A method of heat treating an electron beam physical vapor deposition glass microsphere coating
By employing multi-stage vacuum heat treatment to coat glass microspheres with electron beam physical vapor deposition, the problems of narrow bandwidth and unstable performance of microwave absorbing materials were solved, and the bonding strength and material properties of the coating were improved.
Patent Information
- Application Number
- CN202411091992.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-08-09
AI Technical Summary
Existing microwave absorbing materials have narrow bandwidth and unstable absorption performance. Single absorbers are difficult to meet the expected goals, and it is necessary to improve the impedance matching and electromagnetic loss characteristics of the materials.
A multi-stage vacuum heat treatment method using electron beam physical vapor deposition to coat glass microspheres includes multiple stages of heat preservation and cooling processes, controlling temperature and vacuum levels to improve the mechanical properties of the material.
By using a multi-segment thermal insulation method, the coating bonding strength is improved under low vacuum conditions, the integrity of the microspheres is maintained, and the microwave absorption performance of the material is improved.
Smart Images

Figure CN118930064B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of aero-engine coating materials and relates to a heat treatment method for electron beam physical vapor deposition of glass microsphere coatings. Background Technology
[0002] Microwave-absorbing coatings generally consist of adhesives, absorbents, and various additives, with the absorbent being the main material and directly determining the coating's microwave absorption performance. According to the principles of microwave absorption, key factors affecting the performance of microwave-absorbing materials include their impedance matching characteristics and attenuation characteristics. Improving electromagnetic wave attenuation requires enhancing the electromagnetic loss characteristics of the absorbing material, while impedance matching necessitates good dielectric matching properties. However, single absorbents suffer from drawbacks such as narrow bandwidth and unstable absorption performance, resulting in microwave-absorbing materials that fall short of expectations. Therefore, surface modification of absorbents has received widespread attention. Surface modification is a unique method for modifying absorbents and is widely used in absorbent surface treatment. It can not only improve the bonding strength of absorbing materials but also reduce the dielectric constant and improve impedance matching, ultimately enhancing the microwave absorption performance of the material. Summary of the Invention
[0003] The purpose of this invention is to address the shortcomings of the prior art by providing a heat treatment method for electron beam physical vapor deposition (EBPD) glass microsphere coatings. The aim is to improve the mechanical properties of the material by inducing changes in the crystal structure and microstructure of the glass microsphere coatings through vacuum heat treatment.
[0004] To solve this technical problem, the technical solution of the present invention is as follows:
[0005] A heat treatment method for coating glass microspheres with an electron beam physical vapor deposition (EBPV) coating is provided, wherein the heat treatment process is as follows:
[0006] Electron beam physical vapor deposition (EBPV) coatings were applied to glass microspheres and placed in a vacuum heat treatment furnace. The furnace temperature was then raised to 800±50℃, with a vacuum degree <1×10⁻⁶. -2 Pa, after holding at this temperature for 2-4 hours, cool the furnace to 600±50℃, hold for 30±5 minutes, then cool the furnace to 250±50℃, hold for 30±5 minutes, then cool the furnace to room temperature. After cooling to room temperature, open the vacuum chamber and remove the coating.
[0007] The coating system is an iron-cobalt-nickel based pentagonal high-entropy microwave absorbing coating FeCoNiXY, wherein X and Y are both metal or transition metal atoms.
[0008] The glass microspheres have a diameter of 100-200 μm. This particle size range makes it easier to achieve uniform coating and is easy to prepare, achieving a good balance between cost and performance.
[0009] The electron beam physical vapor deposition process parameters are: evaporation current 0.8-1.2A, rotation speed 5-10RPM, coating thickness 10-100μm, and glass microsphere diameter 100-200μm.
[0010] The heat treatment method further includes the steps of cleaning and dehydrating the coating prior to heat treatment.
[0011] The cleaning steps are as follows: the iron-cobalt-nickel-based high-entropy microwave absorbing coating on the electron beam physical vapor deposition glass microspheres is immersed in 10±5% water-based cleaning agent for 30±5 min, and then the iron-cobalt-nickel-based high-entropy microwave absorbing coating on the electron beam physical vapor deposition glass microspheres is immersed in deionized water for 30±5 min.
[0012] Preferably, the water-based cleaning agent is a degreasing agent with a pH of 7±0.5.
[0013] The dehydration and drying steps are as follows: the iron-cobalt-nickel-based high-entropy microwave absorbing coating on the electron beam physical vapor deposition glass microspheres is immersed in an organic solvent for 10±5 min, and then taken out and placed in an oven to dry at 80±10℃ for 15±5 min.
[0014] Preferably, the organic solvent is acetone or ethanol, and its purity is analytical grade.
[0015] The advantages and beneficial effects of this invention are as follows:
[0016] In the heat treatment process of this invention, a multi-stage heat preservation method is adopted. Under low vacuum conditions, by controlling the heat preservation time and temperature at each stage, the bonding strength of the coating layer is improved, while maintaining the integrity of the microspheres, ultimately improving the performance of the material. Attached Figure Description
[0017] To more clearly illustrate the technical solutions implemented in this invention, the accompanying drawings used in the embodiments of this invention will be briefly explained below. Obviously, the drawings described below are merely some embodiments of this invention. Those skilled in the art can obtain other drawings based on these drawings without any creative effort.
[0018] Figure 1 The appearance changes of the glass microsphere coating before and after heat treatment in Example 1 are shown below. Figure 1 As can be seen from the image, the glass microspheres appear black after being coated with an iron-cobalt-nickel-based pentagonal high-entropy absorbing coating, indicating that the coating is uniform.
[0019] Figure 2 The variation in bonding strength of the glass microsphere coatings in Examples 1, 2, 3 and the comparative examples is shown.
[0020] from Figure 2 As can be seen, the multi-segment insulation method of 800-600-250℃ improves the bonding strength of the coating, reaching over 8MPa. Detailed Implementation
[0021] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0022] The features of various aspects of embodiments of the present invention will now be described in detail. In the following detailed description, numerous specific details are set forth in order to provide a thorough understanding of the invention. However, it will be apparent to those skilled in the art that the invention can also be practiced without these specific details.
[0023] The technical solution of the invention will be further described in detail below with reference to the embodiments:
[0024] The process conditions for the washing and dehydration drying steps in this embodiment of the invention are the same as those in the comparative example, and the steps are as follows:
[0025] (1) Preparation of iron-cobalt-nickel-based high-entropy microwave absorbing coating by electron beam physical vapor deposition of glass microspheres: The electron beam physical vapor deposition process parameters are: evaporation current 0.8-1.2A, rotation speed 5-10RPM, coating thickness 10-100μm, and glass microsphere diameter 100-200μm.
[0026] (2) Cleaning: The iron-cobalt-nickel-based high-entropy microwave absorbing coating on the electron beam physical vapor deposition glass microspheres was immersed in 10% water-based cleaning agent for 30 minutes. Then, the iron-cobalt-nickel-based high-entropy microwave absorbing coating on the electron beam physical vapor deposition glass microspheres was immersed in deionized water for 30 minutes. The water-based cleaning agent was a degreasing agent with a pH of 7. Specifically, the water-based cleaning agent was an environmentally friendly water-based cleaning agent, a multi-purpose water-based cleaning agent, or a strong water-based cleaning agent.
[0027] (3) Dehydration and drying: The iron-cobalt-nickel-based high-entropy microwave absorbing coating on the electron beam physical vapor deposition glass microspheres was immersed in an organic solvent for 10 min, and then taken out and placed in an oven to dry at 80℃ for 15 min. The organic solvent was acetone or ethanol with analytical grade.
[0028] Example 1:
[0029] High-temperature heat treatment: The cleaned electron beam physical vapor deposition glass microspheres coated with an iron-cobalt-nickel-based high-entropy microwave absorbing coating (specific composition: FeCoNiTiAl) are placed in a vacuum heat treatment furnace and heated to 850℃ with a vacuum degree of 5×10⁻⁶. -3 Pa, after holding at this temperature for 2 hours, cool to 650°C in the furnace, hold at this temperature for 30 minutes, then cool to 200°C in the furnace, hold at this temperature for 30 minutes, then cool to room temperature in the furnace. After cooling to room temperature, open the vacuum chamber and remove the glass microspheres.
[0030] Example 2:
[0031] High-temperature heat treatment: The cleaned electron beam physical vapor deposition glass microspheres coated with an iron-cobalt-nickel-based high-entropy microwave absorbing coating (specific composition: FeCoNiMnPt) are placed in a vacuum heat treatment furnace and heated to 800℃ with a vacuum degree of 3×10⁻⁶. -3 Pa, after holding at this temperature for 3 hours, cool to 600°C in the furnace, hold for 30 minutes, then cool to 250°C in the furnace, hold for 30 minutes, then cool to room temperature in the furnace, and finally open the vacuum chamber to remove the glass microspheres.
[0032] Example 3:
[0033] High-temperature heat treatment: The cleaned electron beam physical vapor deposition glass microspheres coated with an iron-cobalt-nickel-based high-entropy microwave absorbing coating (specific composition: FeCoNiMgZn) are placed in a vacuum heat treatment furnace and heated to 750℃ with a vacuum degree of 3×10⁻⁶. -3 Pa, after holding at this temperature for 4 hours, cool to 550°C in the furnace, hold for 30 minutes, then cool to 300°C in the furnace, hold for 30 minutes, then cool to room temperature in the furnace. After cooling to room temperature, open the vacuum chamber and remove the glass microspheres.
[0034] Comparative example:
[0035] High-temperature heat treatment: The cleaned electron beam physical vapor deposition glass microspheres coated with an iron-cobalt-nickel-based high-entropy microwave absorbing coating (specific composition: FeCoNiWAg) are placed in a vacuum heat treatment furnace and heated to 700℃ with a vacuum degree of 3×10⁻⁶. -3 Pa, after holding at this temperature for 5 hours, cool to 500°C in the furnace, hold for 30 minutes, then cool to 300°C in the furnace, hold for 30 minutes, then cool to room temperature in the furnace, and finally open the vacuum chamber to remove the glass microspheres.
[0036] like Figure 2The figure shows the changes in the bonding strength of the glass microsphere coatings in Examples 1, 2, 3, and the comparative example. It can be seen that due to the differences in the heat preservation temperature parameters and the heat preservation segment parameters, the coating bonding strength in the comparative example is only 5 MPa, while the combination of the heat preservation temperature parameters and the segmented temperature design in Examples 1, 2, and 3 results in coating bonding strengths all above 8 MPa. In the heat treatment process of this invention embodiment, a multi-segment heat preservation method is adopted: the temperature is raised to 800±50℃ in the furnace, held for 2-4 hours, then cooled to 600±50℃ in the furnace, held for 30±5 minutes, then cooled to 250±50℃ in the furnace, held for 30±5 minutes, and then cooled to room temperature in the furnace under vacuum conditions (vacuum degree <1×10⁻⁶). -2 By controlling the insulation time and temperature at each stage under (Pa) conditions, the bonding strength of the coating layer can be improved. On the other hand, from Figure 2 It can also be seen that, since the maximum insulation parameter was changed in the comparative example compared to other embodiments (the temperature was reduced to 700°C compared to other embodiments), the coating bonding strength was found to be significantly reduced.
[0037] In summary, it can be seen that the heat treatment process of this invention employs a multi-stage heat preservation method, which is effective when the vacuum degree is <1×10⁻⁶. -2 Under Pa conditions, by controlling the heat preservation time and temperature at each stage, the bonding strength of the coating layer was increased to 8 MPa, while maintaining the integrity of the microspheres, ultimately improving the material's performance.
[0038] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in the present invention, and these modifications or substitutions should be covered within the protection scope of the present invention.
Claims
1. A heat treatment method for coating glass microspheres with an electron beam physical vapor deposition coating, characterized in that: The heat treatment process is as follows: Electron beam physical vapor deposition (EBPV) coatings were applied to glass microspheres and placed in a vacuum heat treatment furnace. The furnace temperature was then raised to 800±50℃, with a vacuum degree <1×10⁻⁶. -2 Pa, after holding at the temperature for 2-4 hours, cool with the furnace to 600±50℃, hold at the temperature for 30±5 minutes, then cool with the furnace to 250±50℃, hold at the temperature for 30±5 minutes, then cool with the furnace to room temperature, and after cooling to room temperature, open the vacuum chamber and remove the coating. The coating system is an iron-cobalt-nickel based pentagonal high-entropy microwave absorbing coating FeCoNiXY, where X and Y are both metal atoms.
2. The heat treatment method according to claim 1, characterized in that: The diameter of the glass microspheres is 100-200 μm.
3. The heat treatment method according to claim 1, characterized in that: The electron beam physical vapor deposition process parameters are: evaporation current 0.8-1.2A, rotation speed 5-10RPM, coating thickness 10-100μm, and glass microsphere diameter 100-200μm.
4. The heat treatment method according to claim 1, characterized in that: The method further includes the steps of cleaning and dehydrating the coating prior to heat treatment.
5. The heat treatment method according to claim 4, characterized in that: The cleaning steps are as follows: the electron beam physical vapor deposition glass microspheres coated with the iron-cobalt-nickel-based pentagonal high-entropy microwave absorbing coating are immersed in 10±5% water-based cleaning agent for 30±5 min, and then the electron beam physical vapor deposition glass microspheres coated with the iron-cobalt-nickel-based pentagonal high-entropy microwave absorbing coating are immersed in deionized water for 30±5 min.
6. The heat treatment method according to claim 5, characterized in that: The water-based cleaning agent is a degreasing agent with a pH of 7±0.
5.
7. The heat treatment method according to claim 4, characterized in that: The dehydration and drying steps are as follows: the iron-cobalt-nickel-based pentagonal high-entropy microwave absorbing coating on the electron beam physical vapor deposition glass microspheres is immersed in an organic solvent for 10±5 min, and then taken out and placed in an oven to dry at 80±10℃ for 15±5 min.
8. The heat treatment method according to claim 7, characterized in that: The organic solvent is acetone or ethanol, and its purity is analytical grade.
Citation Information
Patent Citations
Ceramic microsphere coated nickel coating and preparation method thereof
CN115368166A
Preparation method for surface strengthening of hollow glass beads based on ion exchange