A catalyst for the one-step preparation of 2-methylnaphthalene or 2,6-dimethylnaphthalene from carbon dioxide hydrogenation and naphthalene, and a preparation method and application thereof

By using a catalyst composed of polymetallic oxides and modified zeolite molecular sieves, 2-methylnaphthalene or 2,6-dimethylnaphthalene is prepared in one step by carbon dioxide hydrogenation and naphthalene. This solves the problem of easy catalyst deactivation, improves the conversion rate of naphthalene and the selectivity of the target product, and realizes an economical and efficient process route.

CN118950074BActive Publication Date: 2026-11-24NORTHWEST UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411034066.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2026-11-24
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

In existing technologies, the catalyst in the naphthalene methylation process is prone to deactivation, the single-pass conversion rate of naphthalene is low, and methanol fails to effectively participate in the methylation reaction, resulting in the generation of a large amount of low-carbon olefins by methanol side reaction, causing catalyst carbon deposition and deactivation.

Method used

A catalyst composed of polymetallic oxides and modified zeolite molecular sieves is used to prepare 2-methylnaphthalene or 2,6-dimethylnaphthalene in a one-step process via carbon dioxide hydrogenation and naphthalene. The polymetallic oxides increase the strong acid density of the catalyst and the acid site distribution of the modified zeolite molecular sieves, thereby inhibiting deep alkylation reactions and improving the selectivity of the target product.

Benefits of technology

It improves the conversion rate of naphthalene and the selectivity of the target product, prolongs the stability of the catalyst, reduces the cost of raw materials, has a simple and efficient process route, reduces the emission of waste, sludge, and solid waste, is easy to separate and purify, has low catalyst preparation cost, and is suitable for industrial application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004970610020000141
    Figure BDA0004970610020000141
  • Figure BDA0004970610020000151
    Figure BDA0004970610020000151
  • Figure BDA0004970610020000152
    Figure BDA0004970610020000152
Patent Text Reader

Abstract

This invention discloses a catalyst, its preparation method, and its application for the one-step synthesis of 2-methylnaphthalene or 2,6-dimethylnaphthalene via carbon dioxide hydrogenation and naphthalene. The catalyst comprises a polymetallic oxide and a modified zeolite molecular sieve; wherein the metal oxide is an oxide composed of two or three metals selected from Zn, Al, In, Zr, and Ga; the mass percentage of the polymetallic oxide in the catalyst is 20%–60%. This catalyst can be used for the one-step synthesis of 2-methylnaphthalene or 2,6-dimethylnaphthalene via carbon dioxide hydrogenation and naphthalene. In this invention, carbon dioxide hydrogenation acts as an alkylating agent, effectively reducing the concentration of methylation intermediates, suppressing intermediate side reactions, and achieving in-situ generation and consumption of methylation intermediates. Simultaneously, the carbon dioxide atmosphere significantly inhibits coking, greatly extending the catalyst's stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of reaction technology for the alkylation of polycyclic aromatic hydrocarbons into high-value-added chemicals, specifically to a catalyst, preparation method, and application for the one-step synthesis of 2-methylnaphthalene or 2,6-dimethylnaphthalene from carbon dioxide hydrogenation and naphthalene. Background Technology

[0002] With the development of coal chemical and petrochemical industries, developing the synthesis of 2-methylnaphthalene and 2,6-dimethylnaphthalene using naphthalene as a raw material can not only increase the added value of naphthalene, but also reduce the production cost of 2,6-dimethylnaphthalene, laying the foundation for industrial application.

[0003] 2-Methylnaphthalene and 2,6-dimethylnaphthalene are important raw materials for synthesizing high-performance polymers. 2-Methylnaphthalene is used in medicine as an intermediate in the production of vitamin K3, and its oxidation produces β-naphthol, used in long-acting or short-acting oral contraceptives. In agriculture, it is used to synthesize plant growth regulators and DDT emulsifiers; after sulfonation, it can be used as a detergent, and also as a raw material for fiber dyeing auxiliaries, wetting agents, surfactants, and pesticides. 2,6-Dimethylnaphthalene (2,6-DMN) is an important raw material for synthesizing high-performance polymers. Its oxidation produces 2,6-naphthalenedicarboxylic acid (2,6-NDCA), which, when condensed with ethylene glycol, yields ethylene glycol 2,6-naphthalenedicarboxylic acid (PEN), a novel polyester material. Compared to traditional polyethylene terephthalate (PET), PEN offers superior gas barrier properties, heat resistance, chemical stability, and radiation resistance. It has wide applications in the manufacturing of fibers, electronic components, building components, instruments, insulating materials, film, magnetic tape, food packaging films, beer bottles, and aerospace and nuclear energy materials, demonstrating immense development potential and making it one of the fastest-growing polymer materials in the past decade. The traditional methanol-naphthalene methylation process involves directly alkylating methanol and naphthalene on a molecular sieve catalyst. While this technology is relatively mature, it suffers from the following problems: methanol itself reacts more readily (e.g., methanol to olefins) than in methanol-naphthalene methylation, resulting in a large amount of methanol failing to participate in the methylation reaction, leading to a low single-pass conversion rate of naphthalene. Furthermore, methanol readily generates large amounts of low-carbon olefins and other carbon-depositing precursors under the action of the catalyst, causing catalyst deactivation due to carbon buildup. Summary of the Invention

[0004] To overcome the problem of catalyst deactivation in the methanol-naphthalene methylation process in the prior art, the purpose of this invention is to provide a catalyst, preparation method and application for the one-step preparation of 2-methylnaphthalene or 2,6-dimethylnaphthalene by carbon dioxide hydrogenation and naphthalene. The catalyst prepared by this method has good catalytic activity.

[0005] To achieve the above objectives, the present invention adopts the following technical solution:

[0006] A catalyst for the one-step synthesis of 2-methylnaphthalene / 2,6-dimethylnaphthalene from carbon dioxide and hydrogen and naphthalene comprises a polymetallic oxide and a modified zeolite molecular sieve.

[0007] Among them, metal oxides are oxides composed of two or three metals selected from Zn, Al, In, Zr and Ga;

[0008] The mass percentage of polymetallic oxides in the catalyst is 20% to 60%.

[0009] Furthermore, the metal oxide is ZnZrO. x ,InZrO x ZnAlO x GaZrO x and ZnGaO x One of them.

[0010] Furthermore, the modified zeolite molecular sieve is prepared by the following process: HZSM-5 molecular sieve is immersed in a solution of zinc nitrate, gallium nitrate, cerium nitrate or lanthanum nitrate, allowed to stand, dried, and calcined to obtain the modified molecular sieve.

[0011] Furthermore, the calcination temperature is 400-600℃ and the time is 3-5h; the loading of zinc, gallium, cerium or lanthanum elements in the modified molecular sieve is 1%-3% of the molecular sieve mass.

[0012] Furthermore, the modified zeolite molecular sieve is prepared by the following process: crystallizing one of the following metal salts: nitrate metal salt and acetylacetone metal salt, tetrapropylammonium bromide, silica sol, ethylamine and water at 140-170℃ for 3-4 days, and then calcining at 400-600℃ for 6 hours to obtain the modified molecular sieve.

[0013] Furthermore, the metal is Ga, Zn, Fe, or Ge.

[0014] Furthermore, the molar ratio of tetrapropylammonium bromide, silica sol, ethylamine, water, and metal nitrate salt is 0.15:1:1:17:(0.001-0.01);

[0015] The molar ratio of tetrapropylammonium bromide, silica sol, ethylamine, water and acetylacetone metal salt is 0.15:1:1:17:(0.001-0.01).

[0016] A method for preparing a catalyst for the one-step synthesis of 2-methylnaphthalene / 2,6-dimethylnaphthalene from carbon dioxide and hydrogen with naphthalene, characterized by comprising the following steps:

[0017] Metal oxides were mixed with modified molecular sieves and pressed into tablets of 20–40 mesh to obtain a catalyst for the one-step synthesis of 2-methylnaphthalene / 2,6-dimethylnaphthalene from carbon dioxide hydrogenation and naphthalene.

[0018] Application of a catalyst in the one-step production of 2-methylnaphthalene or 2,6-dimethylnaphthalene by hydrogenation of carbon dioxide and naphthalene.

[0019] Furthermore, the catalyst is added to a fixed-bed reactor, and then carbon dioxide, hydrogen and naphthalene are introduced. The reaction is carried out at a temperature of 300 to 550°C and a pressure of 1 to 5 MPa to produce 2-methylnaphthalene or 2,6-dimethylnaphthalene.

[0020] The volume ratio of carbon dioxide to hydrogen is (0.1–8):1, and the volume hourly space velocity (VHSV) of carbon dioxide and hydrogen is 1000–50000 h⁻¹. -1 The mass hourly space velocity (HSV) of naphthalene is 0.1–5 h⁻¹. -1 .

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The catalyst in this invention comprises polymetallic oxides and modified zeolite molecular sieves, which can increase the strong acid density of the catalyst and weaken the strong acid strength, thus exerting a stronger pulling effect on the naphthalene alkylation process and enhancing the conversion of naphthalene. Simultaneously, it inhibits the deep alkylation reaction of the product, effectively improving the selectivity of methylnaphthalene. Furthermore, the modified molecular sieves possess a more rational acid site distribution, which is beneficial for improving the selectivity of 2-methylnaphthalene / 2,6-dimethylnaphthalene.

[0023] This invention uses carbon dioxide and hydrogen instead of methanol as methylating agents to efficiently convert naphthalene onto a catalyst prepared in this invention. The main route involves converting carbon dioxide and hydrogen into active intermediates such as methanol on a metal catalyst, followed by methylation with naphthalene at acidic sites on a zeolite molecular sieve. Therefore, the production of high-value-added chemicals using the methylation reaction of carbon dioxide and hydrogen with naphthalene has advantages such as a short process route, high naphthalene conversion rate, high catalyst stability, and high selectivity for the target product, making it more economical and efficient. In this invention, carbon dioxide is used as an alkylating agent, which can significantly reduce the concentration of the alkylating agent, generate methanol intermediates in situ on the metal oxide, consume the intermediates in situ, suppress methanol side reactions, and greatly extend the catalyst lifetime. Specific advantages are as follows:

[0024] 1) The raw material carbon dioxide is low in cost, widely available, and its conversion and utilization as a greenhouse gas is simple, efficient, and economically advantageous:

[0025] 2) The technology is advanced, with no waste discharge and zero pollution in the process.

[0026] 3) Simple separation and purification with high product selectivity: It uses carbon dioxide as raw material and produces fewer byproducts such as polymethyl aromatic hydrocarbons. The reactant composition is simple and conducive to separation and purification.

[0027] 4) The catalyst is prepared using non-precious metals, which has low preparation cost and is conducive to industrialization. Detailed Implementation

[0028] The present invention will be further described in detail below with reference to the embodiments, but the scope of protection of the present invention is not limited to these embodiments.

[0029] In this invention, carbon dioxide hydrogenation is used as an alkylating agent, effectively reducing the concentration of methylation intermediates, suppressing intermediate side reactions, and achieving in-situ generation and consumption of methylation intermediates. Simultaneously, the carbon dioxide atmosphere significantly inhibits coking, greatly extending catalyst stability. Therefore, using carbon dioxide hydrogenation and naphthalene methylation to produce high-value-added chemicals has advantages such as a shorter process route, higher naphthalene conversion rate, higher catalyst stability, and higher selectivity for the target product, making it more economical and efficient.

[0030] The catalyst of the present invention for the one-step production of 2-methylnaphthalene / 2,6-dimethylnaphthalene from carbon dioxide and hydrogen and naphthalene is a "metal-zeolite" bifunctional catalyst composed of a mixture of polymetallic oxides and modified zeolite molecular sieves.

[0031] The metal oxide component can be an oxide composed of two or three metals such as Zn, Al, In, Zr and Ga.

[0032] In the catalyst, the mass percentage of polymetallic oxides is 20% to 60%, and the remainder is modified zeolite molecular sieve.

[0033] Polymetallic oxides are prepared by ball milling or co-precipitation.

[0034] Modification methods for zeolite molecular sieves include metal / non-metal element modification, NH4F modification, and alkali treatment modification.

[0035] The present invention provides a method for preparing a catalyst for the one-step synthesis of 2-methylnaphthalene / 2,6-dimethylnaphthalene from carbon dioxide and hydrogen with naphthalene, comprising the following steps:

[0036] Preparation of metal oxides by co-precipitation or mechanical ball milling:

[0037] 1) Preparation of ZnZrO by coprecipitation method x metal oxides

[0038] Step 1: Dissolve 0.01-0.1 mol of zinc nitrate and 0.01-0.1 mol of zirconium nitrate in 100-140 mL of deionized water;

[0039] Step 2: Add 3-6g of ammonium carbonate to the solution from Step 1 above;

[0040] Step 3: With continuous stirring, raise the temperature to 50-80℃ and maintain it for 2-4 hours;

[0041] Step 4: Cool down, let stand for aging for 4 hours, then centrifuge and wash several times, dry at 110℃ overnight, and finally calcine at 400-600℃ for 3-5 hours to obtain ZnZrO. x Metal oxides.

[0042] GaZrO was prepared simultaneously using the above method. x ,InZrO x ZnAlO x ZnGaO x Metal oxides, etc.

[0043] InZrO is prepared by replacing zinc nitrate with indium nitrate in the above steps. x ZnAlO was prepared by replacing zirconium nitrate with aluminum nitrate. x ZnGaO was prepared by replacing zirconium nitrate with gallium nitrate. x GaZrO was prepared by replacing zinc nitrate with gallium nitrate. x .

[0044] 2) Preparation of ZnZrO by mechanical ball milling x metal oxides

[0045] Step 1: Place 0.01-0.1 mol of zinc nitrate, 0.01-0.1 mol of zirconium nitrate, and 0.05-0.5 mol of urea into a ball mill jar;

[0046] Step 2: Mechanical ball milling for 0.5-3 hours;

[0047] Step 3: Calcination at 400-600℃ for 3-5 hours to obtain ZnZrO. x Metal oxides.

[0048] GaZrO was prepared simultaneously using the above method. x ,InZrO x ZnAlO x ZnGaO x Metal oxides, etc.

[0049] InZrO was prepared by replacing zinc nitrate with indium nitrate in the above steps. x ZnAlO was prepared by replacing zirconium nitrate with aluminum nitrate. x ZnGaO was prepared by replacing zirconium nitrate with gallium nitrate. x GaZrO was prepared by replacing zinc nitrate with gallium nitrate. x .

[0050] 3) Preparation of modified zeolite molecular sieves:

[0051] Method a): 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a silica content of 30% by mass, 1 mol ethylamine, 17 mol water and 0.0001-0.001 mol aluminum nitrate were stirred and placed in a hydrothermal reactor. The mixture was then crystallized in a rotary oven at 140-170℃ for 3-4 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 400-600℃ for 6 hours to obtain HZSM-5 molecular sieve.

[0052] HZSM-5 molecular sieve is immersed in a solution of zinc nitrate, gallium nitrate, cerium nitrate, or lanthanum nitrate with a concentration of 0.0001-0.001 mol / L, allowed to stand for 1-2 hours, dried, and then calcined at 400-600℃ for 3-5 hours to obtain a modified molecular sieve; wherein the loading of zinc, gallium, cerium, or lanthanum is 1%-3% of the molecular sieve mass.

[0053] Method b): 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a silica content of 30%, 1 mol ethylamine, 17 mol water, and 0.001-0.01 mol nitrate metal salt (or acetylacetone metal salt, metals being Ga, Zn, Fe, or Ge) were stirred and placed in a hydrothermal reactor. The mixture was then crystallized in a rotary oven at 140-170℃ for 3-4 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 400-600℃ for 6 hours to obtain the modified molecular sieve, named in-situ synthesized Ga, Zn, Fe, Ge modified Silicalile-1 molecular sieve.

[0054] The catalyst prepared by the above method is used in a fixed-bed reactor for the one-step production of 2-methylnaphthalene / 2,6-dimethylnaphthalene by carbon dioxide hydrogenation and naphthalene. The application method is as follows: the catalyst is added to the fixed-bed reactor, and then carbon dioxide and hydrogen are introduced with naphthalene. The reaction is carried out at a temperature of 300-550℃ and a pressure of 1-5MPa to produce 2-methylnaphthalene or 2,6-dimethylnaphthalene.

[0055] The volume ratio of carbon dioxide to hydrogen is (0.1–8):1, and the volume hourly space velocity (VHSV) of carbon dioxide and hydrogen is 1000–50000 h⁻¹. -1 The mass hourly space velocity (HSV) of naphthalene is 0.1–5 h⁻¹. -1 The catalyst needs to be reduced for 0.5-1 h before use. The catalyst is used to catalyze the reaction of carbon dioxide hydrogenation with naphthalene to produce 2-methylnaphthalene / 2,6-dimethylnaphthalene in a fixed-bed reactor.

[0056] Catalyst preparation:

[0057] Select metal oxides (such as ZnZrO) x ,InZrO x ZnAlO x GaZrOx and ZnGaO x One of the following is mixed with a modified molecular sieve and pressed into tablets of 20-40 mesh to obtain a catalyst for the one-step production of 2-methylnaphthalene / 2,6-dimethylnaphthalene by carbon dioxide hydrogenation and naphthalene, namely a "metal-zeolite" bifunctional catalyst.

[0058] Catalyst evaluation:

[0059] A 1g "metal-molecular sieve" bifunctional catalyst was loaded for catalytic performance testing. The catalyst required reduction for 0.5-1h at a reaction temperature of 380℃ and a pressure of 3MPa. The feed gas consisted of CO2 and H2 (volume ratio H2 / CO2 = 3), with a space velocity (GHSV) of 2400mL / (g). cat Naphthalene is dissolved in trimethylbenzene and pumped into a fixed bed under pressure by a horizontal flow pump. The liquid hourly space velocity (LHSV) of naphthalene is 0.2 h⁻¹. -1 .

[0060] The following are specific examples.

[0061] Comparative Example 1 ZnZrO x HZSM-5 is specifically produced through the following process:

[0062] ZnZrO x The metal oxide was prepared by a co-precipitation method: 0.002 mol of zinc nitrate and 0.017 mol of zirconium nitrate were dissolved in 100 mL of deionized water; 3.1 g of ammonium carbonate was added to the above solution; the temperature was raised to 70 °C and maintained for 2 h under continuous stirring; the temperature was lowered, and the mixture was allowed to stand for 4 h for aging; then it was centrifuged and washed several times, dried at 110 °C overnight, and finally calcined at 500 °C for 3 h to obtain ZnZrO. x Metal oxides.

[0063] HZSM-5 molecular sieve is prepared by a hydrothermal method: 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a silica content of 30% by mass, 1 mol ethylamine, 17 mol water and 0.0001-0.001 mol aluminum nitrate are stirred and then placed in a hydrothermal reactor. The mixture is then crystallized in a rotary oven at 170℃ for 3 days. After crystallization, the mixture is washed 3-5 times, dried for 5 hours, and then calcined at 550℃ for 6 hours to obtain HZSM-5 molecular sieve.

[0064] Weigh out 0.6g of the above-mentioned ZnZrO x Metal oxides and 0.6 g of HZSM-5 molecular sieve were ground in an agate mortar for 30 minutes to obtain a uniformly mixed powder. This mixed powder was then placed in a tablet press and sieved through a tablet press to obtain 20-40 mesh ZnZrO. x &HZSM-5 granules.

[0065] Comparative Example 2InZrO x Preparation of HZSM-5

[0066] InZrO was prepared using the method described in Comparative Example 1. x Metal oxides; the amount of indium nitrate is 0.004 mol and the amount of zirconium nitrate is 0.036 mol.

[0067] HZSM-5 molecular sieve, same as comparative example 1.

[0068] Weigh out 0.6g of the above-mentioned InZrO x The metal oxide was ground with 0.6 g of HZSM-5 molecular sieve in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved through a tableting sieve to obtain 20-40 mesh InZrO. x &HZSM-5 granules.

[0069] Comparative Example 3ZnAlO x Preparation of HZSM-5

[0070] ZnAlO was prepared using the method described in Comparative Example 1. x Metal oxides; the amount of zinc nitrate is 0.004 mol and the amount of aluminum nitrate is 0.036 mol.

[0071] HZSM-5 same comparison ratio 1.

[0072] Weigh out 0.6g of the above-mentioned ZnAlO x The metal oxide was ground with 0.6 g of HZSM-5 molecular sieve in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved through a tableting sieve to obtain 20-40 mesh ZnAlO. x &HZSM-5 granules.

[0073] Comparative example 4ZnGaO x Preparation of HZSM-5

[0074] ZnGaO was prepared using the method described in Comparative Example 1. x Metal oxides; the amount of zinc nitrate is 0.004 mol and the amount of gallium nitrate is 0.036 mol.

[0075] HZSM-5 same comparison ratio 1.

[0076] Weigh out 0.6g of the above-mentioned ZnGaO x The metal oxide and 0.6 g of HZSM-5 molecular sieve were ground in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved through a tableting sieve to obtain 20-40 mesh ZnGaO. x &HZSM-5 granules.

[0077] Comparative example 5GaZrO x Preparation of HZSM-5

[0078] GaZrO was prepared using the method described in Comparative Example 1. x Metal oxides; the amount of gallium nitrate is 0.004 mol and the amount of zirconium nitrate is 0.036 mol.

[0079] HZSM-5 same comparison ratio 1.

[0080] Weigh out 0.6g of the above-mentioned GaZrO x The metal oxide was ground with 0.6 g of HZSM-5 molecular sieve in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved through a tableting sieve to obtain 20-40 mesh GaZrO. x &HZSM-5 granules.

[0081] Comparative Example 6ZnZrO x Preparation of HMCM-22

[0082] ZnZrO x The preparation method of the metal oxide is the same as that of Comparative Example 1.

[0083] HMCM-22 is a commercial molecular sieve.

[0084] Weigh out 0.6g of the above-mentioned ZnZrO x The metal oxide and 0.6 g of HMCM-22 molecular sieve were ground in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved to obtain 20-40 mesh ZnZrO. x &HMCM-22 granules.

[0085] Comparative Example 7ZnZrO x Preparation of SAPO-11

[0086] ZnZrO x The preparation method of the metal oxide is the same as that of Comparative Example 1.

[0087] SAPO-11 is a commercial molecular sieve.

[0088] Weigh out 0.6g of the above-mentioned ZnZrO x The metal oxide and 0.6 g of SAPO-11 molecular sieve were ground in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved through a tableting sieve to obtain 20-40 mesh ZnZrO. x &SAPO-11 granules.

[0089] Comparative example 8ZnZrOx Preparation of &HMOR

[0090] ZnZrO x The preparation method of the metal oxide is the same as that of Comparative Example 1.

[0091] HMOR is a commercial molecular sieve.

[0092] Weigh out 0.6g of the above-mentioned ZnZrO x The metal oxide and 0.6 g of HMOR molecular sieve were ground together in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved through a tableting sieve to obtain 20-40 mesh ZnZrO. x &HMOR granules.

[0093] Comparative Example 9ZnZrO x Preparation of Hβ

[0094] ZnZrO x The preparation method of the metal oxide is the same as that of Comparative Example 1.

[0095] Hβ is a commercial molecular sieve.

[0096] Weigh out 0.6g of the above-mentioned ZnZrO x The metal oxide and 0.6 g of Hβ molecular sieve were ground together in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved to obtain 20-40 mesh ZnZrO. x &Hβ particles.

[0097] The overnight time in this invention is 12 hours.

[0098] Example 1 ZnZrO x Preparation of Zn-HZSM-5

[0099] ZnZrO x The metal oxide was prepared by a co-precipitation method: 0.002 mol of zinc nitrate and 0.017 mol of zirconium nitrate were dissolved in 100 mL of deionized water; 3.1 g of ammonium carbonate was added to the above solution; the temperature was raised to 70 °C and maintained for 2 h under continuous stirring; the temperature was lowered, and the mixture was allowed to stand for 4 h for aging; then it was centrifuged and washed several times, dried at 110 °C overnight, and finally calcined at 500 °C for 3 h to obtain ZnZrO. x Metal oxides.

[0100] HZSM-5 molecular sieve was prepared by a hydrothermal method: 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a silica content of 30% by mass, 1 mol ethylamine, 17 mol water and 0.0001 mol aluminum nitrate were stirred and placed in a hydrothermal reactor, then crystallized in a rotary oven at 170℃ for 3 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 550℃ for 6 hours to obtain HZSM-5 molecular sieve.

[0101] HZSM-5 molecular sieve was immersed in zinc nitrate solution, stirred evenly with a glass rod, and then allowed to stand for 2 hours before being placed in an 80℃ oven for 10 hours. After drying, it was calcined at 500℃ for 4 hours to obtain Zn-HZSM-5; the Zn loading was 3%.

[0102] Weigh out 0.6g of the above-mentioned ZnZrO x The metal oxide was ground with 0.6 g of Zn-HZSM-5 molecular sieve in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved through a tableting sieve to obtain 20-40 mesh ZnZrO. x &Zn-HZSM-5 granules.

[0103] Example 2 ZnZrO x Preparation of La-HZSM-5

[0104] ZnZrO x The preparation method of the metal oxide is the same as in Example 1.

[0105] Preparation of modified molecular sieve: Zinc nitrate in Example 1 was replaced with lanthanum nitrate to prepare La-HZSM-5; the loading of La was 3%.

[0106] Weigh out 0.6g of the above-mentioned ZnZrO x The metal oxide and 0.6 g of La-HZSM-5 molecular sieve were ground in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved to obtain 20-40 mesh ZnZrO. x &La-HZSM-5 granules.

[0107] Example 3 ZnZrO x Preparation of Ga-HZSM-5

[0108] ZnZrO x The preparation method of the metal oxide is the same as in Example 1.

[0109] Preparation of modified molecular sieve: Zinc nitrate in Example 1 was replaced with gallium nitrate to prepare Ga-HZSM-5; the Ga loading was 3%.

[0110] Weigh out 0.6g of the above-mentioned ZnZrOx The metal oxide and 0.6 g of Ga-HZSM-5 molecular sieve were ground in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved to obtain 20-40 mesh ZnZrO. x &Ga-HZSM-5 particles.

[0111] Example 4 ZnZrO x Preparation of Ce-HZSM-5

[0112] ZnZrO x The preparation method of the metal oxide is the same as in Example 1.

[0113] Preparation of modified molecular sieve: Zinc nitrate in Example 1 was replaced with cerium nitrate to obtain Ce-HZSM-5; the Ce loading was 3%.

[0114] Weigh out 0.6g of the above-mentioned ZnZrO x The metal oxide was ground with 0.6 g of Ce-HZSM-5 molecular sieve in an agate mortar for 30 minutes to achieve a uniform mixture. The resulting powder was then fed into a tablet press and sieved to obtain 20-40 mesh ZnZrO. x &Ce-HZSM-5 granules.

[0115] Example 5

[0116] ZnZrO x The preparation method of the metal oxide is the same as in Example 1.

[0117] Preparation of modified molecular sieves:

[0118] 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a mass content of 30% silica, 1 mol ethylamine, 17 mol water and 0.0085 mol gallium nitrate were stirred and placed in a hydrothermal reactor. The mixture was then crystallized in a rotary oven at 170℃ for 3 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 550℃ for 6 hours to obtain the modified molecular sieve, named Ga-S-1.

[0119] Catalyst preparation: ZnZrO x The modified molecular sieve is mixed at a mass ratio of 1:1 and compressed into tablets to obtain 20-40 mesh ZnZrO. x &Ga-S-1 particles.

[0120] Example 6

[0121] ZnZrO x The preparation method of the metal oxide is the same as in Example 1.

[0122] Preparation of modified molecular sieves:

[0123] 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a mass content of 30% silica, 1 mol ethylamine, 17 mol water and 0.0085 mol iron acetylacetone were stirred and placed in a hydrothermal reactor. The mixture was then crystallized in a rotary oven at 170℃ for 3 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 550℃ for 6 hours to obtain the modified molecular sieve, which was named in-situ synthesized Fe modified Silicalile-1 molecular sieve.

[0124] Catalyst preparation: ZnZrO x The modified molecular sieve is mixed at a mass ratio of 1:1 and compressed into tablets to obtain 20-40 mesh ZnZrO. x &Fe-S-1 particles.

[0125] Example 7

[0126] ZnZrO x The preparation method of the metal oxide is the same as in Example 1.

[0127] Preparation of modified molecular sieves:

[0128] 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a silica content of 30%, 1 mol ethylamine, 17 mol water and 0.0085 mol zinc nitrate were stirred and placed in a hydrothermal reactor. The mixture was then crystallized in a rotary oven at 170℃ for 3 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 550℃ for 6 hours to obtain the modified molecular sieve, which was named in-situ synthesized Zn modified Silicalile-1 molecular sieve.

[0129] Catalyst preparation: ZnZrOx and modified molecular sieve were mixed at a mass ratio of 1:1 and compressed into tablets to obtain 20-40 mesh ZnZrOx&Zn-S-1 particles.

[0130] Example 8

[0131] ZnZrO x The preparation method of the metal oxide is the same as in Example 1.

[0132] Preparation of modified molecular sieves:

[0133] 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a silica content of 30%, 1 mol ethylamine, 17 mol water and 0.0085 mol germanium dioxide were stirred and placed in a hydrothermal reactor. The mixture was then crystallized in a rotary oven at 170℃ for 3 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 550℃ for 6 hours to obtain the modified molecular sieve, which was named in-situ synthesized Ge-modified Silicalile-1 molecular sieve.

[0134] Catalyst preparation: ZnZrOx and modified molecular sieve were mixed at a mass ratio of 1:1 and compressed into tablets to obtain 20-40 mesh ZnZrOx&Ge-S-1 particles.

[0135] Example 9

[0136] GaZrO x The preparation method of the metal oxide is the same as in Example 1, except that zinc nitrate is replaced with gallium nitrate.

[0137] HZSM-5 molecular sieve was prepared by a hydrothermal method: 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a silica content of 30% by mass, 1 mol ethylamine, 17 mol water and 0.0001 mol aluminum nitrate were stirred and then placed in a hydrothermal reactor. The mixture was then crystallized in a rotary oven at 140℃ for 4 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 400℃ for 6 hours to obtain HZSM-5 molecular sieve.

[0138] HZSM-5 molecular sieve was immersed in a 0.001 mol / L gallium nitrate solution, stirred evenly with a glass rod, and then allowed to stand for 2 hours before being placed in an 80℃ oven for 10 hours. After drying, it was calcined at 500℃ for 4 hours to obtain Ga-HZSM-5; the Ga loading was 3%.

[0139] Weigh out 0.2g of the above-mentioned GaZrO x The metal oxide and 0.8 g of Ga-HZSM-5 molecular sieve were ground in an agate mortar for 30 minutes to achieve a uniform mixture. The mixed powder was then placed in a tablet press and sieved to obtain a 20-40 mesh catalyst for the one-step synthesis of 2-methylnaphthalene or 2,6-dimethylnaphthalene by carbon dioxide hydrogenation and naphthalene.

[0140] Example 10

[0141] ZnAlO x The method for preparing the metal oxide is the same as in Example 1, except that zirconium nitrate is replaced with aluminum nitrate.

[0142] HZSM-5 molecular sieve was prepared by a hydrothermal method: 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a silica content of 30% by mass, 1 mol ethylamine, 17 mol water and 0.001 mol aluminum nitrate were stirred and placed in a hydrothermal reactor, then crystallized in a rotary oven at 150℃ for 3.5 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 600℃ for 6 hours to obtain HZSM-5 molecular sieve.

[0143] HZSM-5 molecular sieve was immersed in a 0.0001 mol / L cerium nitrate solution, stirred evenly with a glass rod, and then allowed to stand for 2 hours before being placed in an 80℃ oven for 10 hours. After drying, it was calcined at 500℃ for 4 hours to obtain Ce-HZSM-5; the Ce loading was 3%.

[0144] Weigh out 0.6g of the above-mentioned ZnAlO x The metal oxide and 0.4 g of Ce-HZSM-5 molecular sieve were ground in an agate mortar for 30 minutes to achieve a uniform mixture. The mixed powder was then placed in a tablet press and sieved to obtain a 20-40 mesh catalyst for the one-step synthesis of 2-methylnaphthalene or 2,6-dimethylnaphthalene by carbon dioxide hydrogenation and naphthalene.

[0145] Example 11

[0146] ikB x The method for preparing the metal oxide is the same as in Example 1, except that zinc nitrate is replaced with indium nitrate.

[0147] Preparation of Fe-S-1 modified molecular sieve: 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a silica content of 30% by mass, 1 mol ethylamine, 17 mol water and 0.001 mol acetylacetone iron were stirred and placed in a hydrothermal reactor. Then, the mixture was crystallized in a rotary oven at 150℃ for 4 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 500℃ for 6 hours to obtain Fe-S-1 modified molecular sieve.

[0148] Weigh out 0.3g of the above-mentioned InZrO x The metal oxide and 0.7 g of Fe-S-1 modified molecular sieve were ground in an agate mortar for 30 minutes to achieve a uniform mixture. The mixed powder was then placed in a tablet press and sieved to obtain a 20-40 mesh catalyst for the one-step synthesis of 2-methylnaphthalene or 2,6-dimethylnaphthalene from carbon dioxide hydrogenation and naphthalene.

[0149] Example 12

[0150] ZnGaO x The method for preparing the metal oxide is the same as in Example 1, except that zirconium nitrate is replaced with gallium nitrate.

[0151] Preparation of Ga-S-1 modified molecular sieve: 0.15 mol tetrapropylammonium bromide, 1 mol silica sol with a mass content of 30% silica, 1 mol ethylamine, 17 mol water and 0.001-0.01 mol gallium nitrate were stirred and placed in a hydrothermal reactor. Then, the mixture was crystallized in a rotary oven at 170℃ for 3 days. After crystallization, the mixture was washed 3-5 times, dried for 5 hours, and then calcined at 600℃ for 6 hours to obtain Ga-S-1 modified molecular sieve.

[0152] Weigh out 0.4g of the above-mentioned ZnGaO x The metal oxide and 0.6 g of Ga-S-1 modified molecular sieve were ground in an agate mortar for 30 minutes to achieve a uniform mixture. The mixed powder was then placed in a tablet press and sieved to obtain a 20-40 mesh catalyst for the one-step synthesis of 2-methylnaphthalene or 2,6-dimethylnaphthalene by carbon dioxide hydrogenation and naphthalene.

[0153] The catalytic performance of the one-step synthesis of 2-methylnaphthalene / 2,6-dimethylnaphthalene via carbon dioxide hydrogenation and naphthalene is tested as follows:

[0154] 1. Performance tests were conducted on the catalysts of Comparative Examples 1 to 5:

[0155] Evaluation conditions: 380℃, 3MPa;

[0156] Table 1 shows the results of the reaction evaluation at 380℃ and 3MPa.

[0157]

[0158] 2. The catalysts in Comparative Examples 6-9 were subjected to performance testing;

[0159] Evaluation conditions: 380℃, 3MPa;

[0160] Table 2. Results of the catalyst evaluation reaction at 380℃ and 3MPa.

[0161]

[0162] 3. The catalysts in Examples 1-4 above were subjected to performance testing;

[0163] Evaluation conditions: 380℃, 3MPa;

[0164] Table 3. Results of the catalyst evaluation reaction at 380℃ and 3MPa.

[0165]

[0166] As shown in Table 3, compared with HZSM-5 modified with Zn, La, Ga and Ce, the modified molecular sieves are superior to the parent HZSM-5 molecular sieve in terms of naphthalene conversion, 2-methylnaphthalene selectivity and 2,6-dimethylnaphthalene selectivity. The results show that the Ga-modified molecular sieve has the best performance, with the naphthalene conversion increasing from 22% to 26%, the 2-methylnaphthalene selectivity increasing from 66% to 80%, and the 2,6-dimethylnaphthalene selectivity increasing from 10% to 13%.

[0167] 4. The catalysts in Examples 5-8 above were subjected to performance testing; evaluation conditions: 380℃, 3MPa;

[0168] Table 4. Results of the catalyst evaluation reaction at 380℃ and 3MPa.

[0169]

[0170] A comparison of Tables 1, 2, 3, and 4 shows that ZnZrOx & HZSM-5 exhibits the longest catalyst stability compared to other metal oxides and zeolite molecular sieves with different topologies. Furthermore, its naphthalene conversion, 2-methylnaphthalene selectivity, and 2,6-dimethylnaphthalene selectivity are all superior to other metal oxide catalysts. Compared to HZSM-5, the Zn, La, Ga, and Ce modified HZSM-5 zeolite molecular sieves demonstrate superior performance in naphthalene conversion, 2-methylnaphthalene selectivity, and 2,6-dimethylnaphthalene selectivity. The results indicate that the Ga-modified molecular sieve performs best, increasing naphthalene conversion from 22% to 26%, 2-methylnaphthalene selectivity from 66% to 80%, and 2,6-dimethylnaphthalene selectivity from 10% to 13%. Metal modification of HZSM-5 molecular sieves reduces the total acid content; appropriate L-acidity facilitates the desorption of naphthalene and the target product, thereby improving naphthalene conversion efficiency, inhibiting deep alkylation reactions, and increasing the selectivity of the target product. Compared to modified HZSM-5 molecular sieves, the in-situ synthesized Ga-S-1 exhibits superior naphthalene conversion, 2-methylnaphthalene selectivity, and 2,6-dimethylnaphthalene selectivity compared to Ga-modified HZSM-5 zeolite molecular sieves. Naphthalene conversion increased from 26% to 31%, 2-methylnaphthalene selectivity from 80% to 81%, and 2,6-dimethylnaphthalene selectivity from 13% to 15%. Compared to metal-modified HZSM-5 molecular sieves, the in-situ introduction of heteroatomic metals forms a high-density, moderately strong Brønsted acid, which, while improving naphthalene conversion, also enhances the desorption of the target product and inhibits deep alkylation reactions.

[0171] ZnZrO prepared by mechanical ball milling in this invention x ZnZrO obtained by combining with in-situ synthesized Ga-S-1 x &Ga-S-1 exhibits excellent stability, naphthalene conversion, and 2-methylnaphthalene selectivity along the carbon dioxide hydrogenation route.

[0172] In this invention, the use of carbon dioxide hydrogenation as an alkylating agent differs from the alkylation reaction of syngas with naphthalene. The methylation intermediates generated by carbon dioxide hydrogenation as an alkylating agent differ from those generated by syngas alkylation. This invention effectively reduces the concentration of methylation intermediates, thereby inhibiting further deep alkylation by the intermediates and achieving in-situ generation and consumption of methylation intermediates. The carbon dioxide atmosphere also significantly inhibits coking. The catalyst stability of the syngas route (CN112657538B) is 90 hours, while the catalyst stability of this invention reaches 500 hours. This process route achieves high selectivity for methylnaphthalene while significantly extending catalyst stability.

[0173] In this invention, metal heteroatom-modified zeolite molecular sieves can increase the density of strong acids and weaken their strength, thus exerting a stronger pulling effect on the naphthalene alkylation process and enhancing naphthalene conversion. Simultaneously, it inhibits deep alkylation reactions of the products, effectively improving the selectivity of methylnaphthalene. Furthermore, the modified molecular sieves possess a more rational acid site distribution, which is beneficial for improving the selectivity of 2-methylnaphthalene / 2,6-dimethylnaphthalene.

[0174] This invention utilizes methanol and other active intermediates obtained by reacting carbon dioxide and hydrogen on metal oxides, and further reacts them with naphthalene through a molecular sieve methylation catalyst to achieve a one-step method for preparing high-value-added chemicals. This method overcomes the shortcomings of traditional methanol-naphthalene methylation preparation methods, such as low naphthalene conversion rate and target product selectivity, numerous by-products, rapid catalyst deactivation, and long process flow.

[0175] The above description is only of the preferred embodiment of the present invention and should not be construed as limiting the scope of the claims. The present invention is not limited to the above embodiments, and variations in its specific structure are permitted. All variations made within the scope of the independent claims of the present invention are also within the scope of protection of the present invention.

[0176] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

Claims

1. A catalyst for the one-step synthesis of 2-methylnaphthalene / 2,6-dimethylnaphthalene from carbon dioxide and hydrogen with naphthalene, characterized in that, Including polymetallic oxides and modified zeolite molecular sieves; Among them, metal oxides are oxides composed of two or three metals selected from Zn, Al, In, Zr and Ga; The mass percentage of polymetallic oxides in the catalyst is 20%~60%; Modified zeolite molecular sieves are prepared by the following process: crystallizing a metal nitrate salt and one of an acetylacetone metal salt, tetrapropylammonium bromide, silica sol, ethylamine, and water at 140-170°C for 3-4 days, followed by calcination at 400-600°C for 6 hours to obtain the modified molecular sieve; the metal is Ga, Zn, Fe, or Ge. The molar ratio of tetrapropylammonium bromide, silica sol, ethylamine, water, and metal nitrate salt is 0.15:1:1:17:(0.001-0.01). The molar ratio of tetrapropylammonium bromide, silica sol, ethylamine, water and acetylacetone metal salt is 0.15:1:1:17:(0.001-0.01).

2. The catalyst according to claim 1 for the one-step production of 2-methylnaphthalene / 2,6-dimethylnaphthalene from carbon dioxide and hydrogen and naphthalene, characterized in that, The metal oxide is ZnZrO x ,InZrO x ZnAlO x GaZrO x and ZnGaO x One of them.

3. A method for preparing a catalyst as described in any one of claims 1-2 for the one-step synthesis of 2-methylnaphthalene / 2,6-dimethylnaphthalene from carbon dioxide and hydrogen with naphthalene, characterized in that, Includes the following steps: Metal oxides were mixed with modified molecular sieves and pressed into tablets of 20-40 mesh to obtain a catalyst for the one-step synthesis of 2-methylnaphthalene / 2,6-dimethylnaphthalene from carbon dioxide hydrogenation and naphthalene.

4. The use of a catalyst as described in any one of claims 1-2 in the one-step production of 2-methylnaphthalene or 2,6-dimethylnaphthalene by hydrogenation of carbon dioxide and naphthalene.

5. An application according to claim 4, characterized in that, The catalyst is added to a fixed-bed reactor, and then carbon dioxide, hydrogen and naphthalene are introduced. The reaction is carried out at a temperature of 300 to 550°C and a pressure of 1 to 5 MPa to produce 2-methylnaphthalene or 2,6-dimethylnaphthalene. The volume ratio of carbon dioxide to hydrogen is (0.1–8):1, and the volume hourly space velocity (VHSV) of carbon dioxide and hydrogen is 1000–50000 h⁻¹. -1 The mass hourly space velocity (HSV) of naphthalene is 0.1–5 h⁻¹. -1 .

Citation Information

Patent Citations

  • A method for preparing and applying a catalyst for the one-step synthesis of 2-methylnaphthalene / 2,6-dimethylnaphthalene from syngas and naphthalene.

    CN112657538B

  • Combined catalyst and preparation method thereof, and method for preparing xylene through carbon dioxide hydrogenation coupled toluene alkylation

    CN110743609A

  • Preparation method and application of catalyst for preparing 2-methylnaphthalene / 2, 6-dimethylnaphthalene from synthesis gas and naphthalene through one-step method

    CN112657538A

  • Synthesis of gallium containing silicate molecular sieve catalyst