Metal oxide insulating layer film and preparation method and application thereof

CN118932289AActive Publication Date: 2024-11-12WUYI UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410900517.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-12
Estimated Expiration
2044-07-05

Smart Images

  • Figure HDA0004930345130000011
    Figure HDA0004930345130000011
  • Figure HDA0004930345130000012
    Figure HDA0004930345130000012
  • Figure HDA0004930345130000021
    Figure HDA0004930345130000021
Patent Text Reader

Abstract

The invention discloses a metal oxide insulating layer thin film and a preparation method and application thereof, and belongs to the technical field of thin film transistors (TFT). The preparation method of the metal oxide insulating layer film comprises the following steps: S1, mixing metal alkoxide and a solvent to obtain a precursor solution, and standing to separate out a crystal to obtain a metal organic compound crystal; s2, grinding the metal organic compound crystal into powder, placing the powder in a crucible, placing a mask plate above the crucible, and enabling the conductive surface of the substrate to face the mask plate side; and S3, performing near-field thermal evaporation operation to obtain the metal oxide insulating layer film. According to the method, the low-leakage-current metal oxide insulating film can be directly prepared in the air atmosphere through a simple process without additional chemical synthesis, a high-temperature annealing process and an inert gas atmosphere, and the method is of great significance to preparation of the high-performance metal oxide insulating film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thin film transistors, and in particular to a metal oxide insulating layer thin film and a preparation method and application thereof. Background Art

[0002] With the development of display devices such as smart phones, tablet computers, TVs, computer monitors and virtual reality devices, people's demand for high-resolution and high-reliability ultra-high-definition display panels continues to increase. Thin-film transistor (TFT) driving backplane technology is the core technology of display panels. In the face of the development needs of ultra-high-definition display panels, TFT driving backplane technology needs to achieve large-scale integration of high-mobility and miniaturized TFT devices. Therefore, with the continuous development of semiconductor devices such as TFT, the number of transistors on a single display panel has increased exponentially, and the power consumption of the product has also gradually increased. Among them, the gate insulation layer material is the main factor affecting the power consumption of TFT. The use of high dielectric constant metal oxide materials (high k) can significantly reduce the power consumption of the device. At the same time, the high-k metal oxide insulating layer is expected to realize low-power oxide TFT devices due to its excellent electrical properties (high unit area capacitance, high dielectric constant, low leakage current, etc.). However, due to the poor compatibility of high-k materials with other devices, the annealing process is incompatible, the thermal stability is poor, the processing process is complex and the efficiency is low. As a result, the application effect of high-k materials is not ideal, the performance of devices is degraded, and it is difficult to achieve large-scale production.

[0003] Therefore, it is necessary to find a method for preparing a metal oxide insulating layer film to solve the problems of high temperature post-annealing, low preparation efficiency and insufficient performance existing in the prior art. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for preparing a metal oxide insulating layer film, which is low-temperature, simple and efficient, does not require an annealing process, and can obtain a metal oxide insulating layer film with high dielectric properties.

[0005] The invention also provides the metal oxide insulating layer film.

[0006] The present invention also provides the above-mentioned thin film transistor.

[0007] A first aspect of the present invention provides a method for preparing a metal oxide insulating layer film, the preparation method comprising the following steps:

[0008] S1, mixing a metal alkoxide and a solvent to obtain a precursor solution, and allowing the solution to stand to precipitate crystals to obtain metal organic compound crystals;

[0009] S2, grinding the metal organic compound crystal into powder and placing it in a crucible, placing a mask plate above the crucible, and facing the conductive surface of the substrate toward the mask plate side;

[0010] S3, performing near-field thermal evaporation operation to obtain the metal oxide insulating layer thin film.

[0011] The method for preparing the metal oxide insulating layer film according to the first aspect of the present invention has at least the following beneficial effects:

[0012] The preparation method described in the present invention precipitates crystals (evaporation source) from a metal oxide precursor solution by means of solution saturation, and achieves low-temperature preparation of a metal oxide insulating layer film by near-field thermal evaporation in an air atmosphere. No additional chemical synthesis, high-temperature annealing process, or inert gas atmosphere is required, thereby greatly improving the preparation efficiency of the dielectric film.

[0013] The preparation method of the present invention has the advantages of safe and reliable whole production process, clear and simple process conditions and easy control, wide material sources, low energy consumption in the production process and is suitable for industrial large-scale production.

[0014] According to some embodiments of the present invention, in step S1, the metal alkoxide includes Zr(NO3)4·5H2O, ZrO(NO3)2, (C5H7O2)4Zr, C 12 H 28 O4Zr, (C5H8O2)4Hf, [(CH3)2N]4Hf, [(CH3)2N]4Hf, Hf(CH2CHCO2(CH2)2CO2)4, C5H5Cl3Hf, Mg(OCH3)2, Mg(OC2H5)2, MgBr2O(C2H5)2, (CH3COO)2Ba, C8H 18 At least two of BaO2 and Ba(OCH(CH3)2)2.

[0015] According to some embodiments of the present invention, in step S1, the metal alkoxide includes (C5H8O2)4Hf and Zr(C5H7O2)4.

[0016] According to some embodiments of the present invention, in step S1, the solvent includes C2H6O, C3H8O2, (CH2OH)2, C3H7NO, CH3(CH2)4OH, C6H 14 O6, CH3(CH2)6OH, CH3(CH2)4OH, (CH3O)2CO, (CH3O)2CO, CH3COOCH2CH3 and C6H 14 At least one or more of.

[0017] According to some embodiments of the present invention, the volume ratio of the precursor solution containing (C5H8O2)4Hf and the precursor solution containing Zr(C5H7O2)4 is (1-3):(1-3), for example, it can be 1:1, 1:2, 1:3, 2:1, 3:1, 3:2, 2:3.

[0018] According to some embodiments of the present invention, in step S1, the concentration of the metal alkoxide in the precursor solution is 0.1-0.6 mol / L.

[0019] Preferably, in step S1, the concentration of the metal alkoxide in the precursor solution is 0.15-0.5 mol / L.

[0020] According to some embodiments of the present invention, in step S1, the mixing time is 2 to 3 hours.

[0021] According to some embodiments of the present invention, in step S1, the mixing temperature is 45-50°C.

[0022] According to some embodiments of the present invention, in step S1, the standing time is 1 to 2 days.

[0023] According to some embodiments of the present invention, in step S1, the ambient temperature during the standing state is 20-25°C.

[0024] According to some embodiments of the present invention, in step S2, the distance between the substrate and the metal organic compound crystal powder is 5 to 10 mm.

[0025] Preferably, in step S2, the distance between the substrate and the metal organic compound crystal powder is 6-8 mm.

[0026] If the distance is too far, the volatilized molecules will be scattered in the air, resulting in the possibility of failure of evaporation. If it is too close, it will not be able to fully react with oxygen in the air atmosphere during the evaporation process, and it is not easy to form oxides. The appropriate distance will achieve the effect of no need for subsequent high-temperature annealing to react with oxygen in the air.

[0027] According to some embodiments of the present invention, in step S3, the heating temperature of the near-field thermal evaporation is 100-250°C.

[0028] Preferably, in step S3, the heating temperature of the near-field thermal evaporation is 150-200°C.

[0029] According to some embodiments of the present invention, in step S3, the near-field thermal evaporation is performed for a time of 1 to 2 minutes.

[0030] According to some embodiments of the present invention, in step S2, the material of the substrate is selected from at least one of ITO glass, FTO glass, TCO glass and metal foil.

[0031] Preferably, in step S2, the substrate can be rigid ITO glass, FTO glass, TCO glass, or flexible ITO, FTO and TCO or metal foil with polyimide (PI), polyethylene naphthalate (PEN), polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polystyrene (PS), polysulfone ether (PES) as the substrate.

[0032] The second aspect of the present invention provides a metal oxide insulating layer film, which is prepared by the above-mentioned preparation method.

[0033] A third aspect of the present invention provides a thin film transistor, comprising the metal oxide insulating layer thin film prepared by the above preparation method.

[0034] According to some embodiments of the present invention, the thin film transistor further includes a substrate, an active layer, and a gate electrode.

[0035] According to some embodiments of the present invention, the active layer is made of an oxide semiconductor by a physical vapor deposition process, a chemical vapor deposition process, an atomic layer deposition process, a laser deposition process or a solution method.

[0036] According to some embodiments of the present invention, the substrate can be a rigid alkali glass, alkali-free glass, quartz glass and silicon substrate, or a flexible polyimide (PI), polyethylene naphthalate (PEN), polyethylene terephthalate (PET), polyethylene (PE), polypropylene (PP), polystyrene (PS), polysulfone ether (PES) or metal foil.

[0037] According to some embodiments of the present invention, the oxide semiconductor may be at least one of indium gallium zinc oxide (IGZO), indium tin zinc oxide (ITZO), indium zinc oxide (IZO), and indium oxide (In2O3).

[0038] According to some embodiments of the present invention, the gate electrode may be a transparent conductive oxide, graphene, a metal-oxide semiconductor stack or a metal-metal stack. Transparent conductive oxides include ITO, AZO, GZO, IZO, ITZO, and FTO; metal-oxide semiconductor stacks include ITO / Ag / ITO and IZO / Ag / IZO; and metal-metal stacks include Mo / Al / Mo and Ti / Al / Ti.

[0039] According to some embodiments of the present invention, the gate electrode may be prepared by sputtering, electroplating, thermal evaporation or other deposition methods, preferably sputtering deposition, because the film prepared by this method has good adhesion to the substrate, excellent uniformity, and can be prepared on a large area.

[0040] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0042] Figure 1 This is an XRF characterization diagram of the metal organic compound crystal powder obtained in Example 1 of the present invention;

[0043] Figure 2 This is a real shot of the metal organic compound crystal obtained in Example 1 of the present invention;

[0044] Figure 3 This is a schematic diagram of the near-field thermal evaporation structure in Example 1 of the present invention;

[0045] Figure 4 This is an XRF characterization diagram of the metal organic compound crystal powder obtained in Example 4 of the present invention;

[0046] Figure 5 This is an XRF characterization diagram of the metal organic compound crystal powder obtained in Example 5 of the present invention;

[0047] Figure 6 This is the XRD data result diagram in Test Example 1 of the present invention;

[0048] Figure 7 This is a graph showing the TG-DSC characterization results in Test Example 1 of the present invention;

[0049] Figure 8 This is the EDS element distribution diagram in Test Example 2 of the present invention;

[0050] Fig. 9 This is a result diagram of the dielectric properties of the pure Hf thin film device obtained in Example 4 of Test Example 3 of the present invention;

[0051] Fig.10 This is a result diagram of the dielectric properties of the pure Zr thin film device obtained in Example 5 of Test Example 3 of the present invention;

[0052] Fig.11 This is a graph showing the dielectric properties of a pure Hf:Zr=75%:25% thin film device obtained in Example 1 in Test Example 3 of the present invention.

[0053] Reference numerals:

[0054] 01. Rotating table; 02. Substrate; 03. Mask plate; 04. Metal oxide crystal powder; 05. Crucible; 06. Heating table. DETAILED DESCRIPTION

[0055] The embodiments of the present invention are described in detail below, and the same or similar reference numerals throughout the embodiments represent the same or similar elements or elements with the same or similar functions. The embodiments described below are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0056] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0057] The words "preferably", "more preferably", etc. in the present invention refer to embodiments of the present invention that may provide certain beneficial effects in certain circumstances. However, other embodiments may also be preferred under the same circumstances or other circumstances. In addition, the description of one or more preferred embodiments does not imply that other embodiments are not applicable, nor is it intended to exclude other embodiments from the scope of the present invention.

[0058] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0059] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.

[0060] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0061] Example 1

[0062] This embodiment provides a metal oxide insulating layer film, and the specific preparation method thereof includes:

[0063] 1) Preparation of precursor solution: Dissolve 0.18 g (C5H8O2)4Hf (Hafnium acetylacetonate) (McLean, 17475-67-1) in 2 ml of organic solvent, stir at 45°C for 2 h, and obtain a precursor solution A with a concentration of 0.16 mol / L;

[0064] Dissolve 0.16 g Zr(C5H7O2)4 (zirconium acetylacetonate) (McLean, 17501-44-9) in 2 ml organic solvent and stir at 45 °C for 2 h to obtain a precursor solution B with a concentration of 0.16 mol / L;

[0065] 2) Precursor solutions A and B were mixed in a volume ratio of 3:1 to obtain a blended hafnium zirconium oxide precursor solution. The prepared blended hafnium zirconium oxide precursor solution was allowed to stand for 1 day to allow crystals to precipitate, and the crystals were ground into powder for XRF peak characterization (X-ray tube voltage and current were set to 50 kV and 220 A, respectively, for a measurement time of 15 minutes in a vacuum environment). The results are as follows: Figure 1 As shown, the elements can be further obtained. The elements are concentrated during the crystallization process. The actual picture of the obtained metal organic compound crystal is as follows Figure 2 As shown;

[0066] 3) The metal organic compound crystal powder prepared above is placed in a crucible, the crucible is placed on a hot plate and heated in the range of 200°C, a hollow gasket is placed above the crucible, the conductive surface of the substrate is facing the side of the hollow gasket, the distance between the metal organic compound powder and the substrate is 8mm, and the near-field thermal evaporation operation is performed for 1 minute, and a metal oxide insulating layer film is obtained without post-annealing. The structural schematic diagram of the near-field thermal evaporation is shown as follows Figure 3 shown.

[0067] Example 2

[0068] This embodiment provides a metal oxide insulating layer film, and the specific preparation method thereof includes:

[0069] 1) Preparation of precursor solution: Dissolve 0.18 g (C5H8O2)4Hf (Hafnium acetylacetonate) (McLean, 17475-67-1) in 2 ml of organic solvent, stir at 45°C for 2 h, and obtain a precursor solution A with a concentration of 0.16 mol / L;

[0070] Dissolve 0.16 g Zr(C5H7O2)4 (zirconium acetylacetonate) (McLean, 17501-44-9) in 2 ml organic solvent and stir at 45 °C for 2 h to obtain a precursor solution B with a concentration of 0.16 mol / L;

[0071] 2) Precursor solutions A and B are mixed in a volume ratio of 1:1 to obtain a blended hafnium zirconium oxide precursor solution, the prepared blended hafnium zirconium oxide precursor solution is allowed to stand for 1 day to allow crystals to precipitate, and the crystals are ground into powder;

[0072] 3) The metal organic compound crystal powder prepared above is placed in a crucible, the crucible is placed on a hot table and heated in the range of 200°C, a hollow gasket is placed on the crucible, the conductive surface of the substrate is facing the side of the hollow gasket, the distance between the metal organic compound powder and the substrate is 8 mm, and a near-field thermal evaporation operation is performed for 1 minute, and a metal oxide insulating layer film is obtained without post-annealing.

[0073] Example 3

[0074] This embodiment provides a metal oxide insulating layer film, and the specific preparation method thereof includes:

[0075] 1) Preparation of precursor solution: Dissolve 0.18 g (C5H8O2)4Hf (Hafnium acetylacetonate) (McLean, 17475-67-1) in 2 ml of organic solvent, stir at 45°C for 2 h, and obtain a precursor solution A with a concentration of 0.16 mol / L;

[0076] Dissolve 0.16 g Zr(C5H7O2)4 (zirconium acetylacetonate) (McLean, 17501-44-9) in 2 ml organic solvent and stir at 45 °C for 2 h to obtain a precursor solution B with a concentration of 0.16 mol / L;

[0077] 2) Precursor solutions A and B are mixed in a volume ratio of 1:3 to obtain a blended hafnium zirconium oxide precursor solution, the prepared blended hafnium zirconium oxide precursor solution is allowed to stand for 1 day to allow crystals to precipitate, and the crystals are ground into powder;

[0078] 3) The metal organic compound crystal powder prepared above is placed in a crucible, the crucible is placed on a hot table and heated in the range of 200°C, a hollow gasket is placed on the crucible, the conductive surface of the substrate is facing the side of the hollow gasket, the distance between the metal organic compound powder and the substrate is 8 mm, and a near-field thermal evaporation operation is performed for 1 minute, and a metal oxide insulating layer film is obtained without post-annealing.

[0079] Example 4

[0080] This embodiment provides a method for preparing a metal oxide insulating layer thin film, which is different from Embodiment 1 in that:

[0081] Preparation of precursor solution: Dissolve 0.18g (C5H8O2)4Hf (Hafnium acetylacetonate) (McLean, 17475-67-1) in 2ml organic solvent, stir at 45℃ for 2h to obtain a precursor solution containing hafnium element with a concentration of 0.16mol / L, let it stand for one day to allow crystals to precipitate, and characterize the peak position of XRF (X-ray tube voltage and current are set to 50kV and 220A respectively, measurement time is 15 minutes, in vacuum environment). The results are as follows: Figure 4 shown.

[0082] Example 5

[0083] This embodiment provides a method for preparing a metal oxide insulating layer thin film, which is different from Embodiment 1 in that:

[0084] Preparation of precursor solution: Dissolve 0.16g Zr(C5H7O2)4 (zirconium acetylacetonate) (McLean, 17501-44-9) in 2ml organic solvent, stir at 45℃ for 2h to obtain a precursor solution containing zirconium element with a concentration of 0.16mol / L, let it stand for one day to allow crystals to precipitate, and characterize the peak position of XRF (X-ray tube voltage and current are set to 50kV and 220A respectively, measurement time is 15 minutes, in vacuum environment). The results are as follows: Figure 5 shown.

[0085] Test Example 1

[0086] The metal oxide insulating layer films prepared in Examples 1 to 3 were characterized by XRD (X-ray diffraction angle was 2°, measured in thin film mode), and the results were as follows: Figure 6 As shown, by comparing the diffraction peaks of pure zirconium oxide and hafnium oxide, as well as the pdf standard card, relevant diffraction peaks appear under the three different Hf and Zr ratios of Examples 1 to 3, indicating that the oxide insulating films prepared in Example 1 contain relevant material elements.

[0087] The metal oxide insulating layer film obtained in Example 1 was subjected to TG-DSC analysis. At 172°C, the residual mass began to decrease significantly, indicating that the metal organic compound crystal powder began to thermally decompose at this temperature, probably because the organic ligand began to volatilize or decompose. At 192°C, an obvious endothermic peak appeared, indicating that the sample underwent a significant endothermic reaction at this temperature. The near-field thermal evaporation operation at 200°C further proved that this temperature range was suitable for the thermal decomposition and evaporation of the crystal powder to form a uniform metal oxide insulating layer film. The results are shown in FIG. Figure 7 shown.

[0088] Test Example 2

[0089] The metal oxide insulating layer film obtained in Example 1 was subjected to EDS element analysis. The hafnium element was represented by yellow and the zirconium element was represented by green. The yellow and green colors were evenly dispersed in the region. Therefore, it can be judged from the analysis results that in the random region of the oxide insulating layer, the hafnium and zirconium elements are evenly distributed in the random region, and the content of the elements can be judged based on the depth of the color, indicating that the hafnium element is significantly more than the zirconium element. The results are in line with expectations. The hafnium and zirconium elements in the obtained metal oxide insulating layer film are evenly distributed. The results are as follows Figure 8 shown.

[0090] Test Example 3

[0091] The metal electrode / metal oxide insulating layer film / metal electrode (MIM) device prepared from the metal oxide insulating layer film obtained in Example 1, Example 4 and Example 5 was subjected to a dielectric property test, mainly using IV testing means, under the same conditions (metal electrode area, material, etc.), the size of the current that can pass through the oxide film dielectric film is characterized according to the size of the applied voltage, and the dielectric property is reflected according to the current size, and the smaller the current, the better the dielectric property.

[0092] As the voltage increases to 20V, the metal oxide insulating layer film in Example 1 has good anti-breakdown characteristics under a bias voltage of less than 20V. Fig. 9 , Fig.10 and Fig.11 shown.

[0093] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A method for preparing a metal oxide insulating layer film, characterized in that: The preparation method comprises the following steps: S1, mixing a metal alkoxide and a solvent to obtain a precursor solution, and allowing the solution to stand to precipitate crystals to obtain metal organic compound crystals; S2, grinding the metal organic compound crystal into powder and placing it in a crucible, placing a mask plate above the crucible, and facing the conductive surface of the substrate toward the mask plate side; S3, performing near-field thermal evaporation operation to obtain the metal oxide insulating layer thin film.

2. The preparation method according to claim 1, characterized in that: In step S1, the metal alkoxide includes Zr(NO3)4·5H2O, ZrO(NO3)2, (C5H7O2)4Zr, C 12 H 28 O4Zr, (C5H8O2)4Hf, [(CH3)2N]4Hf, [(CH3)2N]4Hf, Hf(CH2CHCO2(CH2)2CO2)4, C5H5Cl3Hf, Mg(OCH3) 2、 Mg(OC2H5) 2、 MgBr2O(C2H5) 2、 (CH3COO)2Ba、C8H 18 At least two of BaO2 and Ba(OCH(CH3)2)2; preferably, when the precursor solution is a mixture of two metal alkoxides, the volume ratio of the two precursor solutions is (1-3): (1-3).

3. The preparation method according to claim 1, characterized in that: In step S1, the solvent includes C2H6O, C3H8O2, (CH2OH)2, C3H7NO, CH3(CH2)4OH, C6H 14 O6, CH3(CH2)6OH, CH3(CH2)4OH, (CH3O)2CO, (CH3O)2CO, CH3COOCH2CH3 and C6H 14 At least one of .

4. The preparation method according to claim 1, characterized in that: In step S1, the concentration of the metal alkoxide in the precursor solution is 0.1-0.6 mol / L.

5. The preparation method according to claim 1, characterized in that: In step S1, the mixing time is 2 to 3 hours; preferably, in step S1, the mixing temperature is 45 to 50°C; preferably, in step S1, the standing time is 1 to 2 days; preferably, in step S1, the ambient temperature during the standing time is 20 to 25°C.

6. The preparation method according to claim 1, characterized in that: In step S2, the distance between the substrate and the metal organic compound crystal powder is 5 to 10 mm.

7. The preparation method according to claim 1, characterized in that: In step S3, the heating temperature of the near-field thermal evaporation is 100-250°C; preferably, in step S3, the time of the near-field thermal evaporation is 1-2 minutes.

8. The preparation method according to claim 1, characterized in that: In step S2, the material of the substrate is selected from at least one of ITO glass, FTO glass, TCO glass and metal foil.

9. A metal oxide insulating layer film, characterized in that: The metal oxide insulating layer thin film is prepared by the preparation method according to any one of claims 1 to 8.

10. A thin film transistor, characterized in that: The invention comprises a metal oxide insulating layer film prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Process for producing spherical submicron metal with hydro-thermal treatment

    CN101428348A

  • Solubilized metal alkoxides in alkoxyalkanol solvent

    EP0369533A2

  • Oxide semiconductor layer method using sol-gel method including oxygen plasma processing process and oxide semiconductor layer manufactured by same

    KR101460489B1

  • Composition for dielectric thin film, metal oxide dielectric thin film using the same and preparation method thereof

    KR1020080030454A

  • Yttrium-doped Indium Oxide Transparent Conductive Thin-Film Transistor and Method for Making Same

    US20140021464A1