Preparation method of high-performance compressed desert sand concrete

By compressive pouring and chemical treatment in concrete, desert sand replaces natural river sand, solving the problem of poor desert sand grade, significantly improving the mechanical properties and durability of concrete, and achieving the goal of 100% replacement of desert sand.

CN118930173APending Publication Date: 2024-11-12SHENZHEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411002731.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

Smart Images

  • Figure CN118930173A_ABST
    Figure CN118930173A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of building materials, and particularly relates to a preparation method of high-performance compressed desert sand concrete. The preparation method of the high-performance compressed desert sand concrete provided by the invention comprises the following steps: mixing cement, coarse aggregate, fine aggregate and water, and sequentially carrying out compression pouring and maintenance to obtain the high-performance compressed desert sand concrete, the pressure of compression pouring is 2 MPa or above, and the time of compression pouring is 2 min or above. The desert sand is used for replacing natural river sand to serve as fine aggregate, concrete defects caused by direct use of the desert sand for replacing the natural river sand can be effectively reduced through compression pouring, and 100% replacement of the natural river sand by the desert sand is achieved on the premise that the excellent mechanical property and durability of desert sand concrete are guaranteed; the obtained high-performance compressed desert sand concrete is improved in mechanical property and durability and good in comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a method for preparing high-performance compressed desert sand concrete. Background Art

[0002] Concrete has become one of the most widely used building materials in the engineering industry due to its easy availability of raw materials, excellent performance and economy. Concrete production requires a large amount of sand and gravel aggregates, and many countries are facing the problem of shortage of natural resources such as sand and gravel. In recent years, with the intensification of desertification, people have begun to pay attention to the resource utilization of desert sand, trying to solve the problem of scarcity of natural river sand and achieve the goal of controlling desertification.

[0003] However, compared with natural river sand, the properties of desert sand are very different: natural river sand usually has a uniform particle size distribution, good grading and excellent quality, while desert sand has poor grading, the particles are mostly round and smooth, the fineness is high, and the physical and mechanical properties are relatively weak.

[0004] The researchers prepared desert sand concrete by direct substitution. In the process of preparing concrete, desert sand was directly added to replace natural river sand as the fine aggregate of concrete. However, due to the poor gradation of desert sand, the particles are round and smooth, and the fineness is high, resulting in poor durability and mechanical properties of concrete, and the substitution rate of desert sand in concrete is low. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing high-performance compressed desert sand concrete. The preparation method provided by the present invention achieves 100% replacement of desert sand without reducing the mechanical properties and durability of concrete.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The invention provides a preparation method of high-performance compressed desert sand concrete, comprising the following steps: mixing cement, coarse aggregate, fine aggregate and water, and then compressing, casting and curing in sequence to obtain high-performance compressed desert sand concrete; the compression casting comprises filling the mixed fresh concrete mixture into a steel mold and pressurizing the mixture simultaneously; the fine aggregate comprises river sand and desert sand in a mass ratio of 0 to 99:1 to 100; the pressure of the compression casting is above 2 MPa, and the time of the compression casting is above 2 min.

[0008] Preferably, the mass ratio of water to cement is 0.1 to 0.7:1.

[0009] Preferably, the mass ratio of cement to coarse aggregate is 1:0.5-10.

[0010] Preferably, the desert sand is chemically treated before use; the chemical treatment includes one or more of acid leaching, alkali leaching and heat treatment.

[0011] Preferably, the acid used for the acid leaching includes one or more of hydrochloric acid and sulfuric acid.

[0012] Preferably, the mixed raw materials further include one or more of metal mesh and fiber; the fiber includes one or more of steel fiber and synthetic fiber.

[0013] Preferably, the total volume of the metal mesh and the fibers accounts for less than 2% of the high performance compressed desert sand concrete.

[0014] Preferably, the pressurization time is 24 hours.

[0015] Preferably, the curing temperature is 18-30° C., the relative humidity is above 60%, and the curing time is 14-28 days.

[0016] Preferably, the high-performance compressed desert sand concrete is used to manufacture desert sand bricks, desert sand blocks, desert sand prefabricated pipes, desert sand prefabricated building beams, desert sand prefabricated building walls or desert sand prefabricated building panels.

[0017] The present invention provides a method for preparing high-performance compressed desert sand concrete. The present invention uses desert sand to replace natural river sand as fine aggregate, and through compression and pouring, can effectively reduce the mechanical properties and durability defects of concrete caused by directly using desert sand to replace natural river sand. On the premise of ensuring that the mechanical properties and durability of desert sand concrete are excellent (compared with direct replacement with desert sand), 100% replacement of natural river sand by desert sand is achieved, and the obtained high-performance compressed desert sand concrete has improved mechanical properties and durability, and good comprehensive performance.

[0018] The results of the embodiments show that compared with the river sand concrete and desert sand concrete of the comparative examples, the compressive strength, elastic modulus and splitting tensile strength of the high-performance compressed desert sand concrete of the present invention are respectively increased by 125%, 82% and 70%; as the desert sand content increases, the increase is particularly obvious; compared with the natural river sand concrete of the comparative example, the water absorption rate of the high-performance compressed desert sand concrete of the present invention is reduced by 41%, 38% and 27% respectively; as the desert sand content increases, the carbonation resistance and chloride ion penetration resistance of the comparative example concrete also decrease, but compression casting significantly improves the carbonation resistance and chloride ion penetration resistance of the high-performance compressed desert sand concrete, so that the carbonation resistance of the high-performance compressed desert sand concrete is increased by 100%, and the chloride ion penetration resistance is increased by 64%.

[0019] The preparation method provided by the present invention is expected to bring significant benefits, so that high-performance compressed desert sand concrete can be applied to actual engineering structures. It can be used to prepare desert sand bricks, desert sand blocks, desert sand prefabricated pipes, desert sand prefabricated building beams, desert sand prefabricated building walls or desert sand prefabricated building panels, etc., to promote environmental sustainable development and the innovation and application of green high-performance building materials, thereby solving the problem of scarce natural river sand resources and contributing to desertification control and global sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 A process flow chart of a method for preparing high-performance compressed desert sand concrete provided by the present invention;

[0022] Figure 2 is the gradation curve of coarse aggregate (a) and fine aggregate (b) of Examples 1 to 9 and Comparative Examples 1 to 9;

[0023] Figure 3 The process flow chart of the preparation of high performance compressed desert sand concrete of the embodiment and the preparation of comparative concrete;

[0024] Figure 4 Preparation device (a) and testing device (b) used in Examples 1 to 9 and Comparative Examples 1 to 9;

[0025] Figure 5 It is the compressive strength diagram of concrete of Examples 1 to 9 and Comparative Examples 1 to 9;

[0026] Figure 6 It is the elastic modulus diagram of concrete of Examples 1 to 9 and Comparative Examples 1 to 9;

[0027] Figure 7 It is a graph of splitting tensile strength of concrete of Examples 1 to 9 and Comparative Examples 1 to 9;

[0028] Figure 8 It is the water absorption graph of the concrete of Examples 1 to 9 and Comparative Examples 1 to 9;

[0029] Fig. 9 The carbonization depth diagram of the concrete of Examples 1 to 9 and Comparative Examples 1 to 9;

[0030] Fig.10 Graph showing chloride ion migration coefficients of concrete of Examples 1 to 9 and Comparative Examples 1 to 9. DETAILED DESCRIPTION

[0031] The invention provides a preparation method of high-performance compressed desert sand concrete, comprising the following steps: mixing cement, coarse aggregate, fine aggregate and water, and then compressing, casting and curing in sequence to obtain high-performance compressed desert sand concrete; the compression casting comprises filling the mixed fresh concrete mixture into a steel mold and pressurizing the mixture simultaneously; the fine aggregate comprises river sand and desert sand in a mass ratio of 0 to 99:1 to 100; the pressure of the compression casting is above 2 MPa, and the time of the compression casting is above 2 min.

[0032] The present invention mixes cement, coarse aggregate, fine aggregate and water. The present invention has no special requirements on the usage of cement, coarse aggregate, fine aggregate and water.

[0033] In the present invention, the cement is preferably Portland cement, more preferably P.O42.5 silicate cement.

[0034] In the present invention, the mass ratio of water to cement is preferably 0.1 to 0.7:1, more preferably 0.3 to 0.6:1, and further preferably 0.4 to 0.5:1.

[0035] In the present invention, the coarse aggregate is preferably determined according to the specification of "Pebbles and Crushed Stones for Construction" GB / T 14685:2011.

[0036] In the present invention, the coarse aggregate is preferably dried before use; the drying is preferably oven drying.

[0037] In the present invention, the mass ratio of cement to coarse aggregate is preferably 1:0.5-10, more preferably 1:1-7, and further preferably 1:4-5.

[0038] In the present invention, the river sand of the fine aggregate is preferably determined according to the specification of "Construction Sand" GB / T 14684:2011, and is more preferably natural river sand.

[0039] In the present invention, the fine aggregate is preferably dried before use; the drying is preferably oven drying.

[0040] In the present invention, the gradation of the coarse aggregate and the fine aggregate is preferably determined according to ASTM C33:2016 standard.

[0041] In the present invention, there is no requirement for the origin of the desert sand; in a specific embodiment of the present invention, the desert sand is preferably taken from the Kubuqi Desert in the northwest of China's Inner Mongolia Autonomous Region; the desert sand is preferably chemically treated before use; the chemical treatment preferably includes one or more of acid leaching, alkali leaching and heat treatment.

[0042] In the present invention, the acid used for acid leaching preferably includes one or more of hydrochloric acid and sulfuric acid; the alkali used for alkali leaching preferably includes one or more of metal hydroxides, carbonates and bicarbonates; the metal hydroxide preferably includes one or more of sodium hydroxide and potassium hydroxide; the carbonate is preferably sodium carbonate; the bicarbonate is preferably sodium bicarbonate; the heat treatment is preferably: washing the desert sand with water and then drying; the drying temperature is preferably 110°C, and the insulation time is preferably 24h. The present invention removes impurities through chemical treatment.

[0043] In the present invention, the desert sand is preferably dried before use (when chemical treatment is involved, preferably chemical treatment is performed first and then drying); the drying is preferably oven drying.

[0044] In the present invention, the mass ratio of river sand to desert sand is preferably 0-90:10-100, more preferably 0-60:40-100, and further preferably 0:100. The preparation method provided by the present invention can use 1-100% desert sand to replace fine aggregates such as natural river sand, and improve the mechanical properties and durability of high-performance compressed desert sand concrete.

[0045] In the present invention, the mixed raw materials preferably further include one or more of metal mesh and fiber; the metal mesh is preferably a steel mesh; and the fiber preferably includes one or more of steel fiber and synthetic fiber.

[0046] In the present invention, the total volume of the metal mesh and the fiber is preferably less than 2% of the high performance compressed desert sand concrete, more preferably 1-2%. The preparation method provided by the present invention has a similar performance improvement effect on fiber concrete as that on desert sand concrete, and the degree of improvement in mechanical properties such as strength is different depending on the type and amount of fiber.

[0047] In the present invention, the mixed raw materials preferably further include a water reducer; the water reducer is preferably a modified polycarboxylate water reducer; the mass ratio of the water reducer to cement is preferably 0.5 to 3:100, more preferably 1 to 2:100.

[0048] In the present invention, the mixing is preferably stirring; the stirring is preferably performed according to ASTM C192:2016 standard.

[0049] After mixing, the present invention sequentially performs compression casting and curing to obtain high-performance compressed desert sand concrete. In the present invention, the compression casting mold is a steel mold; the steel mold is preferably a cylindrical mold, a cubic mold, a cuboid mold or a special-shaped mold.

[0050] In the present invention, the compression pouring pressure is preferably above 2 MPa, more preferably 2-30 MPa, further preferably 10-25 MPa, and further preferably 15-20 MPa. The compression pouring time is preferably above 2 min, more preferably 2-1440 min.

[0051] In the present invention, the pressurization time is preferably 24 hours.

[0052] In the present invention, the compression casting preferably further includes removing the mold.

[0053] In the present invention, the curing temperature is preferably 18-30°C, more preferably 20-24°C, the relative humidity is preferably above 60%, more preferably 80-100%, further preferably 95-100%, the curing time is preferably 14-28 days, more preferably 21-28 days; the curing is preferably carried out in a standard curing room.

[0054] The preparation method of the high-performance compressed desert sand concrete provided by the present invention has a process flow chart as shown in FIG. Figure 1 As shown. The preparation method of high-performance compressed desert sand concrete provided by the present invention comprises the following steps: mixing cement, coarse aggregate, fine aggregate and water, and then performing compression casting (the present invention) or non-compression casting (comparative example), and then performing curing to obtain high-performance compressed desert sand concrete, after which the high-performance compressed desert sand concrete can be further tested for performance. The preparation method provided by the present invention is suitable for preparing compressed casting desert sand cement mortar materials and structures, such as desert sand bricks, blocks, prefabricated pipes, prefabricated building beams, prefabricated building walls and prefabricated building panels.

[0055] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.

[0056] Example

[0057] In this embodiment, desert sand was taken from the Kubuqi Desert in the northwest of Inner Mongolia Autonomous Region, China; coarse aggregate (stone) and natural river sand were taken from Shenzhen, China; cement was ordinary Portland cement (P.O42.5), water was tap water, and the admixture was a high-efficiency water reducer (modified polycarboxylate water reducer);

[0058] The gradation of coarse aggregate and fine aggregate is as follows: Figure 2 The physical and mechanical properties of coarse aggregate and fine aggregate are shown in Table 1 and Table 2; the water-cement ratio used is 0.7 and 0.3; the natural river sand is replaced by desert sand (by weight), and the replacement rates are 0%, 50% and 100% respectively;

[0059] Table 1 Physical and mechanical properties of coarse aggregate

[0060] Performance Indicators coarse aggregate <![CDATA[Bulk density (kg / m 3 )]]> 1609 Water absorption (%) 0.83 Saturated surface dry weight 2.58 Drying specific gravity 2.56 Apparent specific gravity 2.61

[0061] Table 2 Physical and mechanical properties of fine aggregate

[0062] Performance Indicators river sand Desert Sand <![CDATA[Bulk density (kg / m 3 )]]> 1729 1582 Water absorption (%) 2.90 1.83 Fineness modulus 2.69 0.94

[0063] All aggregates were dried for 24 hours before mixing and mixed using a double-shaft mixer according to ASTM C192:2016 standard; after mixing, high-performance compressed desert sand concrete and ordinary desert sand concrete (uncompressed casting) of the present invention were prepared respectively. The preparation process is as follows: Figure 3 The preparation and testing equipment are shown in Figure 4 As shown;

[0064] The specifications and proportions of the prepared concrete are shown in Table 3. The dimensions are 100 mm × 200 mm (diameter × height), and the design strength grades are C30, C50 and C70 (i.e., 30, 50 and 70 MPa), respectively; wherein the concrete name indicates the target strength, desert sand replacement rate and whether it is compressed and cast. For example, C50-D50-P represents concrete with a target strength of 50 MPa, 50% of natural river sand replaced by desert sand and compressed and cast, and C50 represents ordinary natural sand concrete with a desert sand replacement rate of 0% (uncompressed and cast).

[0065] Table 3 Specifications and proportions of concrete prepared in Examples 1 to 9 and Comparative Examples 1 to 9

[0066]

[0067]

[0068] The preparation method of desert sand concrete in this embodiment is as follows:

[0069] P.O42.5 silicate cement, coarse aggregate, fine aggregate (river sand and desert sand) and water are mixed, and then the fresh concrete obtained by the mixture is compressed and poured in a steel mold (the pressure is above 2MPa, and the compression pouring time is above 2min), the steel mold is placed at room temperature for 24h, and then the mold is taken out, and then cured for 14 to 28 days in a standard curing room with a temperature of 18 to 30°C and a relative humidity of above 60% to obtain desert sand concrete.

[0070] Test Example 1

[0071] The compressive strength test of the concrete prepared in Examples 1 to 9 and Comparative Examples 1 to 9 was carried out according to ASTM C39:2021. Figure 5 As shown. Figure 5It can be seen that compared with the comparative example C30 concrete, the compressive strength of the comparative examples C30-D50 and C30-D100 concretes decreased by 7% and 14% respectively; similarly, compared with the comparative examples C50 and C70 concretes, the compressive strength of the comparative examples C50-D50 and C50-D100, C70-D50 and C70-D100 concretes decreased by 7% and 10%, 2% and 9% respectively; compared with the relatively high strength mixes (i.e. C50 and C70), the compressive strength of the comparative example concrete with a low strength mix (i.e. C30) decreased by a greater margin; compared with the comparative examples C30, C50 and C70 concretes, the compressive strength of the comparative examples C30-D100, C50-D100 and C70-D100 concretes decreased by 14%, 10% and 9% respectively. It can be seen that with the increase of desert sand content, the compressive strength of all comparative examples of concrete will decrease.

[0072] In the example concretes, different effects of desert sand content can be observed for each concrete mix (i.e., C30, C50, and C70): compared with the example C30 concrete, the compressive strengths of the example C30-D50 and C30-D100 concretes were increased by 5% and 7%, respectively, which was attributed to the combined effects of desert sand and compression casting to improve the concrete pore structure.

[0073] Compared with the concrete of comparative examples C30, C30-D50 and C30-D100, the compressive strength of the concrete of embodiment C30, C30-D50 and C30-D100 increased by 81%, 105% and 125% respectively; similarly, compared with the concrete of comparative examples C50, C50-D50 and C50-D100, the compressive strength of the concrete of embodiment C50, C50-D50 and C50-D100 increased by 67%, 79% and 88% respectively; compared with the concrete of comparative examples C70, C70-D50 and C70-D100, the compressive strength of the concrete of embodiment C70, C70-D50 and C70-D100 also increased by 55%, 58% and 67% respectively. It can be seen that the preparation method provided by the present invention can significantly improve the compressive strength of high-performance compressed desert sand concrete through compression casting.

[0074] Test Example 2

[0075] The concrete prepared in Examples 1 to 9 of the present invention and Comparative Examples 1 to 9 was tested for elastic modulus in accordance with ASTM C469:2014. The results are as follows: Figure 6 As shown. Figure 6It can be seen that for the comparative examples, as the desert sand content increases, the elastic modulus of all comparative example concretes decreases: compared with the comparative example C30 concrete, the elastic modulus of comparative examples C30-D50 and C30-D100 concretes decreases by 6% and 16%, respectively; similarly, compared with the comparative example C50 concrete, the comparative examples C50-D50 and C50-D100 concretes decrease by 6%, respectively; compared with the comparative example C70 concrete, the comparative examples C70-D50 and C70-D100 concretes decrease by 1% and 4%, respectively.

[0076] The elastic modulus of the low-strength mix (i.e., C30) concrete decreased more significantly than that of the relatively higher-strength mixes (i.e., C50 and C70): the elastic modulus of the C30-D100, C50-D100, and C70-D100 concretes decreased by 16%, 6%, and 4%, respectively, compared with the C30, C50, and C70 concretes.

[0077] Compared with Example C30 concrete, the elastic modulus of Example C30-D50 and C30-D100 concrete increased by 4% and 11%, respectively, which was attributed to the combined effect of desert sand and compression casting to improve the pore structure of concrete; compared with Example C50 concrete, there was no obvious difference in the elastic modulus of Example C50-D50 and C50-D100 concrete; similarly, the elastic modulus of Example C70-D50 concrete was similar to that of Example C70 concrete; however, compared with Example C70 concrete, the elastic modulus of Example C70-D100 concrete was slightly reduced by 3%.

[0078] Compared with the concrete of comparative examples C30, C30-D50 and C30-D100, the elastic modulus of the concrete of embodiment C30, C30-D50 and C30-D100 increased by 38%, 54% and 82% respectively; similarly, compared with the concrete of comparative examples C50, C50-D50 and C50-D100, the elastic modulus of the concrete of embodiment C50, C50-D50 and C50-D100 increased by 32%, 40% and 40% respectively; compared with the concrete of comparative examples C70, C70-D50 and C70-D100, the elastic modulus of the concrete of embodiment C70, C70-D50 and C70-D100 increased by 25%, 28% and 26% respectively. It can be seen that the elastic modulus of high-performance compressed desert sand concrete can be significantly improved by compression casting.

[0079] Test Example 3

[0080] The concrete prepared in Examples 1 to 9 of the present invention and Comparative Examples 1 to 9 was subjected to a splitting tensile strength test in accordance with ASTM C496:2017. The results are as follows: Figure 7 As shown. Figure 7 It can be seen that for the comparative concretes, as the desert sand content increases, the splitting tensile strength of all concretes decreases: compared with the comparative example C30 concrete, the comparative examples C30-D50 and C30-D100 concretes decrease by 6% and 10%, respectively; similarly, compared with the comparative example C50 concrete, the comparative examples C50-D50 and C50-D100 concretes decrease by 5% and 8%, respectively; compared with the comparative example C70 concrete, the comparative examples C70-D50 and C70-D100 concretes decrease by 3% and 7%, respectively.

[0081] The splitting tensile strength of the comparative concrete with a low strength mix (i.e., C30) decreased more significantly than that of the comparative concretes with relatively higher strengths (i.e., C50 and C70): the splitting tensile strength of the comparative concretes C30-D100, C50-D100, and C70-D100 decreased by 10%, 8%, and 7%, respectively, compared to the comparative concretes C30, C50, and C70.

[0082] Compared with Example C30 concrete, the splitting tensile strength of Example C30-D50 and C30-D100 concretes increased slightly by 5% and 9%, respectively; compared with Example C50 concrete, there was no significant difference in splitting tensile strength between Example C50-D50 and C50-D100 concretes; similarly, the splitting tensile strength of Example C70-D50 concrete was similar to that of Example C70 concrete; however, compared with Example C70 concrete, the splitting tensile strength of Example C70-D100 concrete decreased slightly by 4%.

[0083] Compared with the concrete of comparative examples C30, C30-D50 and C30-D100, the splitting tensile strength of the concrete of embodiment C30, C30-D50 and C30-D100 increased by 42%, 59% and 70% respectively; similarly, compared with the concrete of comparative examples C50, C50-D50 and C50-D100, the splitting tensile strength of the concrete of C50, C50-D50 and C50-D100 increased by 22%, 29% and 30% respectively after compression casting; compared with the concrete of comparative examples C70, C70-D50 and C70-D100, the splitting tensile strength of the concrete of embodiment C70, C70-D50 and C70-D100 also increased by 17%, 20% and 20% respectively. It can be seen that the present invention can significantly improve the splitting tensile strength of high-performance compressed desert sand concrete through compression casting.

[0084] Test Example 4

[0085] The water absorption of concrete is crucial, as it determines whether harmful ions can penetrate into the concrete, leading to durability problems and reduced mechanical properties.

[0086] The concrete prepared in Examples 1 to 9 of the present invention and Comparative Examples 1 to 9 was tested for water absorption in accordance with ASTM C642:2013. The results are as follows: Figure 8 shown.

[0087] according to Figure 8 It can be seen that with the increase of desert sand content, the water absorption rate of concrete is also increasing: compared with the comparative examples C30, C50 and C70 concretes, the water absorption rates of the comparative examples C30-D100, C50-D100 and C70-D100 concretes after immersion in water are 9%, 6% and 4% respectively; the reason for the increase in the water absorption rate of the comparative concrete after adding desert sand may be that the poor grading of desert sand leads to pores in the desert sand concrete, which in turn leads to an increase in water absorption rate.

[0088] Compared with the comparative concrete, the water absorption of the concretes of all the embodiments is significantly reduced: compared with the comparative concretes of C30, C50 and C70, the water absorption of the concretes of embodiments C30, C50 and C70 is reduced from 8%, 5% and 3% to 5%, 3% and 2%; similarly, compared with the comparative concretes of C30-D100, C50-D100 and C70-D100, the water absorption of the concretes of embodiments C30-D100, C50-D100 and C70-D100 after immersion in water is reduced from 9%, 6% and 4% to 5%, 3% and 2%; in addition, compared with the comparative concretes of C30, C50 and C70, the water absorption of the concretes of embodiments C30-D100, C50-D100 and C70-D100 after immersion in water is reduced by 41%, 38% and 27%, respectively. It can be seen that the present invention can significantly reduce the water absorption rate of high-performance compressed desert sand concrete through compression casting, thereby making the high-performance compressed desert sand concrete structure more compact and durable.

[0089] Test Example 5

[0090] Carbonization of cement-based materials in concrete can aggravate steel corrosion and reduce the durability of concrete structures. Excessive carbon dioxide infiltrating into the pore structure of concrete can corrode calcium silicate hydrates, produce cracks and large pores, affect porosity, strength and chemical composition, and lead to cracking, shrinkage and durability problems.

[0091] The carbonation resistance of the concrete prepared in Examples 1 to 9 of the present invention and Comparative Examples 1 to 9 was tested in accordance with GB / T 50082:2009. The results are as follows: Fig. 9 As shown. Fig. 9It can be seen that the carbonation depth increases with the increase of desert sand content: compared with the comparative examples C30, C50 and C70 concretes, the carbonation depth of the comparative examples C30-D100, C50-D100 and C70-D100 concretes increases from 40, 18 and 11 mm to 48, 21 and 15 mm.

[0092] Compared with the comparative example concrete, the carbonation resistance of the concretes of all the embodiments is significantly improved: compared with the comparative example C30, C50 and C70 concretes, the carbonation depths of the concretes of embodiments C30, C50 and C70 are reduced from 40, 18 and 11 mm to 10, 1 and 0 mm; similarly, compared with the comparative example C30-D100, C50-D100 and C70-D100 concretes, the carbonation depths of the concretes of embodiments C30-D100, C50-D100 and C70-D100 are reduced from 48, 21 and 15 mm to 9, 1 and 0 mm.

[0093] Compared with the comparative examples C30, C50 and C70 concrete, the carbonation resistance of the concrete of the examples C30-D100, C50-D100 and C70-D100 was increased by 77%, 94% and 100%, respectively. The significant improvement in the carbonation resistance of the concrete of the examples is due to the reduction of porosity by compression casting, and the reduction of porosity effectively blocks the path of carbon dioxide diffusion from the atmosphere to the concrete, thereby reducing the carbonation depth. It can be seen that the present invention can significantly improve the carbonation resistance of high-performance compressed desert sand concrete through compression casting, thereby effectively reducing the penetration of carbon dioxide and improving the corrosion resistance of desert sand reinforced concrete structural components.

[0094] Test Example 6

[0095] Corrosion of reinforced concrete structures due to chloride intrusion is a serious deterioration mechanism that depends primarily on the transport capacity of chloride ions.

[0096] The concrete prepared in Examples 1 to 9 of the present invention and Comparative Examples 1 to 9 was tested for its chloride ion penetration resistance in accordance with NT-Build 492:2011. The results are as follows: Fig.10 As shown. Fig.10 It can be seen that with the increase of desert sand content, the resistance of concrete to chloride ion penetration decreases: compared with the comparative examples C30, C50 and C70 concrete, the chloride ion rapid migration coefficient (D RCM ) from 48×10 -12 , 20×10 -12 and 10×10 -12 m 2 / sec increased to 54×10 -12, 22×10 -12 and 14×10 -12 m 2 / sec.

[0097] Compared with the concrete of the comparative example, the chloride ion resistance of the concrete of all the examples is significantly improved: compared with the concrete of the comparative example C30, C50 and C70, the D RCM Value from 48×10 -12 , 20×10 -12 and 10×10 -12 m 2 / sec decreased to 19×10 -12 ,7×10 -12 and 3×10 -12 m 2 / sec; Similarly, compared with the comparative examples C30-D100, C50-D100 and C70-D100 concrete, the D RCM Value from 48×10 -12 , 20×10 -12 and 10×10 -12 m 2 / sec decreased to 18×10 -12 ,7×10 -12 and 4×10 -12 m 2 / sec; In addition, compared with the comparative examples C30, C50 and C70 concrete, the D RCM The values ​​were reduced by 62%, 63% and 64% respectively. It can be seen that the present invention can significantly improve the chloride ion penetration resistance of high-performance compressed desert sand concrete through compression casting, making it a feasible solution for improving the durability of concrete structures.

[0098] It can be seen from the above embodiments that the high-performance compressed desert sand concrete obtained by the preparation method provided by the present invention shows a significant performance improvement effect. Its compressive strength, elastic modulus and splitting tensile strength are increased by 125%, 82% and 70% respectively, and its water absorption resistance, chloride ion resistance and carbonization resistance are also increased by 41%, 64% and 100% respectively.

[0099] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing high-performance compressed desert sand concrete, It is characterized in that The following steps are involved: The cement, coarse aggregate, fine aggregate and water are mixed and compressed, poured and cured in sequence to obtain high-performance compressed desert sand concrete; The compression casting comprises filling the fresh concrete mixture obtained by mixing into a steel mold while applying pressure; The fine aggregate includes river sand and desert sand in a mass ratio of 0 to 99:1 to 100; The compression pouring pressure is above 2 MPa, and the compression pouring time is above 2 min.

2. The preparation method according to claim 1, It is characterized in that The curing temperature is 18-30° C., the relative humidity is above 60%, and the curing time is 14-28 days.

3. The preparation method according to claim 1, It is characterized in that The pressurization time is 24 hours.

4. The preparation method according to claim 1, It is characterized in that The mass ratio of water to cement is 0.1-0.7:

1.

5. The preparation method according to claim 1 or 4, It is characterized in that The mass ratio of the cement to the coarse aggregate is 1:0.5-10.

6. The preparation method according to claim 1, It is characterized in that The desert sand is chemically treated before use; The chemical treatment includes one or more of acid leaching, alkali leaching and heat treatment.

7. The preparation method according to claim 6, It is characterized in that The acid used for the acid leaching includes one or more of hydrochloric acid and sulfuric acid.

8. The preparation method according to claim 1, It is characterized in that The mixed raw materials also include one or more of metal mesh and fiber; The fibers include one or more of steel fibers and synthetic fibers.

9. The preparation method according to claim 8, It is characterized in that The total volume of the metal mesh and the fibers accounts for less than 2% of the high performance compressed desert sand concrete.

10. The preparation method according to claim 1, It is characterized in that The high-performance compressed desert sand concrete is used to manufacture desert sand bricks, desert sand blocks, desert sand prefabricated pipes, desert sand prefabricated building beams, desert sand prefabricated building walls or desert sand prefabricated building panels.