Cement-based composite material based on fiber reinforcement
By using steel fibers and modified polyvinyl alcohol fibers in cement-based materials, combined with fly ash and fine aggregates, the problems of low tensile strength and high brittleness of traditional cement-based materials are solved, and crack resistance and durability are significantly improved. , reduces costs and performs excellently under extreme conditions.
Patent Information
- Application Number
- CN202411122454.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-15
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of cement-based materials, and more particularly to a cement-based composite material based on fiber reinforcement. Background Art
[0002] In modern construction projects, cement-based composites are an important building material and are widely used in structures such as bridges, tunnels, and buildings. However, traditional cement-based materials have many limitations, such as low tensile strength, high brittleness, and easy cracking. These problems are particularly prominent in certain special applications. In order to improve these defects, fiber reinforcement technology has been gradually introduced in recent years. By adding fiber materials to the cement matrix, its crack resistance, durability, and mechanical properties can be improved.
[0003] At present, commonly used reinforcing fibers include steel fiber, glass fiber, carbon fiber and polymer fiber. Among them, steel fiber is widely used in high-strength concrete materials due to its excellent tensile strength and durability. However, although the single use of steel fiber can significantly improve the crack resistance of cement-based composite materials, its cost is relatively high, and under certain extreme conditions, the performance of the material still has certain deficiencies. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the present invention provides a fiber-reinforced cement-based composite material, and the specific scheme is as follows:
[0005] A fiber-reinforced cement-based composite material comprises the following components in percentage by mass: 5-15% steel fiber; 0.5-5% modified polyvinyl alcohol fiber; 20-30% fly ash; 40-50% cement; 10-20% fine aggregate; and 0.2-1% water reducing agent.
[0006] Furthermore, the length of the steel fiber is 10 to 30 mm, and the diameter is 0.2 to 0.5 mm.
[0007] Furthermore, the length of the polyvinyl alcohol fiber is 5 to 15 mm, and the diameter is 10 to 20 μm.
[0008] Furthermore, the particle size of the fine aggregate is 0.1 to 5 mm.
[0009] Furthermore, the water reducing agent is a polycarboxylic acid water reducing agent.
[0010] Further, the preparation of modified polyvinyl alcohol fiber is as follows:
[0011] S1 pretreatment: the polyvinyl alcohol fiber is cut into a length of 5 to 15 mm and soaked in warm water at 80 to 100°C for 2 to 4 hours to remove surface impurities and low molecular weight components;
[0012] S2 Drying: Dry the pretreated polyvinyl alcohol fiber at 60-80°C for 4-6 hours until the moisture content of the fiber drops below 1%;
[0013] S3 heat treatment: place the dried polyvinyl alcohol fiber in an oven at 150-200°C for heat treatment for 1-3 hours. By controlling the temperature and time, the crystallinity of the fiber is increased to 45-60%, thereby enhancing the strength and modulus of the fiber;
[0014] S4 cooling: the heat-treated polyvinyl alcohol fiber is naturally cooled to 20-25°C at room temperature to ensure the stability of the fiber structure and avoid stress concentration caused by sudden cooling;
[0015] S5 Surface treatment: The cooled polyvinyl alcohol fiber is treated with a silane coupling agent and stirred at 40-60°C for 2-3 hours. The fiber is then filtered, washed and dried again to improve the hydrophilicity of the fiber and the interfacial bonding performance with the cement matrix.
[0016] Furthermore, the concentration of the silane coupling agent in S5 is 1-3%.
[0017] Furthermore, the preparation method comprises the following steps:
[0018] S1: Prepare the raw materials according to 5-15% steel fiber, 0.5-5% modified polyvinyl alcohol fiber, 20-30% fly ash, 40-50% cement, 10-20% fine aggregate and 0.2-1% water reducing agent;
[0019] S2: Mix fine aggregate, fly ash and cement in a low-speed mixer for 3 to 5 minutes, then gradually add steel fiber and modified polyvinyl alcohol fiber and continue mixing for 5 to 7 minutes until they are evenly dispersed;
[0020] S3: Slowly add water and water reducing agent and stir evenly; the stirring time is controlled within 10 to 15 minutes to ensure the uniformity and fluidity of the mixture;
[0021] S4: Pour the well-mixed mixture into a mold and vibrate or tamp it to ensure that the material is dense;
[0022] S5: The molded specimens were cured under standard curing conditions of 20-25°C for 24 hours, then demolded and further cured for 28 days in an environment with a humidity of more than 90% and a temperature of 20-25°C.
[0023] Beneficial effects:
[0024] The present invention provides a fiber-reinforced cement-based composite material, which specifically includes the following advantages:
[0025] (1) Steel fibers form a three-dimensional network structure in the composite material, which can absorb and disperse external stress, thereby significantly enhancing the toughness and impact resistance of the material. Cement-based composites with added steel fibers perform well in compressive strength, flexural strength and elastic modulus, especially in resisting crack propagation and reducing crack width. Modified polyvinyl alcohol fiber, as a flexible fiber material, has excellent toughness and durability. Its addition can further enhance the material's crack resistance at the microscopic level, especially under high strain conditions, and can effectively delay the formation and propagation of cracks. The synergistic effect of modified polyvinyl alcohol fiber and steel fiber makes the composite material have both high strength and high toughness.
[0026] (2) The polyvinyl alcohol fibers in the composite material are first heat treated and then surface treated, which can significantly improve the interfacial bonding between the fibers and the cement matrix. The heat treatment process can improve the thermal stability of the fibers, reduce the internal stress of the fibers, make them more stable during the concrete preparation process, and avoid fiber shedding or interface damage caused by differences in thermal expansion coefficients. The surface treatment uses silane coupling agents to treat the fiber surface, which enhances the chemical bonding between the fibers and the matrix and further improves the overall performance of the material. The treated polyvinyl alcohol fibers can form a stronger interfacial bond when in contact with the cement matrix, improving the material's crack resistance and anti-aging properties. DETAILED DESCRIPTION
[0027] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0028] Embodiment 1:
[0029] A fiber-reinforced cement-based composite material comprises the following components in percentage by weight:
[0030] Steel fiber: 10%
[0031] Modified polyvinyl alcohol fiber: 2%
[0032] Fly ash: 25%
[0033] Cement: 45%
[0034] Fine aggregate: 15%
[0035] Polycarboxylic acid water reducer: 0.5%
[0036] The preparation method of the modified polyvinyl alcohol fiber comprises the following steps:
[0037] (1) Pretreatment: PVA fibers were cut into 10 mm pieces and soaked in 90°C warm water for 3 hours.
[0038] (2) Drying: The pretreated fibers were dried at 70°C for 5 hours until the moisture content of the fibers dropped below 0.5%.
[0039] (3) Heat treatment: Heat treatment in an oven at 180°C for 2 hours.
[0040] (4) Cooling: The fiber is cooled naturally to room temperature (about 23°C).
[0041] (5) Surface treatment: The fiber was stirred in a 1.5% silane coupling agent solution at 50°C for 2.5 hours, filtered, washed and dried.
[0042] The preparation method of cement-based composite material comprises the following steps:
[0043] (1) Raw material preparation: weigh steel fiber, modified polyvinyl alcohol fiber, fly ash, cement, fine aggregate and water reducing agent according to the proportion.
[0044] (2) Mixing: Fine aggregate, fly ash and cement were mixed in a low-speed mixer for 4 minutes, and then steel fiber and modified polyvinyl alcohol fiber were added and mixed for another 6 minutes.
[0045] (3) Add water and stir: Slowly add water and water reducer and stir for 12 minutes to ensure uniformity.
[0046] (4) Molding: Pour the mixture into a mold and vibrate to form it.
[0047] (5) Curing: After molding, cure at 23°C and 95% humidity for 24 hours, then demould and continue curing for another 28 days.
[0048] Embodiment 2:
[0049] A fiber-reinforced cement-based composite material comprises the following components in percentage by weight:
[0050] Steel Fiber: 12%
[0051] Modified polyvinyl alcohol fiber: 3%
[0052] Fly ash: 22%
[0053] Cement: 43%
[0054] Fine aggregate: 18%
[0055] Polycarboxylic acid water reducer: 0.8%
[0056] The preparation method of modified polyvinyl alcohol fiber comprises the following steps:
[0057] (1) Pretreatment: PVA fibers were cut into 8 mm pieces and soaked in 85°C warm water for 3.5 hours.
[0058] (2) Drying: Dry at 75°C for 5 hours until the moisture content of the fiber drops to 0.8%.
[0059] (3) Heat treatment: Heat treatment in an oven at 170°C for 2 hours.
[0060] (4) Cooling: The fiber is cooled naturally to 24°C.
[0061] (5) Surface treatment: The fiber was stirred in a 2% silane coupling agent solution at 55°C for 3 hours, filtered, washed and dried.
[0062] The preparation method of cement-based composite material comprises the following steps:
[0063] (1) Raw material preparation: weigh steel fiber, modified polyvinyl alcohol fiber, fly ash, cement, fine aggregate and water reducing agent according to the proportion.
[0064] (2) Mixing: Fine aggregate, fly ash and cement were mixed in a low-speed mixer for 5 minutes, then steel fiber and modified polyvinyl alcohol fiber were added and mixing was continued for 7 minutes.
[0065] (3) Add water and stir: Slowly add water and water reducer and stir for 13 minutes to ensure uniformity.
[0066] (4) Molding: Pour the mixture into a mold and vibrate to form it.
[0067] (5) Curing: After molding, cure at 24°C and 93% humidity for 24 hours, then demould and continue curing for another 28 days.
[0068] Embodiment 3:
[0069] A fiber-reinforced cement-based composite material comprises the following components in percentage by weight:
[0070] Steel fiber: 15%
[0071] Modified polyvinyl alcohol fiber: 4%
[0072] Fly ash: 28%
[0073] Cement: 42%
[0074] Fine aggregate: 11%
[0075] Polycarboxylic acid water reducer: 1%
[0076] The preparation method of modified polyvinyl alcohol fiber comprises the following steps:
[0077] (1) Pretreatment: PVA fibers were cut into 12 mm pieces and soaked in 95°C warm water for 4 hours.
[0078] (2) Drying: Drying at 80°C for 4.5 hours, the moisture content of the fiber dropped to 0.7%.
[0079] (3) Heat treatment: Heat treatment in an oven at 190°C for 2 hours.
[0080] (4) Cooling: The fiber is cooled naturally to 22°C.
[0081] (5) Surface treatment: The fiber was stirred in a 2.5% silane coupling agent solution at 58°C for 3 hours, filtered, washed and then dried.
[0082] The preparation method of cement-based composite material comprises the following steps:
[0083] (1) Raw material preparation: weigh steel fiber, modified polyvinyl alcohol fiber, fly ash, cement, fine aggregate and water reducing agent according to the proportion.
[0084] (2) Mixing: Fine aggregate, fly ash and cement were mixed in a low-speed mixer for 5 minutes, then steel fiber and modified polyvinyl alcohol fiber were added and mixing was continued for 7 minutes.
[0085] (3) Add water and stir: Slowly add water and water reducer and stir for 15 minutes to ensure uniformity.
[0086] (4) Molding: Pour the mixture into a mold and vibrate to form it.
[0087] (5) Curing: After molding, cure at 24°C and 93% humidity for 24 hours, then demould and continue curing for another 28 days.
[0088] Comparative Example 1:
[0089] The preparation method is similar to that of the embodiment, except that the composite material component does not contain modified polyvinyl alcohol fiber.
[0090] Comparative Example 2:
[0091] The preparation method is similar to that of the embodiment, except that unmodified polyvinyl alcohol fibers are added to the composite material component.
[0092] The cement-based composite materials obtained in Examples 1 to 3 and Comparative Examples 1 and 2 were tested for performance, and the test data are as follows:
[0093] Inspection items Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Compressive strength(MPa) 60.5 63.2 61.8 48.7 54.3 Flexural strength(MPa) 9.8 10.1 9.9 7.2 8.1 Elastic modulus(GPa) 35.2 36.0 35.5 28.4 32.1 Tensile strength(MPa) 7.5 7.9 7.6 5.5 6.3 <![CDATA[Material density (g / cm 3 )]]> 2.35 2.38 2.36 2.25 2.30
[0094] It can be seen from the above table that the embodiment adding modified polyvinyl alcohol fiber significantly improves the overall performance of the cement-based composite material, which has obvious advantages over the comparative example material without adding or adding unmodified polyvinyl alcohol fiber.
[0095] As a further improvement, the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A fiber-reinforced cement-based composite material, characterized in that: The cement-based composite material comprises the following components in percentage by mass: 5 to 15% steel fiber; Modified polyvinyl alcohol fiber 0.5-5%; fly ash 20-30%; cement 40-50%; fine aggregate 10-20%; water reducing agent 0.2-1%.
2. A fiber-reinforced cement-based composite material according to claim 1, characterized in that: The length of the steel fiber is 10 to 30 mm and the diameter is 0.2 to 0.5 mm.
3. The fiber-reinforced cement-based composite material according to claim 1, characterized in that: The length of the polyvinyl alcohol fiber is 5 to 15 mm and the diameter is 10 to 20 μm.
4. The fiber-reinforced cement-based composite material according to claim 1, characterized in that: The particle size of fine aggregate is 0.1 to 5 mm.
5. The fiber-reinforced cement-based composite material according to claim 1, characterized in that: The water reducing agent is a polycarboxylic acid water reducing agent.
6. The fiber-reinforced cement-based composite material according to claim 1, characterized in that: The preparation of modified polyvinyl alcohol fiber is as follows: S1 pretreatment: cut the polyvinyl alcohol fiber to 5-15 mm and soak it in warm water at 80-100°C for 2-4 hours; S2 Drying: Dry the pretreated polyvinyl alcohol fiber at 60-80°C for 4-6 hours until the moisture content of the fiber drops to less than 1%; S3 heat treatment: placing the dried polyvinyl alcohol fiber in an oven at 150-200°C for heat treatment for 1-3 hours; S4 cooling: cooling the heat-treated polyvinyl alcohol fiber naturally to 20-25° C. at room temperature; S5 Surface treatment: The cooled polyvinyl alcohol fiber is treated with a silane coupling agent and stirred at 40 to 60° C. for 2 to 3 hours, and then the fiber is filtered, washed and dried again.
7. The fiber-reinforced cement-based composite material according to claim 6, characterized in that: The concentration of the silane coupling agent in S5 is 1 to 3%.
8. The method for preparing a fiber-reinforced cement-based composite material according to claim 1, characterized in that: The preparation method comprises the following steps: S1: Prepare the raw materials according to 5-15% steel fiber, 0.5-5% modified polyvinyl alcohol fiber, 20-30% fly ash, 40-50% cement, 10-20% fine aggregate and 0.2-1% water reducing agent; S2: fine aggregate, fly ash and cement are mixed in a low-speed mixer for 3 to 5 minutes, and then steel fiber and modified polyvinyl alcohol fiber are gradually added and mixed for 5 to 7 minutes until they are evenly dispersed; S3: Slowly add water and water reducing agent and stir evenly; the stirring time is controlled within 10 to 15 minutes to ensure the uniformity and fluidity of the mixture; S4: Pour the well-mixed mixture into a mold and vibrate or tamp it to ensure that the material is dense; S5: The molded specimens were cured under standard curing conditions of 20-25°C for 24 hours, then demolded and further cured for 28 days in an environment with a humidity of more than 90% and a temperature of 20-25°C.
Citation Information
Patent Citations
Cement-based composite material with high strength, high ductility, and high water resistance and preparation method of cement-based composite material
CN107382180A
High-tenacity polyvinyl alcohol fiber
JP1990210015A
Polyvinyl alcohol based fiber and its production
JP1998310939A