Heat storage material with enhanced heat conductivity and preparation method thereof
By introducing thermally conductive core-shell molten salt and additives into the thermal storage material, a thermal conductivity pathway is formed, which solves the problem of insufficient heat transfer capacity in high-altitude areas and achieves efficient heat transfer and storage, making it suitable for applications in cold and high-altitude regions.
Patent Information
- Application Number
- CN202410989286.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Existing high-temperature solid thermal energy storage materials have insufficient heat transfer capacity in high-altitude areas, resulting in reduced heat transfer efficiency and failing to meet the application needs of cold and high-altitude regions.
By using thermally conductive enhanced thermal storage materials, a thermally conductive pathway is formed by uniformly distributing core-shell molten salt and additives in the matrix. By combining a specific ratio of matrix, core-shell molten salt and additives, a thermal storage material with high thermal conductivity is prepared.
It improves the thermal conductivity of thermal storage materials, enabling efficient heat transfer and storage in high-altitude areas, and enhancing the thermal utilization efficiency of solid thermal storage technology.
Smart Images

Figure CN118931504A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of energy storage materials, and in particular to a heat storage material with enhanced thermal conductivity and a preparation method thereof. Background Art
[0002] Phase change heat storage materials are the core of phase change electric heat storage technology and the key to the efficient storage and release of electric heat storage devices. Therefore, they have high requirements on their heat storage density, thermal conductivity, stability and cost. Phase change heat storage materials have a great influence on heat storage technology. Therefore, research on low-cost, high heat storage density and high thermal conductivity heat storage materials is of great significance.
[0003] As an energy conversion and storage material, high-temperature composite phase change heat storage materials have the advantages of a wide range of operating temperatures and high heat storage capacity. They can be widely used in civil heating, industrial and commercial heating, renewable energy consumption, power grid frequency modulation and other fields. However, when used in high-altitude areas, due to the low local air pressure and thin air, the heat transfer capacity and efficiency are reduced. The common high-temperature solid-state heat storage materials for electric heat storage, such as magnesium bricks and inorganic salt composite phase change materials, have high costs and insufficient thermal conductivity to support efficient heat transfer and heat exchange in high-altitude and cold areas. Therefore, it is necessary to develop a heat storage material with high heat storage and high thermal conductivity to meet the application of heat storage technology in high-altitude and cold areas. Summary of the invention
[0004] In order to overcome the above-mentioned deficiencies of the prior art, the present application provides a heat storage material with enhanced thermal conductivity and a preparation method thereof, which specifically adopts the following technical solutions:
[0005] A thermal storage material with enhanced thermal conductivity comprises a matrix, a core-shell molten salt and an additive, wherein the mass ratio of the matrix, the core-shell molten salt and the additive is 25-65:20-45:5-20; the core-shell molten salt is randomly and evenly distributed in the matrix; the core-shell molten salt is an inorganic salt wrapped by a thermal conductivity enhancing material, the inner layer of the core-shell molten salt is a plurality of inorganic salt particles, and the additive is distributed at the boundary position or between the gaps of the inorganic salt particles to form a thermal conduction path.
[0006] Optionally, the matrix includes at least one of magnesium oxide and silicon dioxide.
[0007] Optionally, the auxiliary agent includes one or a mixture of montmorillonite powder, vermiculite powder, mica powder, red lead, bismuth oxide and diatomaceous earth.
[0008] Optionally: the thermal conductivity enhancing material includes at least one of aluminum nitride, graphite, and silicon carbide.
[0009] Optionally, the inorganic salt includes one or a mixture of several of sodium carbonate, potassium carbonate, lithium carbonate, sodium carbonate, sodium chloride and barium carbonate.
[0010] In addition, the present application also discloses a method for preparing a heat storage material with enhanced thermal conductivity, the method comprising at least the following steps:
[0011] Step 1: Mix the inorganic salt and the thermal conductivity enhancing material in proportion, and keep the mixture at the melting point of the inorganic salt in an inert atmosphere for 1 hour, then cool it naturally, and grind it to obtain a core-shell molten salt;
[0012] Step 2: uniformly mix the matrix and the core-shell molten salt to form a first mixture; then uniformly mix the first mixture with the additive to form a second mixture;
[0013] Step 3, adding water to the second mixed material to mix the ingredients, and then sieving and granulating to form a second sifted clinker;
[0014] Step 4: placing the second screened clinker into a mold for compression molding to obtain a composite molding material;
[0015] Step 5: After slowly drying the composite molding material, a heat storage material green body is obtained, and then the heat storage material green body is fired under high temperature heating conditions to obtain the heat storage material.
[0016] Optionally: in the step three, 15%-30% of water by mass is added to the second mixed material for mixing and kneading for 30-60 minutes; when sieving and granulating, a sieving machine with a sieve size of 40-100 mesh is used for particle size screening.
[0017] Optionally, when the second screened clinker is compression molded in step 4, the compression molding pressure is selected to be 8-30 MPa.
[0018] Optionally: in the step five, the composite molding material is dried at 20°C for 3-8 hours; the sintering temperature of the heat storage material green body is 400°C-850°C.
[0019] Optionally: When the heat storage material green body is fired, the temperature is first raised from room temperature to 100°C within 4 hours and kept at 100°C for 1 hour; then the temperature is raised from 100°C to 400°C within 4 hours and kept at 400°C for 2 hours; next, the temperature is raised from 400°C to 680-820°C within 5 hours and kept at 1 hour, then the heating is stopped and the material is cooled naturally.
[0020] Beneficial Effects
[0021] The technical solution of this application has the following beneficial effects:
[0022] The heat storage material of the present application improves the thermal conductivity of the heat storage material by adjusting its internal components, and designs the internal structure of the heat storage material during the preparation stage, so that the heat storage material can achieve the transfer of heat from the heating source to the internal heat storage components through the heat conduction path in large-scale practical application scenarios, thereby achieving an efficient heat storage and release process. It is more suitable for high-altitude areas with thin air, and improves the thermal utilization efficiency of solid heat storage technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a comparison chart of thermal conductivity between the heat storage material in the embodiment of the present application and ordinary heat storage materials.
[0024] Figure 2 Schematic diagram of the structure of the heat storage material in the embodiment of the present application. DETAILED DESCRIPTION
[0025] The present application is further described below in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and cannot be used to limit the scope of protection of the present application. It should be noted that the following detailed descriptions are all exemplary and are intended to provide further explanation of the present application.
[0026] Specifically, Figure 2 As shown, the embodiment of the present application specifically discloses a heat storage material with enhanced thermal conductivity, which includes a matrix, a core-shell molten salt and an additive, wherein the mass ratio of the matrix, the core-shell molten salt and the additive is 25-65:20-45:5-20; this component ratio can be effectively formed at the sintering temperature, and can be effectively sintered to prepare a complete solid heat storage material with a certain strength; and ensure that the ratio of the heat storage component and the heat conducting component maintains a reasonable balance, so as to achieve a high level of heat storage capacity and thermal conductivity. The core-shell molten salt is randomly and evenly distributed in the matrix; the core-shell molten salt is an inorganic salt wrapped with a thermally conductive enhancing material, and the inner layer of the core-shell molten salt is a plurality of inorganic salt particles, and the additive is distributed at the boundary position or between the gaps of the inorganic salt particles to form a heat conduction path.
[0027] Preferably, the matrix in this embodiment includes at least one of magnesium oxide and silicon dioxide. The matrix is mainly used as a supporting matrix of the heat storage material.
[0028] Preferably, the auxiliary agent in this embodiment includes one or a mixture of montmorillonite powder, vermiculite powder, mica powder, red lead, bismuth oxide and diatomaceous earth. The auxiliary agent mainly adopts the above-mentioned clay minerals that can assist sintering and bonding under high-temperature sintering conditions, which are indispensable in the sintering and molding stage of heat storage materials.
[0029] Preferably, the core-shell molten salt is an inorganic salt wrapped with a thermally conductive enhancing material, wherein the thermally conductive enhancing material includes at least one of aluminum nitride, graphite, and silicon carbide. The inorganic salt includes a mixture of one or more of sodium carbonate, potassium carbonate, lithium carbonate, sodium carbonate, sodium chloride, and barium carbonate. The inorganic salt has the characteristics of high phase change latent heat, high specific heat capacity, and stable high-temperature performance. It is the core component of the composite heat storage material and is used to store heat; while the thermally conductive enhancing material has stable high-temperature properties and can improve the thermal conductivity of the material itself. By coating the outside of the heat storage material, the heat transfer problem of the heat storage material in the actual application process can be improved, so that a large number of heat storage components inside the material structure can store heat energy from the heating source faster while ensuring efficient heat transmission inside the material, reducing internal thermal stress and improving the structural stability of the material.
[0030] Furthermore, the present application also discloses a method for preparing a heat storage material with enhanced thermal conductivity, the method comprising at least the following steps:
[0031] Step 1: Mix the inorganic salt and the thermal conductivity enhancing material in proportion, and keep the mixture at the melting point of the inorganic salt in an inert atmosphere for 1 hour, then cool it naturally, and grind it to obtain a core-shell molten salt.
[0032] Step 2: uniformly mix the matrix and the core-shell molten salt to form a first mixture; then uniformly mix the first mixture and the additive to form a second mixture.
[0033] Step three, adding water to the second mixture for mixing, wherein preferably adding 15%-30% by mass of water to the second mixture for mixing for 30-60 minutes; then sieving and granulating, preferably using a sieving machine with a sieve size of 40-100 mesh for particle size screening, and finally forming a second sieved clinker.
[0034] Step 4: Place the second screened clinker into a mold for compression molding to obtain a composite molding material; wherein the compression molding pressure is preferably 8-30 MPa.
[0035] Step 5: After the composite molding material is slowly dried at 20°C for 3-8 hours, a heat storage material green body is obtained, and then the heat storage material green body is fired under high temperature heating conditions to obtain the heat storage material. The sintering temperature of the heat storage material green body is preferably 400°C-850°C.
[0036] Furthermore, in order to improve the heat storage performance and structural stability of the heat storage material, when the heat storage material green body is fired, the temperature is first raised from room temperature to 100°C within 4 hours and kept at 100°C for 1 hour; then the temperature is raised from 100°C to 400°C within 4 hours and kept at 400°C for 2 hours; next, the temperature is raised from 400°C to 680-820°C within 5 hours, kept for 1 hour, and then the heating is stopped and finally cooled naturally.
[0037] In the embodiments of the present application, in order to solve the problem that the heat storage efficiency of heat storage materials is low under the condition of thin air in high altitude areas, an innovative material structure is introduced, a heat-conducting component with high thermal conductivity coefficient that is stable at high temperature is introduced and coated with inorganic salts to reduce pores and form a good heat conduction path. In addition, due to the poor hydrothermal conditions in high altitude areas and the large demand for heat, the scale of heat storage materials required in the application is relatively large, and the volume of a single sample prepared by the heat storage material is also large. In order to ensure the effective molding and strength of the solid material, a specific proportion of molding components and a sintering system based on the characteristics of the material components are introduced, so that the effective preparation of large-module heat storage materials can be achieved.
[0038] Embodiment 1:
[0039] The method for preparing a heat storage material with enhanced thermal conductivity disclosed in this embodiment 1 comprises the following steps:
[0040] Step 1: 10 g of sodium chloride, 16 g of barium carbonate, 14 g of sodium carbonate and 6 g of aluminum nitride are uniformly mixed in a ball mill, kept at 820° C. for 1 hour in an inert atmosphere, then naturally cooled, and ground with a mortar to form an inorganic salt material wrapped with aluminum nitride.
[0041] Step 2: 69g of heavy magnesium oxide is uniformly mixed with the inorganic salt material wrapped with aluminum nitride in step 1 to form a first mixture. 5g of montmorillonite powder, 8g of mica powder and 3g of lead oxide are added to the first mixture and uniformly mixed in a ball mill to form a second mixture.
[0042] Step 3: Add 12g of water to the second mixed material, stir and knead the ingredients in a kneader for 20min, and after kneading, granulate through a 40-mesh sieve to form a second sieved clinker;
[0043] Step 4: evenly spread the second sieved clinker in the mold, and perform compression molding in the mold to obtain a composite molding material, with a compression pressure of 16 MPa;
[0044] Step 5: slowly drying the composite molding material in a dry environment for 5 hours to obtain the high thermal conductivity composite structure heat storage material green body;
[0045] Step 6: Sinter the heat storage material green body at a high temperature of 820°C to obtain a high thermal conductivity composite structure heat storage material. The specific sintering system curve is: first, raise the temperature from room temperature to 100°C within 4 hours, and keep it at 100°C for 1 hour; then raise the temperature from 100°C to 400°C within 4 hours, and keep it at 400°C for 2 hours; then raise the temperature from 400°C to 820°C within 5 hours, and keep it at 820°C for 1 hour, then stop heating and finally cool naturally.
[0046] Embodiment 2:
[0047] The present embodiment 2 discloses a method for preparing a heat storage material with enhanced thermal conductivity, comprising the following steps:
[0048] Step 1: 10 g of sodium chloride, 16 g of barium carbonate, 14 g of sodium carbonate and 2 g of graphite are uniformly mixed in a ball mill, kept at 820° C. for 1 hour in an inert atmosphere, then naturally cooled, and ground with a mortar to form a graphite-wrapped inorganic salt material;
[0049] Step 2: 69g of heavy magnesium oxide is uniformly mixed with the inorganic salt material wrapped in graphite in step 1 to form a first mixture. 5g of montmorillonite powder, 8g of mica powder and 3g of lead oxide are added to the first mixture and uniformly mixed in a ball mill to form a second mixture.
[0050] Step 3: Add 12 g of water to the second mixed material, stir and knead the ingredients in a kneader for 20 min, and after kneading, granulate through a 40-mesh sieve to form a second sieved clinker;
[0051] Step 4: evenly spread the second sieved clinker in the mold, and perform compression molding in the mold to obtain a composite molding material, with a compression pressure of 16 MPa;
[0052] Step 5: slowly drying the composite molding material in a dry environment for 5 hours to obtain the high thermal conductivity composite structure heat storage material green body;
[0053] Step 6: Sinter the heat storage material green body at a high temperature of 820°C to obtain a high thermal conductivity composite structure heat storage material. The specific sintering system curve is: first, raise the temperature from room temperature to 100°C within 4 hours, and keep it at 100°C for 1 hour; then raise the temperature from 100°C to 400°C within 4 hours, and keep it at 400°C for 2 hours; then raise the temperature from 400°C to 820°C within 5 hours, and keep it at 820°C for 1 hour, then stop heating and finally cool naturally.
[0054] Embodiment 3:
[0055] The present embodiment 3 discloses a method for preparing a heat storage material with enhanced thermal conductivity, comprising the following steps:
[0056] Step 1: 10 g of sodium chloride, 16 g of barium carbonate, 14 g of sodium carbonate and 10 g of silicon dioxide are uniformly mixed in a ball mill, kept at 820° C. for 1 hour in an inert atmosphere, then naturally cooled, and ground with a mortar to form an inorganic salt material coated with silicon dioxide;
[0057] Step 2: 69g of heavy magnesium oxide is uniformly mixed with the inorganic salt material coated with silicon dioxide in step 1 to form a first mixture. 5g of montmorillonite powder, 8g of mica powder and 3g of lead oxide are added to the first mixture and uniformly mixed in a ball mill to form a second mixture.
[0058] Step 3: Add 12 g of water to the second mixed material, stir and knead the ingredients in a kneader for 20 min, and after kneading, granulate through a 40-mesh sieve to form a second sieved clinker;
[0059] Step 4: evenly spread the second sieved clinker in the mold, and perform compression molding in the mold to obtain a composite molding material, with a compression pressure of 16 MPa;
[0060] Step 5: slowly drying the composite molding material in a dry environment for 5 hours to obtain the high thermal conductivity composite structure heat storage material green body;
[0061] Step 6: Sinter the heat storage material green body at a high temperature of 820°C to obtain a high thermal conductivity composite structure heat storage material. The specific sintering system curve is: first, raise the temperature from room temperature to 100°C within 4 hours, and keep it at 100°C for 1 hour; then raise the temperature from 100°C to 400°C within 4 hours, and keep it at 400°C for 2 hours; then raise the temperature from 400°C to 820°C within 5 hours, and keep it at 820°C for 1 hour, then stop heating and finally cool naturally.
[0062] Embodiment 4:
[0063] This embodiment 4 discloses a method for preparing a heat storage material with enhanced thermal conductivity, comprising the following steps:
[0064] Step 1: 20 g of sodium carbonate, 18 g of potassium carbonate and 5 g of aluminum nitride are uniformly mixed in a ball mill, kept at 710° C. for 1 hour in an inert atmosphere, then naturally cooled, and ground with a mortar to form an inorganic salt material wrapped with aluminum nitride;
[0065] Step 2: 57 g of heavy magnesium oxide is uniformly mixed with the inorganic salt material wrapped with aluminum nitride in step 1 to form a first mixture. 2 g of montmorillonite powder, 3 g of mica powder, and 1 g of lead oxide are added to the first mixture and uniformly mixed in a ball mill to form a second mixture.
[0066] Step 3: Add 10 g of water to the second mixed material, stir and knead the ingredients in a kneader for 20 minutes, and after kneading, granulate through a 40-mesh sieve to form a second sieved clinker;
[0067] Step 4: evenly spread the second sieved clinker in the mold, and perform compression molding in the mold to obtain a composite molding material, with a compression pressure of 16 MPa;
[0068] Step 5: slowly drying the composite molding material in a dry environment for 5 hours to obtain the high thermal conductivity composite structure heat storage material green body;
[0069] Step 6: Sinter the heat storage material green body at 700℃ to obtain a high thermal conductivity composite structure heat storage material. The specific sintering system curve is: first, raise the temperature from room temperature to 100℃ within 4h, and keep it at 100℃ for 1h, then raise the temperature from 100℃ to 400℃ within 4h, and keep it at 400℃ for 2h, then raise the temperature from 400℃ to 700℃ within 4.5h, and keep it at 1h, then stop heating, and finally cool naturally.
[0070] Embodiment 5:
[0071] The present embodiment 5 discloses a method for preparing a heat storage material with enhanced thermal conductivity, comprising the following steps:
[0072] Step 1: 20 g of sodium carbonate, 18 g of potassium carbonate and 5 g of silicon dioxide are uniformly mixed in a ball mill, kept at 710° C. for 1 hour in an inert atmosphere, then naturally cooled, and ground with a mortar to form an inorganic salt material coated with silicon dioxide;
[0073] Step 2: 57 g of heavy magnesium oxide is uniformly mixed with the inorganic salt material coated with silicon dioxide in step 1 to form a first mixture. 2 g of montmorillonite powder, 3 g of mica powder and 1 g of lead oxide are added to the first mixture and uniformly mixed in a ball mill to form a second mixture.
[0074] Step 3: Add 10 g of water to the second mixed material, stir and knead the ingredients in a kneader for 20 minutes, and after kneading, granulate through a 40-mesh sieve to form a second sieved clinker;
[0075] Step 4: evenly spread the second sieved clinker in the mold, and perform compression molding in the mold to obtain a composite molding material, with a compression pressure of 16 MPa;
[0076] Step 5: slowly drying the composite molding material in a dry environment for 5 hours to obtain the high thermal conductivity composite structure heat storage material green body;
[0077] Step 6: Sinter the heat storage material green body at 700℃ to obtain a high thermal conductivity composite structure heat storage material. The specific sintering system curve is: first, raise the temperature from room temperature to 100℃ within 4h, and keep it at 100℃ for 1h, then raise the temperature from 100℃ to 400℃ within 4h, and keep it at 400℃ for 2h, then raise the temperature from 400℃ to 700℃ within 4.5h, and keep it at 1h, then stop heating, and finally cool naturally.
[0078] Combination Figure 1 It is found that the thermal storage material prepared by the method of the present application has a significantly better thermal conductivity than ordinary phase change thermal storage materials. It has a high heat storage capacity and a high thermal conductivity, which can realize faster storage and release of heat during the application of the material, thereby effectively improving the thermal efficiency of solid thermal storage materials under high-altitude environmental conditions, which is conducive to the further promotion and application of solid thermal storage materials in the fields of clean energy consumption and heating.
[0079] The above is only a preferred implementation of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.
Claims
1. A heat storage material with enhanced thermal conductivity, characterized in that: It comprises a matrix, a core-shell molten salt and an additive, wherein the mass ratio of the matrix, the core-shell molten salt and the additive is 25-65:20-45:5-20; the core-shell molten salt is randomly and evenly distributed in the matrix; the core-shell molten salt is an inorganic salt wrapped by a thermal conductivity enhancing material, the inner layer of the core-shell molten salt is a plurality of inorganic salt particles, and the additive is distributed at the boundary position or between the gaps of the inorganic salt particles to form a thermal conduction path.
2. The heat storage material according to claim 1, characterized in that: The matrix includes at least one of magnesium oxide and silicon dioxide.
3. The heat storage material according to claim 1, characterized in that: The auxiliary agent comprises one or a mixture of montmorillonite powder, vermiculite powder, mica powder, red lead, bismuth oxide and diatomaceous earth.
4. The heat storage material according to claim 1, characterized in that: The thermal conductivity enhancing material includes at least one of aluminum nitride, graphite, and silicon carbide.
5. The heat storage material according to claim 1, characterized in that: The inorganic salt includes one or a mixture of sodium carbonate, potassium carbonate, lithium carbonate, sodium carbonate, sodium chloride and barium carbonate.
6. A method for preparing a heat storage material with enhanced thermal conductivity, characterized in that: The method comprises at least the following steps: Step 1: Mix the inorganic salt and the thermal conductivity enhancing material in proportion, and keep the mixture at the melting point of the inorganic salt in an inert atmosphere for 1 hour, then cool it naturally, and grind it to obtain a core-shell molten salt; Step 2: uniformly mix the matrix and the core-shell molten salt to form a first mixture; then uniformly mix the first mixture with the additive to form a second mixture; Step 3, adding water to the second mixed material to mix the ingredients, and then sieving and granulating to form a second sifted clinker; Step 4: placing the second screened clinker into a mold for compression molding to obtain a composite molding material; Step 5: After slowly drying the composite molding material, a heat storage material green body is obtained, and then the heat storage material green body is fired under high temperature heating conditions to obtain the heat storage material.
7. The preparation method according to claim 6, characterized in that: In the step 3, 15%-30% of water by mass is added to the second mixed material for mixing and kneading for 30-60 minutes; when sieving and granulating, a sieving machine with a sieve size of 40-100 mesh is used for particle size screening.
8. The preparation method according to claim 6, characterized in that: When the second screened clinker is compression molded in the step 4, the compression molding pressure is selected to be 8-30 MPa.
9. The preparation method according to claim 6, characterized in that: In the step 5, the composite molding material is dried at 20°C for 3-8 hours; the sintering temperature of the heat storage material green body is 400°C-850°C.
10. The preparation method according to claim 9, characterized in that: When the heat storage material green body is fired, the temperature is first raised from room temperature to 100°C within 4 hours and kept at 100°C for 1 hour; then the temperature is raised from 100°C to 400°C within 4 hours and kept at 400°C for 2 hours; next, the temperature is raised from 400°C to 680-820°C within 5 hours and kept at 1 hour, then the heating is stopped and the material is cooled naturally.