2O3: 2.5-10%;
[0011] 2) ZnO / La2O3 is 0.6 to 1.5, preferably ZnO / La2O3 is 0.7 to 1.4, more preferably ZnO / La2O3 is 0.8 to 1.3, and further preferably ZnO / La2O3 is 0.8 to 1.2;
[0012] 3) (Gd2O3+Y2O3) / ZnO is 0.05 to 0.6, preferably (Gd2O3+Y2O3) / ZnO is 0.1 to 0.5, more preferably (Gd2O3+Y2O3) / ZnO is 0.15 to 0.45, and further preferably (Gd2O3+Y2O3) / ZnO is 0.2 to 0.4;
[0013] 4) (Nb2O5+WO3) / SiO2 is 0.1 to 5.0, preferably (Nb2O5+WO3) / SiO2 is 0.3 to 3.0, more preferably (Nb2O5+WO3) / SiO2 is 0.5 to 2.5, and further preferably (Nb2O5+WO3) / SiO2 is 0.7 to 1.5;
[0014] 5) SiO2 / ZnO is 0.05 to 0.45, preferably SiO2 / ZnO is 0.1 to 0.4, and more preferably SiO2 / ZnO is 0.15 to 0.35;
[0015] 6) Nb2O5 / Y2O3 is 0.1 to 5.0, preferably Nb2O5 / Y2O3 is 0.2 to 3.0, more preferably Nb2O5 / Y2O3 is 0.3 to 2.5, and further preferably Nb2O5 / Y2O3 is 0.5 to 1.5;
[0016] 7) (WO3+Gd2O3+Ta2O5) / ZnO is less than 1.0, preferably (WO3+Gd2O3+Ta2O5) / ZnO is less than 0.8, more preferably (WO3+Gd2O3+Ta2O5) / ZnO is 0.05 to 0.6, and further preferably (WO3+Gd2O3+Ta2O5) / ZnO is 0.1 to 0.45;
[0017] 8) Gd2O3 / WO3 is less than 6.5, preferably Gd2O3 / WO3 is 0.1 to 5.0, more preferably Gd2O3 / WO3 is 0.5 to 4.0, and further preferably Gd2O3 / WO3 is 1.0 to 3.5;
[0018] 9) (Nb2O5+WO3) / ZnO is 0.08 to 0.4, preferably (Nb2O5+WO3) / ZnO is 0.1 to 0.3;
[0019] 10) (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.6 to 2.0, preferably (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.7 to 1.8, more preferably (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.8 to 1.5, and further preferably (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.8 to 1.3;
[0020] 11) (B2O3+WO3) / SiO2 is 2.5~15.0, preferably (B2O3+WO3) / SiO2 is 3.0~10.0, more preferably (B2O3+WO3) / SiO2 is 3.5~8.0, and further preferably (B2O3+WO3) / SiO2 is 4.0~6.0.
[0021] (6) The optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: SiO2: 2-8%, preferably SiO2: 3-7%; and / or B2O3: 20-29%, preferably B2O3: 22-27%; and / or La2O3: 22-33%, preferably La2O3: 24-31%; and / or ZrO2: 1-8%, preferably ZrO2: 1.5-5.5%; and / or ZnO: 20-28%, preferably ZnO: 22-27%; and / or Gd2O3: 0-8%, preferably Gd2O3: 2-7%; and / or Y2O3: 0.5-7%, preferably Y2O3: 1-5%; and / or Nb2O5+WO3: 1-10%, preferably Nb2O5+WO3: 2-8%; and / or Li2O: 0.5-7%, preferably Li2O: 1-5%; and / or Na2O: 0-5%, preferably Na2O: 0-3%, more preferably no Na2O; and / or K2O: 0-5%, preferably K2O: 0-3%, more preferably no K2O; and / or RO: 0-3%, preferably RO: 0-1%, more preferably no RO; and / or TiO2: 0-3%, preferably TiO2: 0-2%, more preferably no TiO2; and / or Ta2O5: 0-3%, preferably Ta2O5: 0-1%, more preferably no Ta2O5; and / or Al2O3: 0-3%, preferably Al2O3: 0-1% , more preferably does not contain Al2O3; and / or Yb2O3: 0-5%, preferably Yb2O3: 0-2%, more preferably does not contain Yb2O3; and / or F: 0-2%, preferably F: 0-1%, more preferably does not contain F; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.2%, the RO is one or more of MgO, CaO, SrO, BaO, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
[0022] (7) The optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: Nb2O5: 0 to 10%, preferably Nb2O5: 0.5 to 8%, more preferably Nb2O5: 1 to 6%; and / or WO3: 0 to 8%, preferably WO3: 0.5 to 6%, more preferably WO3: 1 to 3.8%.
[0023] (8) The refractive index n of the optical glass according to any one of (1) to (4) d is 1.71 to 1.79, preferably 1.72 to 1.78, more preferably 1.73 to 1.77, and further preferably 1.74 to 1.765. The Abbe number v d It is 42 to 49, preferably 43 to 48, more preferably 44 to 47, and further preferably 44.5 to 46.5.
[0024] (9) The optical glass according to any one of (1) to (4) 80 400nm or less, preferably λ 80 390nm or less, preferably λ 80 380nm or less; and / or λ5 is 350nm or less, preferably λ5 is 340nm or less, more preferably λ5 is 330nm or less; and / or water resistance stability D W is 2 or more, preferably 1; and / or the crystallization upper limit temperature is 1080°C or less, preferably 1050°C or less, more preferably 1000°C or less, and further preferably 980°C or less; and / or the Young's modulus E is 10000×10 7 / Pa or more, preferably 10500×10 7 / Pa~13000×10 7 / Pa, more preferably 11000×10 7 / Pa~12000×10 7 / Pa; and / or thermal expansion coefficient α -30 / 70℃ 80×10 -7 / K or less, preferably 75×10 -7 / K or less, more preferably 70×10 -7 / K or less, more preferably 65×10 -7 / K or less; and / or density ρ is 4.50g / cm 3 Below, preferably 4.40 g / cm 3 Below, more preferably 4.30g / cm 3 Below, more preferably 4.20 g / cm 3 Below; and / or wear degree F A90 to 130, preferably 95 to 125, more preferably 100 to 120; and / or transition temperature T g 560°C or less, preferably 550°C or less, more preferably 545°C or less, and further preferably 540°C or less; and / or Knoop hardness H K 600×10 7 Pa or more, preferably 610×10 7 Pa or more, more preferably 620×10 7 Pa or above.
[0025] (10) A glass preform made of the optical glass described in any one of (1) to (9).
[0026] (11) An optical element, made of the optical glass described in any one of (1) to (9), or made of the glass preform described in (10).
[0027] (12) An optical instrument comprising the optical glass described in any one of (1) to (9) and / or the optical element described in (11).
[0028] The beneficial effects of the present invention are as follows: through reasonable component design, the optical glass obtained by the present invention has excellent anti-crystallization performance and is suitable for manufacturing optical elements by methods such as precision molding. DETAILED DESCRIPTION
[0029] The following is a detailed description of the embodiments of the optical glass of the present invention, but the present invention is not limited to the following embodiments and can be implemented with appropriate changes within the scope of the purpose of the present invention. In addition, although there are appropriate omissions of the description of the repeated description, the main purpose of the invention will not be limited thereby. In the following content, the optical glass of the present invention is sometimes referred to as glass.
[0030] [Optical glass]
[0031] The following is an explanation of the range of each component (ingredient) of the optical glass of the present invention. In the present invention, unless otherwise specified, the content, total content, and total content of each component are all expressed in weight percentage (wt%), that is, the content, total content, and total content of each component are expressed in weight percentage relative to the total amount of glass material converted into oxide composition. Here, the "composition converted into oxide" means that when the oxides, complex salts, hydroxides, etc. used as raw materials for the optical glass components of the present invention decompose and transform into oxides during melting, the total amount of the oxide material is taken as 100%.
[0032] Unless otherwise indicated in specific circumstances, the numerical ranges listed herein include upper and lower limits, and "above" and "below" include endpoint values, as well as all integers and fractions within the range, without being limited to the specific values listed when the range is defined. "And / or" as used herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.
[0033] <Essential Components and Optional Components>
[0034] B2O3 is a network former component of glass, which has the function of maintaining glass stability and improving glass melting performance. However, if the content of B2O3 is too high, the chemical stability of the glass will deteriorate, and the viscosity of the glass will decrease, which will increase the difficulty of glass molding; if the content of B2O3 is too low, the performance of the vitrified material and the anti-crystallization performance will deteriorate, and the production performance will decrease. Therefore, the content of B2O3 is 18-31%, preferably 20-29%, and more preferably 22-27%.
[0035] SiO2 can increase the viscosity of molten glass, reduce the coloring of glass, improve the thermal stability of glass, and improve the resistance to devitrification, but if its content is too high, the melting difficulty of glass increases and the transition temperature rises. Therefore, the content of SiO2 is 1 to 10%, preferably 2 to 8%, and more preferably 3 to 7%.
[0036] La2O3 is an effective component for improving the refractive index of glass, and has a significant effect on improving the chemical stability and resistance to devitrification of glass. If its content is less than 20%, it is difficult to achieve the required optical constants; if the content is higher than 35%, the devitrification tendency of the glass increases and the thermal stability deteriorates. Therefore, the content of La2O3 is 20-35%, preferably 22-33%, and more preferably 24-31%.
[0037] Gd2O3 is a high refractive and low dispersion component, which can reduce the relative partial dispersion of glass and improve chemical stability in glass. If its content is too high, the devitrification resistance of glass will deteriorate and the transition temperature will increase. Therefore, the content of Gd2O3 in the present invention is 0-10%, preferably 0-8%, and more preferably 2-7%.
[0038] Y2O3 can improve the refractive index and devitrification resistance of glass and adjust the Young's modulus of glass. If its content exceeds 10%, the chemical stability and weather resistance of glass will deteriorate. Therefore, in the present invention, the Y2O3 content is 0-10%, preferably 0.5-7%, and more preferably 1-5%.
[0039] In some embodiments, the total content of Gd2O3 and Y2O3, Gd2O3+Y2O3, is controlled within the range of 1 to 14%, so that the optical glass can easily obtain the desired refractive index and Abbe number while improving the chemical stability of the glass and preventing the deterioration of the anti-crystallization performance. Therefore, Gd2O3+Y2O3 is preferably 1 to 14%, more preferably Gd2O3+Y2O3 is 2 to 12%, and further preferably Gd2O3+Y2O3 is 2.5 to 10%.
[0040] Yb2O3 is a component that gives glass high refractive and low dispersion properties. If its content exceeds 10%, the anti-crystallization performance of the glass decreases. Therefore, the content of Yb2O3 is 0-10%, preferably 0-5%, and more preferably 0-2%. In some embodiments, it is further preferred that Yb2O3 is not contained.
[0041] ZrO2 can increase the refractive index and devitrification resistance of glass, improve the chemical stability and mechanical properties of glass, but if its content is too high, the melting difficulty of glass will increase, which may lead to inclusions inside the glass and decrease in light transmittance. Therefore, the ZrO2 content is 0-10%, preferably 1-8%, and more preferably 1.5-5.5%.
[0042] Nb2O5 is a high refractive and high dispersion component, which can improve the resistance of glass to devitrification and reduce the thermal expansion coefficient of glass. If the content of Nb2O5 exceeds 10%, the weather resistance and light transmittance of the glass will decrease, and the transition temperature of the glass will increase. Therefore, the content of Nb2O5 in the present invention is 0 to 10%, preferably 0.5 to 8%, and more preferably 1 to 6%.
[0043] In some embodiments, the ratio of Nb2O5 to Y2O3, Nb2O5 / Y2O3, is controlled within the range of 0.1 to 5.0, which can improve the anti-crystallization performance and hardness of the glass. Therefore, Nb2O5 / Y2O3 is preferably 0.1 to 5.0, and Nb2O5 / Y2O3 is more preferably 0.2 to 3.0. Furthermore, controlling Nb2O5 / Y2O3 within the range of 0.3 to 2.5 can further reduce the thermal expansion coefficient of the glass and optimize the abrasiveness of the glass. Therefore, Nb2O5 / Y2O3 is further preferably 0.3 to 2.5, and Nb2O5 / Y2O3 is further preferably 0.5 to 1.5.
[0044] WO3 can improve the refractive index and dispersion of glass. If its content is too high, the light transmittance of glass will decrease and the secondary pressing anti-crystallization performance will deteriorate. Therefore, the WO3 content in the present invention is 0-8%, preferably 0.5-6%, and more preferably 1-3.8%.
[0045] In some embodiments, the total content of Nb2O5 and WO3, Nb2O5+WO3, is controlled within the range of 0.5 to 12%, so that the optical glass can easily obtain the desired refractive index and Abbe number, while optimizing the abrasiveness of the optical glass and preventing the increase of coloration. Therefore, Nb2O5+WO3 is preferably 0.5 to 12%, more preferably Nb2O5+WO3 is 1 to 10%, and further preferably Nb2O5+WO3 is 2 to 8%.
[0046] In some embodiments, by controlling the ratio of the total content of Nb2O5 and WO3 Nb2O5 + WO3 to the content of SiO2 (Nb2O5 + WO3) / SiO2 in the range of 0.1 to 5.0, the hardness and chemical stability of the glass can be improved and the transition temperature of the glass can be prevented from increasing. Therefore, preferably (Nb2O5 + WO3) / SiO2 is 0.1 to 5.0, more preferably (Nb2O5 + WO3) / SiO2 is 0.3 to 3.0, further preferably (Nb2O5 + WO3) / SiO2 is 0.5 to 2.5, and further preferably (Nb2O5 + WO3) / SiO2 is 0.7 to 1.5.
[0047] In some embodiments, by making the ratio of the content of Gd2O3 to the content of WO3 Gd2O3 / WO3 below 6.5, the abrasiveness of the glass can be optimized while reducing the transition temperature of the glass. Therefore, preferably Gd2O3 / WO3 is below 6.5, more preferably Gd2O3 / WO3 is 0.1 to 5.0, further preferably Gd2O3 / WO3 is 0.5 to 4.0, and further preferably Gd2O3 / WO3 is 1.0 to 3.5.
[0048] In some embodiments, the ratio (B2O3+WO3) / SiO2 between the total content of B2O3 and WO3 (B2O3+WO3) and the content of SiO2 is controlled within the range of 2.5 to 15.0, which can improve the hardness and chemical stability of the glass and optimize the abrasiveness of the glass. Therefore, preferably (B2O3+WO3) / SiO2 is 2.5 to 15.0, more preferably (B2O3+WO3) / SiO2 is 3.0 to 10.0, further preferably (B2O3+WO3) / SiO2 is 3.5 to 8.0, and further preferably (B2O3+WO3) / SiO2 is 4.0 to 6.0.
[0049] ZnO can improve the chemical stability of glass and reduce the high temperature viscosity and transition temperature of glass. In the present invention, the above effects are obtained by containing more than 19% ZnO. However, if the content of ZnO is too much, the anti-crystallization performance of the glass decreases, and the high temperature viscosity is small, which brings difficulties to molding. Therefore, the content of ZnO is 19-32%, preferably 20-28%, and more preferably 22-27%.
[0050] In some embodiments, by controlling the ratio ZnO / La2O3 between the content of ZnO and the content of La2O3 in the range of 0.6 to 1.5, the thermal expansion coefficient of the glass can be reduced and the abrasiveness of the glass can be optimized. Therefore, ZnO / La2O3 is preferably 0.6 to 1.5, more preferably 0.7 to 1.4, further preferably 0.8 to 1.3, and further preferably 0.8 to 1.2.
[0051] In some embodiments, the ratio of the total content of Gd2O3 and Y2O3 Gd2O3 + Y2O3 to the content of ZnO (Gd2O3 + Y2O3) / ZnO is controlled within the range of 0.05 to 0.6, which can increase the Young's modulus of the glass and reduce the coloration and density of the glass. Therefore, preferably (Gd2O3 + Y2O3) / ZnO is 0.05 to 0.6, more preferably (Gd2O3 + Y2O3) / ZnO is 0.1 to 0.5, further preferably (Gd2O3 + Y2O3) / ZnO is 0.15 to 0.45, and further preferably (Gd2O3 + Y2O3) / ZnO is 0.2 to 0.4.
[0052] In some embodiments, the ratio of SiO2 to ZnO is set within the range of 0.05 to 0.45, which can improve the Young's modulus and anti-crystallization performance of the glass and reduce the thermal expansion coefficient of the glass. Therefore, SiO2 / ZnO is preferably 0.05 to 0.45, more preferably 0.1 to 0.4, and further preferably 0.15 to 0.35.
[0053] In some embodiments, by controlling the ratio of the total content of Nb2O5 and WO3 Nb2O5 + WO3 to the content of ZnO (Nb2O5 + WO3) / ZnO in the range of 0.05 to 0.5, the anti-crystallization property and Young's modulus of the glass can be improved, and the chemical stability of the glass can be optimized. Therefore, preferably (Nb2O5 + WO3) / ZnO is 0.05 to 0.5, more preferably (Nb2O5 + WO3) / ZnO is 0.08 to 0.4, and further preferably (Nb2O5 + WO3) / ZnO is 0.1 to 0.3.
[0054] In some embodiments, controlling the ratio of the total content of SiO2, WO3, and La2O3 SiO2+WO3+La2O3 to the total content of ZnO and Gd2O3 ZnO+Gd2O3 (SiO2+WO3+La2O3) / (ZnO+Gd2O3) within the range of 0.6 to 2.0 can improve the hardness and chemical stability of the glass and optimize the abrasiveness of the glass. Therefore, the preferred ratio of (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.6~2.0, the more preferred ratio of (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.7~1.8, the further preferred ratio of (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.8~1.5, and the further preferred ratio of (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.8~1.3.
[0055] Li2O can reduce the transition temperature of glass and improve the melting property of glass, but when its content is high, it is not good for the chemical stability, anti-devitrification and thermal expansion coefficient of glass. Therefore, the content of Li2O in the present invention is 0-8%, preferably 0.5-7%, and more preferably 1-5%.
[0056] Na2O can improve the chemical stability of glass and enhance the anti-crystallization performance of glass during secondary compression molding. If the content of Na2O is too high, the refractive index of the glass will be difficult to meet the design requirements. Therefore, the content of Na2O is 0-6%, preferably 0-5%, and more preferably 0-3%. In some embodiments, it is further preferred that Na2O is not contained.
[0057] K2O has the effect of improving the thermal stability and melting property of glass. If its content exceeds 6%, the devitrification resistance and chemical stability of glass will deteriorate. Therefore, the content of K2O in the present invention is 0 to 6%, preferably 0 to 5%, and more preferably 0 to 3%. In some embodiments, it is further preferred that K2O is not contained.
[0058] RO (RO is one or more of MgO, CaO, SrO and BaO) can improve the meltability of glass and adjust the optical constants of glass. If its content exceeds 4%, the devitrification resistance of glass decreases. Therefore, the content of RO in the present invention is 0-4%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that MgO is not contained; and / or CaO is not contained; and / or SrO is not contained; and / or BaO is not contained.
[0059] TiO2 has the effect of increasing the refractive index and dispersion of glass and improving the resistance to devitrification. If its content exceeds 4%, the tendency of crystallization and coloring of glass increases, and the transition temperature rises. Therefore, the content of TiO2 in the present invention is 4% or less, preferably 3% or less, and more preferably 2% or less. In some embodiments, it is further preferred that TiO2 is not contained.
[0060] Ta2O5 has the effect of increasing the refractive index of glass and improving the resistance to devitrification, but if its content is too high, the thermal stability of the glass will decrease, the density will increase, and the cost control of the glass raw materials will be unfavorable. Therefore, the content of Ta2O5 in the present invention is 0-4%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that Ta2O5 is not contained.
[0061] In some embodiments, by controlling the ratio of the total content of WO3, Gd2O3, and Ta2O5, WO3+Gd2O3+Ta2O5, to the content of ZnO (WO3+Gd2O3+Ta2O5) / ZnO to be below 1.0, the Young's modulus can be prevented from decreasing while reducing the coloring of the glass. Therefore, it is preferred that (WO3+Gd2O3+Ta2O5) / ZnO is below 1.0, and it is more preferred that (WO3+Gd2O3+Ta2O5) / ZnO is below 0.8. Furthermore, by making (WO3+Gd2O3+Ta2O5) / ZnO in the range of 0.05 to 0.6, the hardness of the glass can be further improved. Therefore, it is further preferred that (WO3+Gd2O3+Ta2O5) / ZnO is 0.05 to 0.6, and it is further preferred that (WO3+Gd2O3+Ta2O5) / ZnO is 0.1 to 0.45.
[0062] Al2O3 has the effect of reducing the thermal expansion coefficient of glass and improving the thermal stability of glass. However, if the Al2O3 content is too high, the glass transition temperature will increase, and the high-temperature viscosity of the glass will increase, and bubbles will be difficult to eliminate. Therefore, the content of Al2O3 is 0-4%, preferably 0-3%, and more preferably 0-1%. In some embodiments, it is further preferred that Al2O3 is not contained.
[0063] In the present invention, by containing 0-1% of one or more components of Sb2O3, SnO2, SnO, and CeO2 as a clarifier, the clarification effect of the glass can be improved and the bubble degree of the glass can be improved. The content of the clarifier is preferably 0-0.5%, and more preferably 0-0.2%. Since the component types and contents of the optical glass of the present invention are reasonably designed and the bubble degree is excellent, it is further preferred that no clarifier is contained in some embodiments.
[0064] F can be used to adjust the refractive index of glass and reduce the temperature coefficient of refractive index. However, in the production process of optical glass, F volatilizes and generates environmental load. At the same time, it will volatilize from the glass surface in the molding temperature zone to form an inhomogeneous part, which reduces the glass quality and consistency of optical constants. Therefore, the content of F is 0-3%, preferably 0-2%, and more preferably 0-1%. In some embodiments, it is further preferred that F is not contained.
[0065] <Components that should not be contained>
[0066] In the glass of the present invention, even if oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo are contained alone or in combination in small amounts, the glass will be colored and absorption will occur at specific wavelengths in the visible light region, thereby weakening the property of the present invention of improving the visible light transmittance. Therefore, it is preferably substantially free of oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo, especially for optical glasses that require transmittance at wavelengths in the visible light region.
[0067] The oxides of Th, Cd, Tl, Os, Be and Se have a tendency to be controlled in recent years as harmful chemical substances, and environmental protection measures are necessary not only in the manufacturing process of glass, but also in the processing process and the disposal after productization. Therefore, in the case of paying attention to the impact on the environment, it is preferred that they are actually not contained except for being inevitably mixed in. Thus, the optical glass actually does not contain substances that pollute the environment. Therefore, even if special environmental countermeasures are not taken, the optical glass of the present invention can also be manufactured, processed and discarded. At the same time, in order to achieve environmental friendliness, the optical glass of the present invention preferably does not contain As2O3 and PbO.
[0068] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the optical glass of the present invention; however, as raw materials and / or equipment for producing optical glass, there will be certain impurities or components that are not intentionally added, which will be contained in a small amount or trace amount in the final optical glass, and this situation is also within the scope of protection of the patent of this invention.
[0069] The properties of the optical glass of the present invention will be described below:
[0070] <Refractive Index and Abbe Number>
[0071] The refractive index of optical glass (n d ) and the Abbe number (ν d ) Tested according to the method specified in GB / T 7962.1-2010.
[0072] In some embodiments, the refractive index (n d) has an upper limit of 1.79, a preferred upper limit of 1.78, a more preferred upper limit of 1.77, and a further preferred upper limit of 1.765.
[0073] In some embodiments, the refractive index (n d ) has a lower limit of 1.71, a preferred lower limit is 1.72, a more preferred lower limit is 1.73, and a further preferred lower limit is 1.74.
[0074] In some embodiments, the Abbe number (ν d ) has an upper limit of 49, a preferred upper limit of 48, a more preferred upper limit of 47, and a further preferred upper limit of 46.5.
[0075] In some embodiments, the Abbe number (ν d ) has a lower limit of 42, a preferred lower limit of 43, a more preferred lower limit of 44, and a further preferred lower limit of 44.5.
[0076] <Color>
[0077] The short-wave transmission spectrum characteristics of the optical glass of the present invention are expressed by the coloring degree (λ 80 and λ5). 80 It refers to the wavelength when the glass transmittance reaches 80%. 80 The measurement is to use a glass with a thickness of 10±0.1mm and two opposite planes parallel to each other and optically polished, and measure the spectral transmittance in the wavelength range from 280nm to 700nm and the wavelength at which the transmittance is 80%. The so-called spectral transmittance or transmittance is the wavelength at which the incident intensity I is perpendicular to the above surface of the glass. in Light of intensity I passes through the glass and emerges from a plane out The light of the case through I out / I in λ is a quantity that also includes the transmittance of the surface reflection loss on the above surface of the glass. The higher the refractive index of the glass, the greater the surface reflection loss. Therefore, λ 80 A small value of means that the glass itself is less colored and has a high light transmittance.
[0078] The same applies to λ5.
[0079] In some embodiments, the λ of the optical glass of the present invention is 80 400nm or less, preferably λ 80 390nm or less, preferably λ 80 Below 380nm.
[0080] In some embodiments, the optical glass of the present invention has a λ5 of 350 nm or less, preferably a λ5 of 340 nm or less, and more preferably a λ5 of 330 nm or less.
[0081] <Water resistance stability>
[0082] Water resistance stability of optical glass (D W ) (Powder method) Tested in accordance with the method specified in GB / T 17129.
[0083] In some embodiments, the water resistance stability (D W ) is 2 or more types, preferably 1 type.
[0084] <Crystallization upper limit temperature>
[0085] The gradient temperature furnace method was used to determine the anti-crystallization performance of optical glass. The glass was made into a 180×10×10mm sample, polished on the side, and placed in a furnace with a temperature gradient (10℃ / cm) and a highest temperature zone of 1200℃ for 4 hours. Then the sample was taken out and naturally cooled to room temperature. The crystallization of the glass was observed under a microscope. The highest temperature corresponding to the appearance of crystals in the glass was the upper limit temperature of crystallization of the glass.
[0086] In some embodiments, the optical glass of the present invention has a crystallization upper limit temperature of 1080° C. or lower, preferably 1050° C. or lower, more preferably 1000° C. or lower, and further preferably 980° C. or lower.
[0087] <Young's modulus>
[0088] The Young's modulus (E) of optical glass is calculated using the following formula by ultrasonic testing of its longitudinal wave velocity and transverse wave velocity.
[0089]
[0090]
[0091] Where: E is Young's modulus, Pa;
[0092] G is the shear modulus, Pa;
[0093] V T is the shear wave velocity, m / s;
[0094] V S is the longitudinal wave velocity, m / s;
[0095] ρ is the glass density, g / cm 3 .
[0096] In some embodiments, the Young's modulus (E) of the optical glass of the present invention is 10000×107 / Pa or more, preferably 10500×10 7 / Pa~13000×10 7 / Pa, more preferably 11000×10 7 / Pa~12000×10 7 / Pa.
[0097] <Coefficient of Thermal Expansion>
[0098] Thermal expansion coefficient of optical glass (α -30 / 70℃ ) Test results at -30~70℃ according to the method specified in GB / T7962.16-2010.
[0099] In some embodiments, the thermal expansion coefficient (α -30 / 70℃ ) is 80×10 -7 / K or less, preferably 75×10 -7 / K or less, more preferably 70×10 -7 / K or less, more preferably 65×10 -7 / K or less.
[0100] <density>
[0101] The density (ρ) of optical glass is tested according to the method specified in GB / T7962.20-2010.
[0102] In some embodiments, the density (ρ) of the optical glass of the present invention is 4.50 g / cm 3 Below, preferably 4.40 g / cm 3 Below, more preferably 4.30g / cm 3 Below, more preferably 4.20 g / cm 3 the following.
[0103] <Abrasion>
[0104] Abrasiveness of optical glass (F A ) refers to the value obtained by multiplying the ratio of the wear volume of the sample to the wear volume (volume) of the standard sample (H-K9 glass) under exactly the same conditions by 100, and is expressed by the following formula:
[0105] F A =V / V0×100=(W / ρ) / (W0 / ρ0)×100
[0106] Where: V—volume wear of the sample being tested;
[0107] V0—Volume loss of standard sample;
[0108] W—mass wear loss of the sample being tested;
[0109] W0—standard sample mass wear;
[0110] ρ—density of the sample being tested;
[0111] ρ0—standard sample density.
[0112] In some embodiments, the abrasiveness (F A ) has an upper limit of 130, a preferred upper limit of 125, and a more preferred upper limit of 120.
[0113] In some embodiments, the abrasiveness (F A ) has a lower limit of 90, a preferred lower limit of 95, and a more preferred lower limit of 100.
[0114] <Transition Temperature>
[0115] Transition temperature of optical glass (T g ) Tested according to the method specified in GB / T7962.16-2010.
[0116] In some embodiments, the transition temperature (T g ) is 560°C or lower, preferably 550°C or lower, more preferably 545°C or lower, and further preferably 540°C or lower.
[0117] <Knoop hardness>
[0118] Knoop hardness of optical glass (H K ) is tested according to the test method specified in GB / T7962.18-2010. In the present invention, Knoop hardness is sometimes referred to as hardness.
[0119] In some embodiments, the Knoop hardness (H K ) is 600×10 7 Pa or more, preferably 610×10 7 Pa or more, more preferably 620×10 7 Pa or above.
[0120] [Manufacturing method]
[0121] The manufacturing method of the optical glass of the present invention is as follows: the glass of the present invention is produced using conventional raw materials and processes, including but not limited to using oxides, hydroxides, fluorides, various salts (carbonates, nitrates, sulfates) and the like as raw materials, and after mixing the materials according to conventional methods, the prepared furnace materials are put into a melting furnace (such as platinum, gold or platinum alloy crucible) at 900-1400° C. for melting, and after clarification and homogenization, a homogeneous molten glass without bubbles and undissolved substances is obtained, and the molten glass is cast in a mold and annealed. Those skilled in the art can appropriately select raw materials, process methods and process parameters according to actual needs.
[0122] [Glass preforms and optical components]
[0123] The prepared optical glass can be used to make a glass preform by means of direct drop molding, grinding, or compression molding such as hot press molding. That is, the molten optical glass can be directly precision drop molded into a glass precision preform, or the glass preform can be made by mechanical processing such as grinding and grinding, or the preform for compression molding made of the optical glass can be made by hot press molding and then grinding. It should be noted that the means for preparing the glass preform are not limited to the above means.
[0124] As described above, the optical glass of the present invention is useful for various optical elements and optical designs, and it is particularly preferred to form a preform from the optical glass of the present invention and use the preform to perform re-hot pressing, precision stamping, etc. to produce optical elements such as lenses and prisms.
[0125] The glass preform and optical element of the present invention are both formed of the optical glass of the present invention. The glass preform of the present invention has the excellent properties of optical glass; the optical element of the present invention has the excellent properties of optical glass, and can provide various optical elements such as lenses and prisms with high optical value.
[0126] Examples of the lens include various lenses having spherical or aspherical lens surfaces, such as a concave meniscus lens, a convex meniscus lens, a biconvex lens, a biconcave lens, a plano-convex lens, and a plano-concave lens.
[0127] [Optical instruments]
[0128] The optical element formed by the optical glass of the present invention can be used to manufacture optical instruments such as photographic equipment, video equipment, projection equipment, display equipment, vehicle-mounted equipment and monitoring equipment.
[0129] Example
[0130] <Optical Glass Example>
[0131] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided.
[0132] This embodiment adopts the above optical glass manufacturing method to obtain optical glasses having the compositions shown in Tables 1 to 3. In addition, the properties of each glass are measured by the testing method described in the present invention, and the measurement results are shown in Tables 1 to 3.
[0133] Table 1.
[0134]
[0135]
[0136]
[0137] Table 2.
[0138]
[0139]
[0140] Table 3.
[0141]
[0142]
[0143] <Glass Preform Example>
[0144] The glass obtained from optical glass examples 1 to 24# is used, for example, by grinding processing, or by molding methods such as hot pressing, precision stamping, etc., to make preforms of various lenses, prisms, etc., such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses.
[0145] <Optical Element Embodiment>
[0146] The preforms obtained in the above-mentioned glass preform embodiments are annealed to reduce the deformation inside the glass and perform fine adjustments so that the optical properties such as the refractive index reach the desired values.
[0147] Next, each preform is ground and polished to produce various lenses and prisms such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. The surface of the obtained optical element may be coated with an anti-reflection film.
[0148] <Optical Instrument Embodiment>
[0149] The optical element obtained by the above-mentioned optical element embodiment is optically designed to form an optical component or optical assembly by using one or more optical elements. It can be used in, for example, imaging equipment, sensors, microscopes, medical technology, digital projection, communications, optical communication technology / information transmission, optics / lighting in the automotive field, lithography technology, excimer lasers, wafers, computer chips, and integrated circuits and electronic devices including such circuits and chips, or in camera equipment and devices in the vehicle field.
Claims
1. Optical glass, characterized in that: Its components, expressed in weight percentage, include: SiO2: 1-10%; B2O3: 18-31%; La2O3: 20-35%; ZnO: 19-32%; Nb2O5+WO3: 0.5-12%, wherein (Nb2O5+WO3) / ZnO is 0.05-0.
5.
2. The optical glass according to claim 1, characterized in that: Its components, expressed in weight percentage, also contain: ZrO2: 0-10%; and / or Gd2O3: 0-10%; and / or Y2O3: 0-10%; and / or Li2O: 0-8%; and / or Na2O: 0-6%; and / or K2O: 0-6%; and / or RO: 0-4%; and / or TiO2: 0-4%; and / or Ta2O5: 0-4%; and / or Al2O3: 0-4%; and / or Yb2O3: 0-10%; and / or F: 0-3%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
3. Optical glass, characterized in that: The components include SiO2, B2O3, La2O and ZnO. The components are expressed in weight percentage, including Nb2O5+WO3: 0.5-12%, wherein (Nb2O5+WO3) / ZnO is 0.05-0.5, and the refractive index of the optical glass is n d is 1.71~1.79, Abbe number v d The maximum crystallization temperature is 1080°C or lower.
4. The optical glass according to claim 3, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 1-10%; and / or B2O3: 18-31%; and / or La2O3: 20-35%; and / or ZnO: 19-32%; and / or ZrO2: 0-10%; and / or Gd2O3: 0-10%; and / or Y2O3: 0-10%; and / or Li2O: 0-8%; and / or Na2O: 0-6%; and / or K2O: 0-6 %; and / or RO: 0-4%; and / or TiO2: 0-4%; and / or Ta2O5: 0-4%; and / or Al2O3: 0-4%; and / or Yb2O3: 0-10%; and / or F: 0-3%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
5. The optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage and meet one or more of the following 11 conditions: 1) Gd2O3+Y2O3: 1-14%, preferably Gd2O3+Y2O3: 2-12%, more preferably Gd2O3+Y2O3: 2.5-10%; 2) ZnO / La2O3 is 0.6 to 1.5, preferably ZnO / La2O3 is 0.7 to 1.4, more preferably ZnO / La2O3 is 0.8 to 1.3, and further preferably ZnO / La2O3 is 0.8 to 1.2; 3) (Gd2O3+Y2O3) / ZnO is 0.05 to 0.6, preferably (Gd2O3+Y2O3) / ZnO is 0.1 to 0.5, more preferably (Gd2O3+Y2O3) / ZnO is 0.15 to 0.45, and further preferably (Gd2O3+Y2O3) / ZnO is 0.2 to 0.4; 4) (Nb2O5+WO3) / SiO2 is 0.1 to 5.0, preferably (Nb2O5+WO3) / SiO2 is 0.3 to 3.0, more preferably (Nb2O5+WO3) / SiO2 is 0.5 to 2.5, and further preferably (Nb2O5+WO3) / SiO2 is 0.7 to 1.5; 5) SiO2 / ZnO is 0.05 to 0.45, preferably SiO2 / ZnO is 0.1 to 0.4, and more preferably SiO2 / ZnO is 0.15 to 0.35; 6) Nb2O5 / Y2O3 is 0.1 to 5.0, preferably Nb2O5 / Y2O3 is 0.2 to 3.0, more preferably Nb2O5 / Y2O3 is 0.3 to 2.5, and further preferably Nb2O5 / Y2O3 is 0.5 to 1.5; 7) (WO3+Gd2O3+Ta2O5) / ZnO is less than 1.0, preferably (WO3+Gd2O3+Ta2O5) / ZnO is less than 0.8, more preferably (WO3+Gd2O3+Ta2O5) / ZnO is 0.05 to 0.6, and further preferably (WO3+Gd2O3+Ta2O5) / ZnO is 0.1 to 0.45; 8) Gd2O3 / WO3 is less than 6.5, preferably Gd2O3 / WO3 is 0.1 to 5.0, more preferably Gd2O3 / WO3 is 0.5 to 4.0, and further preferably Gd2O3 / WO3 is 1.0 to 3.5; 9) (Nb2O5+WO3) / ZnO is 0.08 to 0.4, preferably (Nb2O5+WO3) / ZnO is 0.1 to 0.3; 10) (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.6 to 2.0, preferably (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.7 to 1.8, more preferably (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.8 to 1.5, and further preferably (SiO2+WO3+La2O3) / (ZnO+Gd2O3) is 0.8 to 1.3; 11) (B2O3+WO3) / SiO2 is 2.5~15.0, preferably (B2O3+WO3) / SiO2 is 3.0~10.0, more preferably (B2O3+WO3) / SiO2 is 3.5~8.0, and further preferably (B2O3+WO3) / SiO2 is 4.0~6.
0.
6. The optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: SiO2: 2-8%, preferably SiO2: 3-7%; and / or B2O3: 20-29%, preferably B2O3: 22-27%; and / or La2O3: 22-33%, preferably La2O3: 24-31%; and / or ZrO2: 1-8%, preferably ZrO2: 1.5-5.5%; and / or ZnO: 20-28%, preferably ZnO: 22-27%; and / or Gd 2O3: 0-8%, preferably Gd2O3: 2-7%; and / or Y2O3: 0.5-7%, preferably Y2O3: 1-5%; and / or Nb2O5+WO3: 1-10%, preferably Nb2O5+WO3: 2-8%; and / or Li2O: 0.5-7%, preferably Li2O: 1-5%; and / or Na2O: 0-5%, preferably Na2O: 0-3%, more preferably no Na2O; and / or K2O: 0-5% , preferably K2O: 0-3%, more preferably no K2O; and / or RO: 0-3%, preferably RO: 0-1%, more preferably no RO; and / or TiO2: 0-3%, preferably TiO2: 0-2%, more preferably no TiO2; and / or Ta2O5: 0-3%, preferably Ta2O5: 0-1%, more preferably no Ta2O5; and / or Al2O3: 0-3%, preferably Al2O3: 0-1%, more preferably no Al2O3; and / or Yb2O3: 0-5%, preferably Yb2O3: 0-2%, more preferably no Yb2O3; and / or F: 0-2%, preferably F: 0-1%, more preferably no F; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.2%, wherein RO is one or more of MgO, CaO, SrO, and BaO, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.
7. The optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: Nb2O5: 0-10%, preferably Nb2O5: 0.5-8%, more preferably Nb2O5: 1-6%; and / or WO3: 0-8%, preferably WO3: 0.5-6%, more preferably WO3: 1-3.8%.
8. The optical glass according to any one of claims 1 to 4, characterized in that: The refractive index n of the optical glass d is 1.71 to 1.79, preferably 1.72 to 1.78, more preferably 1.73 to 1.77, and further preferably 1.74 to 1.
765. The Abbe number v d It is 42 to 49, preferably 43 to 48, more preferably 44 to 47, and further preferably 44.5 to 46.
5.
9. The optical glass according to any one of claims 1 to 4, characterized in that: The λ of the optical glass 80 400nm or less, preferably λ 80 390nm or less, preferably λ 80 380nm or less; and / or λ5 is 350nm or less, preferably λ5 is 340nm or less, more preferably λ5 is 330nm or less; and / or water resistance stability D W is 2 or more, preferably 1; and / or the crystallization upper limit temperature is 1080°C or less, preferably 1050°C or less, more preferably 1000°C or less, and further preferably 980°C or less; and / or the Young's modulus E is 10000×10 7 / Pa or more, preferably 10500×10 7 / Pa~13000×10 7 / Pa, more preferably 11000×10 7 / Pa~12000×10 7 / Pa; and / or thermal expansion coefficient α -30 / 70℃ 80×10 -7 / K or less, preferably 75×10 -7 / K or less, more preferably 70×10 -7 / K or less, more preferably 65×10 -7 / K or less; and / or density ρ is 4.50g / cm 3 Below, preferably 4.40g / cm 3 Below, more preferably 4.30g / cm 3 Below, more preferably 4.20 g / cm 3 Below; and / or wear degree F A 90 to 130, preferably 95 to 125, more preferably 100 to 120; and / or transition temperature T g 560°C or less, preferably 550°C or less, more preferably 545°C or less, and further preferably 540°C or less; and / or Knoop hardness H K 600×10 7 Pa or more, preferably 610×10 7 Pa or more, more preferably 620×10 7 Pa or above.
10. A glass preform, characterized in that: Made of the optical glass described in any one of claims 1 to 9.
11. An optical element, characterized in that The optical glass is made of the optical glass described in any one of claims 1 to 9, or the glass preform described in claim 10.