A MIL-88A(Fe) / BiVO4 composite photocatalyst, its preparation method, and its application.

By loading BiVO₄ onto the surface of MIL-88A(Fe) to form a heterojunction, the problems of insufficient stability and activity of MIL-88A(Fe) photocatalyst were solved, and the effect of efficient reduction of Cr(VI) in water was achieved.

CN118950098BActive Publication Date: 2026-11-24GUILIN UNIVERSITY OF TECHNOLOGY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411012235.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2026-11-24
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The existing MIL-88A(Fe) photocatalyst is prone to photochemical corrosion and rapid recombination of photogenerated electron-hole pairs in the photocatalytic reaction, resulting in insufficient stability and photocatalytic activity, making it difficult to effectively reduce Cr(VI) in water.

Method used

By forming a heterostructure with BiVO₄ in a composite photocatalyst, BiVO₄ is loaded onto the surface of MIL-88A(Fe) to construct a heterojunction, thereby improving the chemical stability and photogenerated electron conduction capability of the material.

Benefits of technology

The material achieves efficient and stable photocatalytic reduction of Cr(VI) in water to Cr(III), improving the photocatalytic activity and Cr(VI) removal efficiency of the material, and the material is recyclable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950098B_ABST
    Figure CN118950098B_ABST
Patent Text Reader

Abstract

This invention proposes a MIL-88A(Fe) / BiVO4 composite photocatalyst, its preparation method, and its application, belonging to the field of photocatalysis technology. This invention uses MIL-88A(Fe) as a support and synthesizes BiVO4 on its surface to construct a heterostructure, significantly improving the chemical stability of the material and preventing photocorrosion. The MIL-88A(Fe) / BiVO4 composite photocatalyst has a high specific surface area, providing a broad contact surface for the adsorption of Cr(VI) in water. The suitable band gap of BiVO4 enhances the conduction ability of photogenerated electrons, enabling efficient catalytic reduction of Cr(VI) in water to Cr(III) under full-spectrum illumination, achieving effective removal of Cr(VI) from wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photocatalysis technology, and particularly relates to a MIL-88A(Fe) / BiVO4 composite photocatalyst, its preparation method, and its application. Background Technology

[0002] Chromium is one of the most important industrial raw materials, used in leather manufacturing, electroplating, textiles, pigments, steel, and catalysis. Due to industrial emissions, chromium pollution in surface and groundwater is becoming a serious problem. In wastewater, chromium generally exists in hexavalent (Cr(VI)) and trivalent (Cr(III)) forms. Cr(VI) is highly water-soluble and has strong migration ability; it is a carcinogenic, teratogenic, and mutagenic pollutant and is classified as a Group A carcinogen. Therefore, the treatment of chromium-containing wastewater mainly targets Cr(VI). Cr(VI) treatment technologies mainly include cation and anion exchange, chemical precipitation, membrane filtration, adsorption, biological methods, and photocatalytic reduction. Among these, photocatalytic reduction is a green and low-cost method and is the preferred method for removing Cr(VI) pollutants from water. Its principle is to reduce the highly toxic Cr(VI) to the less toxic Cr(III).

[0003] The key to the catalytic reduction of Cr(VI) to Cr(III) lies in the choice of catalyst. Metal-organic frameworks (MOFs) have attracted much attention in the field of photocatalysis in recent years due to their excellent photocatalytic performance. The photocatalytic ability of MOFs stems from their abundant metal nodes as catalytic sites, as well as their large specific surface area and the pores required by catalytic molecules. In addition, the characteristics of tunable structure, good biocompatibility, and ease of synthesis make MOFs ideal photocatalysts. MIL-88A(Fe), as a typical MOF material, is composed of Fe... 3+ Synthesized with fumaric acid, MIL-88A(Fe) exhibits unique biocompatibility and environmental friendliness. Compared to other MOF catalysts, MIL-88A(Fe) maintains the integrity of its framework topology while displaying a remarkable reversible swelling effect. This characteristic not only greatly promotes mass transfer in catalytic reactions, allowing reactants to more easily access reaction sites and thus accelerating the reaction, but also ensures that reactants are more effectively adsorbed onto catalytic sites. These advantages make MIL-88A(Fe) a promising candidate for a wide range of applications in catalysis. Despite its excellent adsorption performance, MIL-88A(Fe) still has some significant drawbacks when used as a single-component adsorbent or catalyst. For example, in photocatalytic reactions, MIL-88A(Fe) is prone to photochemical corrosion, as its internal iron-based ions easily escape from the material, leading to dissolution. Furthermore, the rapid recombination of photogenerated electron-hole pairs in MIL-88A(Fe) also significantly limits its photocatalytic activity.

[0004] Therefore, this invention proposes a MIL-88A(Fe) / BiVO4 composite photocatalyst, its preparation method, and its application. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention proposes a MIL-88A(Fe) / BiVO4 composite photocatalyst, its preparation method, and its application. This material possesses high chemical stability, and MIL-88A(Fe) and BiVO4 form a heterostructure, exhibiting excellent visible light responsiveness and photogenerated electron conduction ability, demonstrating superior photocatalytic activity and effectively reducing and removing Cr(VI) from wastewater.

[0006] To achieve the above objectives, the present invention provides a method for preparing a MIL-88A(Fe) / BiVO4 composite photocatalyst, comprising the following steps:

[0007] Bismuth nitrate pentahydrate and ammonium metavanadate were dissolved in dilute nitric acid solution and sodium hydroxide solution, respectively, to obtain bismuth nitrate pentahydrate solution and ammonium metavanadate solution. The ammonium metavanadate solution was added dropwise to the bismuth nitrate pentahydrate solution under magnetic stirring to obtain BiVO4 solution. Then, MIL-88A(Fe) powder was added to the BiVO4 solution, the pH was adjusted, and the mixture was stirred evenly to obtain a mixed solution.

[0008] The mixed solution was poured into a hydrothermal reactor for hydrothermal reaction, then cooled to room temperature, centrifuged, washed and dried to obtain the MIL-88A(Fe) / BiVO4 composite photocatalyst.

[0009] Furthermore, the ratio of bismuth nitrate pentahydrate to dilute nitric acid solution is 1 mmol: 30 mL, and the ratio of ammonium metavanadate to sodium hydroxide solution is 1 mmol: 30 mL.

[0010] Furthermore, the concentrations of both the dilute nitric acid solution and the sodium hydroxide solution are 2M.

[0011] Furthermore, the dropping rate is 5 mL / min.

[0012] Furthermore, the mass ratio of the MIL-88A(Fe) powder to BiVO4 is (2-3):1.

[0013] Further, adjust the pH to 1.

[0014] Furthermore, the hydrothermal reaction is carried out at a temperature of 180°C for 15 hours.

[0015] Further, the method for preparing the MIL-88A(Fe) powder is as follows: fumaric acid and ferric chloride hexahydrate are stirred at 600 r / min for 30 min, and then placed in an oil bath at 100°C for 4 h to obtain MIL-88A(Fe). The MIL-88A(Fe) is washed with ultrapure water (impedance greater than 18Ω), dried at 60°C, and ground to 5-10 μm to obtain MIL-88A(Fe) powder.

[0016] Bismuth vanadate (BiVO4) exhibits excellent chemical stability and a suitable band gap, demonstrating outstanding responsiveness to visible light. This invention innovatively loads BiVO4 onto the surface of MIL-88A(Fe), constructing a novel heterojunction composite material. This strategy not only solves the problem of insufficient stability of single MIL-88A(Fe) material but also enhances the conduction ability of photogenerated electrons through the suitable band gap of BiVO4, thereby significantly enhancing the photocatalytic reduction capability of the composite material and improving the removal efficiency of Cr(VI) from wastewater.

[0017] The present invention also provides a MIL-88A(Fe) / BiVO4 composite photocatalyst prepared by the preparation method described above.

[0018] The present invention also provides the application of the MIL-88A(Fe) / BiVO4 composite photocatalyst in the treatment of Cr(VI)-containing wastewater. The MIL-88A(Fe) / BiVO4 composite photocatalyst is added to Cr(VI)-containing wastewater, and tartaric acid is added to carry out photocatalytic reduction.

[0019] Furthermore, the amount of the MIL-88A(Fe) / BiVO4 composite photocatalyst added to the Cr(VI)-containing wastewater is 400-500 mg / L, the amount of tartaric acid added to the Cr(VI)-containing wastewater is 2 mM, the concentration of Cr(VI) in the Cr(VI)-containing wastewater is 10-20 mg / L, and the pH of the Cr(VI)-containing wastewater is 2-3.

[0020] The tartaric acid is used as a hole trapping agent, interacting with holes through electron transfer to fill holes and restore the electronic balance of the material in water.

[0021] Furthermore, the light intensity for the photocatalytic reduction is 15 A, and the illumination time is 15 min.

[0022] Furthermore, the application of the MIL-88A(Fe) / BiVO4 composite photocatalyst in the treatment of Cr(VI)-containing wastewater specifically includes the following steps:

[0023] The MIL-88A(Fe) / BiVO4 composite photocatalyst and tartaric acid were added to Cr(VI)-containing wastewater and stirred in the dark for 20-30 minutes. Then, the mixture was reacted for 15 minutes under the illumination of a 220W xenon lamp with a light source intensity of 15A.

[0024] Compared with the prior art, the present invention has the following advantages and technical effects:

[0025] (1) This invention synthesizes a novel MIL-88A(Fe) / BiVO4 composite photocatalyst material via a hydrothermal method. This material uses MIL-88A(Fe) as a support, with BiVO4 loaded on its surface to construct a heterostructure, significantly improving the material's chemical stability and preventing photocorrosion. Due to the high specific surface area of ​​the prepared MIL-88A(Fe) / BiVO4 composite photocatalyst material, a broad contact surface is provided for the adsorption of Cr(VI) in water. The suitable band gap of BiVO4 enhances the conduction ability of photogenerated electrons, enabling the efficient catalytic reduction of Cr(VI) in water to Cr(III) under full-spectrum illumination.

[0026] (2) The MIL-88A(Fe) / BiVO4 composite photocatalyst material of the present invention can be recycled. Attached Figure Description

[0027] The accompanying drawings, which form part of this application, are used to provide a further understanding of this application. The illustrative embodiments and descriptions of this application are used to explain this application and do not constitute an undue limitation of this application. In the drawings:

[0028] Figure 1 The image shows a scanning electron microscope (SEM) image of the MIL-88A(Fe) orange photocatalyst in Comparative Example 1.

[0029] Figure 2 The image shows a scanning electron microscope (SEM) image of the BiVO4 photocatalyst in Comparative Example 2.

[0030] Figure 3 This is a scanning electron microscope image of the MIL-88A(Fe) / BiVO4 composite photocatalyst in Example 1;

[0031] Figure 4 The XRD diffraction patterns of the photocatalysts prepared in Comparative Examples 1-5 and Examples 1-2 are shown.

[0032] Figure 5 The UV-Vis diffuse reflectance spectra of the catalysts prepared in Comparative Examples 1-5 and Examples 1-2 are shown, where (a) is the UV-Vis diffuse reflectance spectrum and (b) is the UV-Vis diffuse reflectance-bandgap calculated spectrum.

[0033] Figure 6 The performance curves of composite photocatalysts in reducing Cr(VI) in water for each treatment group are shown.

[0034] Figure 7 The results show the photocatalytic reduction of Cr(VI) in water using the MIL-88A(Fe) / BiVO4 composite photocatalyst in Examples 1, 2, and Comparative Examples 3-5.

[0035] Figure 8 The results show the photocatalytic reduction of Cr(VI) in water by M2B1 under different conditions. Detailed Implementation

[0036] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0037] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.

[0038] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.

[0039] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be readily apparent to those skilled in the art. This specification and embodiments are merely exemplary.

[0040] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.

[0041] This invention provides a method for preparing a MIL-88A(Fe) / BiVO4 composite photocatalyst, comprising the following steps:

[0042] Bismuth nitrate pentahydrate and ammonium metavanadate were dissolved in dilute nitric acid solution and sodium hydroxide solution, respectively, to obtain bismuth nitrate pentahydrate solution and ammonium metavanadate solution. The ammonium metavanadate solution was added dropwise to the bismuth nitrate pentahydrate solution under magnetic stirring to obtain BiVO4 solution. Then, MIL-88A(Fe) powder was added to the BiVO4 solution, and the pH was adjusted to acidic. The mixture was stirred evenly to obtain a mixed solution.

[0043] The mixed solution was poured into a hydrothermal reactor for hydrothermal reaction, then cooled to room temperature, centrifuged, washed and dried to obtain the MIL-88A(Fe) / BiVO4 composite photocatalyst.

[0044] In a preferred embodiment of the present invention, the ratio of bismuth nitrate pentahydrate to dilute nitric acid solution is 1 mmol: 30 mL, and the ratio of ammonium metavanadate to sodium hydroxide solution is 1 mmol: 30 mL.

[0045] In a preferred embodiment of the present invention, the concentrations of both the dilute nitric acid solution and the sodium hydroxide solution are 2M.

[0046] In a preferred embodiment of the present invention, the dripping rate is 5 mL / min.

[0047] In a preferred embodiment of the present invention, the mass ratio of the MIL-88A(Fe) powder to the BiVO4 solution is (2-3):1.

[0048] In a preferred embodiment of the present invention, the pH is adjusted to 1.

[0049] In a preferred embodiment of the present invention, the hydrothermal reaction is carried out at a temperature of 180°C for 15 hours.

[0050] In a preferred embodiment of the present invention, the method for preparing the MIL-88A(Fe) powder is as follows: fumaric acid and ferric chloride hexahydrate are stirred at 600 r / min for 30 min, and then placed in an oil bath at 100°C for 4 h to obtain MIL-88A(Fe). The MIL-88A(Fe) is washed with ultrapure water (impedance greater than 18 Ω), dried at 60°C, and ground to 5-10 μm to obtain MIL-88A(Fe) powder.

[0051] This invention also provides a MIL-88A(Fe) / BiVO4 composite photocatalyst prepared by the aforementioned method.

[0052] The present invention also provides the application of the MIL-88A(Fe) / BiVO4 composite photocatalyst in the treatment of Cr(VI)-containing wastewater. The MIL-88A(Fe) / BiVO4 composite photocatalyst is added to the Cr(VI)-containing wastewater, and tartaric acid is added to carry out photocatalytic reduction.

[0053] In a preferred embodiment of the present invention, the amount of the MIL-88A(Fe) / BiVO4 composite photocatalyst added to the Cr(VI)-containing wastewater is 400-500 mg / L, the amount of tartaric acid added to the Cr(VI)-containing wastewater is 2 mM, the concentration of Cr(VI) in the Cr(VI)-containing wastewater is 10-20 mg / L, and the pH of the Cr(VI)-containing wastewater is 2-3.

[0054] In a preferred embodiment of the present invention, the light intensity of the photocatalytic reduction is 15A and the light exposure time is 15min.

[0055] In a preferred embodiment of the present invention, the application of the MIL-88A(Fe) / BiVO4 composite photocatalyst in the treatment of Cr(VI)-containing wastewater specifically includes the following steps:

[0056] The MIL-88A(Fe) / BiVO4 composite photocatalyst and tartaric acid were added to Cr(VI)-containing wastewater and stirred in the dark for 20-30 minutes. Then, the mixture was reacted for 15 minutes under the illumination of a 220W xenon lamp with a light source intensity of 15A.

[0057] Unless otherwise specified, the equipment, reagents, processes, parameters, etc. involved in the embodiments of this invention are all conventional equipment, reagents, processes, parameters, etc.

[0058] All ranges listed in this invention include all point values ​​within that range.

[0059] In this embodiment of the invention, "room temperature" refers to the normal ambient temperature, which can be 10-30℃.

[0060] The technical solution of the present invention will be further illustrated by the following embodiments.

[0061] Example 1

[0062] A method for preparing a MIL-88A(Fe) / BiVO4 composite photocatalyst, comprising the following steps:

[0063] (1) Dissolve 10 mmol fumaric acid and 10 mmol ferric chloride hexahydrate in 100 mL deionized water, then add the ferric chloride hexahydrate aqueous solution to the fumaric acid solution at room temperature and stir vigorously at 600 r / min for 30 min to obtain solution A.

[0064] (2) Transfer solution A to a three-necked flask and keep it in an oil bath at 100°C for 4 hours to obtain MIL-88A(Fe). After cooling to room temperature, collect the orange precipitate of MIL-88A(Fe) by centrifugation, wash it with ultrapure water (impedance greater than 18Ω), and then vacuum dry it at 60°C for 12 hours to obtain the orange photocatalyst of MIL-88A(Fe). Grind it to 5-10 μm to obtain MIL-88A(Fe) powder.

[0065] (3) Dissolve 1 mmol of bismuth nitrate pentahydrate and 1 mmol of ammonium metavanadate in 30 mL of dilute nitric acid solution and 30 mL of sodium hydroxide solution respectively to obtain bismuth nitrate pentahydrate solution and ammonium metavanadate solution. The concentration of dilute nitric acid solution and sodium hydroxide solution is 2M. Add ammonium metavanadate solution dropwise to bismuth nitrate pentahydrate solution at a rate of 5 mL / min under magnetic stirring until the solution becomes clear and transparent to obtain solution B, which is BiVO4 solution.

[0066] (4) Add 0.6g of MIL-88A(Fe) powder obtained in step (2) to 0.3g of solution B obtained in step (3) (the mass ratio of MIL-88A(Fe) powder to BiVO4 solution is 2:1), adjust the pH to 1, stir for 1h, transfer to a reaction vessel and hydrothermally react at 180℃ for 15h, cool to room temperature, wash repeatedly with ethanol and deionized water 3 times, and dry at 60℃ for 12h to obtain the MIL-88A(Fe) / BiVO4 composite photocatalyst, denoted as M2B1.

[0067] Example 2

[0068] Same as Example 1, except that in step (4), 0.9g of MIL-88A(Fe) powder obtained in step (2) is added to 0.3g of solution B obtained in step (3) (the mass ratio of MIL-88A(Fe) powder to BiVO4 solution is 3:1). The resulting MIL-88A(Fe) / BiVO4 composite photocatalyst is denoted as M3B1.

[0069] Comparative Example 1

[0070] The preparation method of MIL-88A(Fe) orange photocatalyst is the same as steps (1) and (2) in Example 1, specifically as follows:

[0071] (1) Dissolve 10 mmol fumaric acid and 10 mmol ferric chloride hexahydrate in 100 mL deionized water, then add the ferric chloride hexahydrate aqueous solution to the fumaric acid solution at room temperature and stir vigorously at 600 r / min for 30 min to obtain solution A.

[0072] (2) Transfer solution A to a three-necked flask and store it in an oil bath at 100°C for 4 hours to obtain MIL-88A(Fe). After cooling to room temperature, collect the orange precipitate of MIL-88A(Fe) by centrifugation, wash it with ultrapure water (impedance greater than 18Ω), and then vacuum dry it at 60°C for 12 hours to obtain the orange photocatalyst of MIL-88A(Fe). Grind it to 5-10 μm to obtain the orange photocatalyst of MIL-88A(Fe).

[0073] Comparative Example 2

[0074] The preparation method of BiVO4 photocatalyst is the same as step (3) in Example 1, specifically as follows:

[0075] 1 mmol of bismuth nitrate pentahydrate and 1 mmol of ammonium metavanadate were dissolved in 30 mL of dilute nitric acid solution and 30 mL of sodium hydroxide solution, respectively, to obtain bismuth nitrate pentahydrate solution and ammonium metavanadate solution. The concentration of both dilute nitric acid solution and sodium hydroxide solution was 2 M. The ammonium metavanadate solution was added dropwise to the bismuth nitrate pentahydrate solution at a rate of 5 mL / min under magnetic stirring until the solution became clear and transparent, thus obtaining the BiVO4 photocatalyst.

[0076] Comparative Example 3

[0077] Same as Example 1, except that in step (4), the amount of MIL-88A(Fe) powder added is 0.3g (the mass ratio of MIL-88A(Fe) powder to BiVO4 solution is 1:1), and the resulting MIL-88A(Fe) / BiVO4 composite photocatalyst is denoted as M1B1.

[0078] Comparative Example 4

[0079] Same as Example 1, except that in step (4), the amount of MIL-88A(Fe) powder added is 0.15g (the mass ratio of MIL-88A(Fe) powder to BiVO4 solution is 1:2), and the resulting MIL-88A(Fe) / BiVO4 composite photocatalyst is denoted as M1B2.

[0080] Comparative Example 5

[0081] Same as Example 1, except that in step (4), the amount of MIL-88A(Fe) powder added is 0.1g (the mass ratio of MIL-88A(Fe) powder to BiVO4 solution is 1:3), and the resulting MIL-88A(Fe) / BiVO4 composite photocatalyst is denoted as M1B3.

[0082] Comparative Example 6

[0083] Same as Example 1, except that the BiVO4 solution was replaced by an equal mass of Bi2MoO6 solution, which was prepared according to the following method:

[0084] Add 2 mmol of bismuth nitrate pentahydrate to a beaker containing 30 ml of ethanol and stir for 30 min. Then add 4 mmol of sodium molybdate dihydrate to the beaker and stir to obtain a Bi2MoO6 solution.

[0085] The composite photocatalyst obtained in Comparative Example 6 was MIL-88A(Fe) / Bi2MoO6 composite photocatalyst.

[0086] Performance testing

[0087] I. Scanning electron microscope image

[0088] Scanning electron microscopy (SEM) image of the MIL-88A(Fe) orange photocatalyst in Comparative Example 1 is shown below. Figure 1 As shown in the figure, it exhibits a smooth spindle-shaped morphology. The scanning electron microscope image of the BiVO4 photocatalyst in Comparative Example 2 is shown below. Figure 2 As shown, it can be seen that it consists of a bunch of irregular columnar structures. The scanning electron microscope image of the MIL-88A(Fe) / BiVO4 composite photocatalyst in Example 1 is as follows. Figure 3 As shown, the combination of the two results in the formation of many heterojunctions on the surface of the spindle, indicating that the MIL-88A(Fe) / BiVO4 composite photocatalyst was successfully prepared.

[0089] II. XRD Diffraction Pattern

[0090] The XRD diffraction patterns of the photocatalysts prepared in Comparative Examples 1-5 and Examples 1-2 are shown below. Figure 4As can be seen, the characteristic peaks of the MIL-88A(Fe) catalyst in Comparative Example 1 appear at 10.2° and 12.9°, which belong to the (101) and (002) crystal planes of MIL-88A(Fe). The characteristic peaks of the BiVO4 photocatalyst in Comparative Example 2 appear at 28.8° and 30.5°, which belong to the (121) and (040) crystal planes of the BiVO4 standard. The XRD patterns of the MIL-88A(Fe) / BiVO4 composite photocatalysts in Examples 1 and 2 clearly show two characteristic peaks at 28.8° and 30.5°, belonging to the BiVO4 photocatalyst, indicating that the BiVO4 photocatalyst was successfully loaded onto the MIL-88A(Fe) surface. However, due to the change in the surface structure of the composite material, the characteristic peaks of MIL-88A(Fe) shifted. The difference between the MIL-88A(Fe) / BiVO4 composite photocatalysts in Comparative Examples 3-5 and the MIL-88A(Fe) / BiVO4 composite photocatalyst in Example 1 lies in the different peak heights of the characteristic peaks, which is due to the different amounts of MIL-88A(Fe) added.

[0091] III. Ultraviolet-Visible Diffuse Reflectance Spectrum

[0092] The UV-Vis diffuse reflectance spectra of the catalysts prepared in Comparative Examples 1-5 and Examples 1-2 are shown below. Figure 5 (a) is the UV-Vis diffuse reflectance spectrum, and (b) is the UV-Vis diffuse reflectance-bandgap calculated spectrum. It can be seen that the MIL-88A(Fe) / BiVO4 photocatalysts (M2B1, M3B1) described in Examples 1 and 2 have smaller bandgap values, which are more conducive to electron transitions, thus enhancing photocatalytic performance. The photocatalyst materials in Comparative Examples 3-5 differ from the MIL-88A(Fe) / BiVO4 composite photocatalysts described in Examples 1 and 2 in that they have larger bandgap values ​​and slower electron conduction rates than the composite photocatalysts in Examples 1 and 2.

[0093] IV. Test for Cr(VI) in water by photocatalytic reduction

[0094] The MIL-88A(Fe) orange photocatalyst in Comparative Example 1, the BiVO4 photocatalyst in Comparative Example 2, and the MIL-88A(Fe) / BiVO4 composite photocatalyst in Example 1 were tested for photocatalytic reduction of Cr(VI) in water, and the following steps were performed:

[0095] TA / M2B1 treatment group: 20 mg of the MIL-88A(Fe) / BiVO4 composite photocatalyst obtained in Example 1 was weighed and added to 50 mL of water containing 20 mg / L hexavalent chromium (Cr(VI)). Tartaric acid (TA) was added at a dosage of 2 mM for coupling. The pH was adjusted to 2 with dilute nitric acid. After a 30 min dark reaction to allow the catalyst to adsorb at equilibrium, the light source (220 W xenon lamp, light source intensity 15 A) was turned on and irradiated for 15 min. Samples were taken every 3 min and the absorbance was measured with a UV spectrophotometer.

[0096] TA / BiVO4 treatment group: 20 mg of BiVO4 composite photocatalyst obtained in Comparative Example 2 was weighed and added to 50 mL of water containing 20 mg / L hexavalent chromium (Cr(VI)). Tartaric acid (TA) was added at a dosage of 2 mM for coupling. The pH was adjusted to 2 with dilute nitric acid. After a 30 min dark reaction to allow the catalyst to adsorb at equilibrium, the light source (220 W xenon lamp, light source intensity 15 A) was turned on and irradiated for 15 min. Samples were taken every 3 min and the absorbance was measured with a UV spectrophotometer.

[0097] TA treatment group: Tartaric acid (TA) was added to 50 mL of water containing 20 mg / L hexavalent chromium (Cr(VI)) at a dosage of 2 mM. The pH was adjusted to 2 with dilute nitric acid. After a 30 min dark reaction to allow the catalyst adsorption to reach equilibrium, the light source (220 W xenon lamp, light source intensity 15 A) was turned on and irradiated for 15 min. Samples were taken every 3 min and the absorbance was measured with a UV spectrophotometer.

[0098] MIL-88A(Fe) / BiVO4 treatment group: 20 mg of the MIL-88A(Fe) / BiVO4 composite photocatalyst obtained in Example 1 was weighed and added to 50 mL of water containing 20 mg / L hexavalent chromium (Cr(VI)). The pH was adjusted to 2 with dilute nitric acid. After a 30 min dark reaction to allow the catalyst adsorption to reach equilibrium, the light source (220 W xenon lamp, light source intensity 15 A) was turned on and irradiated for 15 min. Samples were taken every 3 min and the absorbance was measured with a UV spectrophotometer.

[0099] MIL-88A treatment group: 20 mg of the MIL-88A(Fe) composite photocatalyst obtained in Comparative Example 1 was weighed and added to 50 mL of water containing 20 mg / L hexavalent chromium (Cr(VI)). The pH was adjusted to 2 with dilute nitric acid. After a 30 min dark reaction to allow the catalyst adsorption to reach equilibrium, the light source (220 W xenon lamp, light source intensity 15 A) was turned on and irradiated for 15 min. Samples were taken every 3 min and the absorbance was measured with an ultraviolet spectrophotometer.

[0100] BiVO4 treatment group: 20 mg of BiVO4 composite photocatalyst obtained from Comparative Example 2 was weighed and added to 50 mL of water containing 20 mg / L hexavalent chromium (Cr(VI)). The pH was adjusted to 2 with dilute nitric acid. After a 30 min dark reaction to allow the catalyst adsorption to reach equilibrium, the light source (220 W xenon lamp, light source intensity 15 A) was turned on and irradiated for 15 min. Samples were taken every 3 min and the absorbance was measured with an ultraviolet spectrophotometer.

[0101] TA / MIL-88A treatment group: 20 mg of MIL-88A (Fe) composite photocatalyst obtained from Comparative Example 1 was weighed and added to 50 mL of water containing 20 mg / L hexavalent chromium (Cr(VI)). Tartaric acid (TA) was added at a dosage of 2 mM for coupling. The pH was adjusted to 2 with dilute nitric acid. After a 30 min dark reaction to allow the catalyst adsorption to reach equilibrium, the light source (220 W xenon lamp, light source intensity 15 A) was turned on and irradiated for 15 min. Samples were taken every 3 min and the absorbance was measured using a UV spectrophotometer.

[0102] MIL-88A(Fe) / Bi2MoO6 treatment group: 20 mg of the MIL-88A(Fe) / Bi2MoO6 composite photocatalyst obtained in Comparative Example 6 was weighed and added to 50 mL of water containing 20 mg / L hexavalent chromium (Cr(VI)). The pH was adjusted to 2 with dilute nitric acid. After a 30 min dark reaction to allow the catalyst adsorption to reach equilibrium, the light source (220 W xenon lamp, light source intensity 15 A) was turned on and irradiated for 15 min. Samples were taken every 3 min and the absorbance was measured with a UV spectrophotometer.

[0103] TA / MIL-88A(Fe) / Bi2MoO6 treatment group: 20 mg of the MIL-88A(Fe) / Bi2MoO6 composite photocatalyst obtained in Comparative Example 6 was weighed and added to 50 mL of water containing 20 mg / L hexavalent chromium (Cr(VI)). Tartaric acid (TA) was added at a dosage of 2 mM for coupling. The pH was adjusted to 2 with dilute nitric acid. After a 30 min dark reaction to allow the catalyst to adsorb at equilibrium, the light source (220 W xenon lamp, light source intensity 15 A) was turned on and irradiated for 15 min. Samples were taken every 3 min and the absorbance was measured with a UV spectrophotometer.

[0104] The performance curves of the photocatalysts in reducing Cr(VI) in water for each treatment group are shown below. Figure 6As can be seen, the MIL-88A(Fe) photocatalyst in Comparative Example 1 and the BiVO4 photocatalyst in Comparative Example 2 exhibit certain adsorption and photocatalytic reduction effects, but the reduction effect is slow and limited. The efficiency of the MIL-88A(Fe) / BiVO4 composite photocatalyst, after combining the two, is greatly improved, and Cr(VI) can be completely reduced to Cr(III) within 9 minutes. In the experiments involving the TA / MIL-88A(Fe) treatment group, due to the instability of the MIL-88A(Fe) material, especially during the coupling reaction with tartaric acid, an unexpected interaction occurred, leading to the dissolution of the MIL-88A(Fe) sample. The data obtained from the TA / MIL-88A(Fe) treatment group cannot accurately reflect the expected experimental results; therefore, this group of data will not be included in the subsequent data analysis and discussion.

[0105] Using the same method described above, the MIL-88A(Fe) / BiVO4 composite photocatalyst in Examples 1, 2, and Comparative Examples 3-5 was tested for photocatalytic reduction of Cr(VI) in water. The test results are shown below. Figure 7 (The figure uses 1∶1n(MIL-88(A)):(BiVO4) as an example, which represents M1B1). It can be seen that in Example 1, the MIL-88A(Fe) / BiVO4 composite photocatalyst material (M2B1) can completely reduce Cr(VI) to Cr(III) within 9 minutes, M3B1 can completely reduce Cr(VI) within 12 minutes, M1B1 can only reduce about 50% of Cr(VI) within 15 minutes, M1B2 can only reduce about 80% of Cr(VI) within 15 minutes, and M1B3 can only reduce about 70% of Cr(VI) within 15 minutes.

[0106] V. Tests of M2B1 photocatalytic reduction of Cr(VI) in water under different conditions

[0107] Using the photocatalyst material M2B1 prepared in Example 1 as the object, the effects of the concentration of Cr(VI) solution (a), the amount of catalyst (M2B1) added (b), the pH value of Cr(VI) solution (c), and the amount of TA added (d) on the removal of Cr(VI) were investigated. Specifically:

[0108] Weigh 20 mg of the M2B1 catalyst prepared in Example 1 and add it to 50 mL of water containing 20 mg / L hexavalent chromium (Cr(VI)). Then add tartaric acid (TA) at a dosage of 2 mM. Adjust the pH to 2 with dilute nitric acid. Allow the catalyst to undergo a dark reaction for 30 min to reach adsorption equilibrium. Then turn on the light source (220 W xenon lamp, light source intensity 15 A) and irradiate for 15 min. Take a sample every 3 min and measure the absorbance with a UV spectrophotometer.

[0109] The concentration of Cr(VI) solution was changed to (10-25) mg / L, the catalyst dosage was (10-25) mg, the pH value of Cr(VI) solution was 1-10, and the TA dosage was (0.4-2.4) mM, respectively, and the performance of M2B1 photocatalytic reduction of Cr(VI) in water was measured under each condition.

[0110] In addition, based on the above method, the use of M2B1 catalyst was omitted, and only (0.4-2.4) mM TA was added. The performance of TA alone in photocatalytic reduction of Cr(VI) in water was tested under the same dark reaction and light conditions.

[0111] The performance of M2B1 in photocatalytic reduction of Cr(VI) in water under varying Cr(VI) solution concentration (a), catalyst (M2B1) dosage (b), Cr(VI) solution pH (c), and TA dosage (d) is shown in the figure. Figure 8 .Depend on Figure 8 (a) It can be seen that when the Cr(VI) concentration is 10, 15, and 20 mg / L, M2B1 can completely reduce Cr(VI) to Cr(III) within 9 minutes. However, when the concentration rises to 25 mg / L, M2B1 can only reduce about 82% of Cr(VI) within 15 minutes. Figure 8 (b) It can be seen that when the dosage of M2B1 is 10 mg, 85% of Cr(VI) can be reduced within 15 minutes; when the dosage is 15 mg, 95% of Cr(VI) can be reduced within 15 minutes; and when the dosage is 20 mg, Cr(VI) can be completely reduced within 9 minutes. However, when the dosage is increased to 25 mg, it takes 12 minutes to completely reduce Cr(VI). This is because the increased dosage reduces the transmission of visible light. Figure 8 (c) It can be seen that M2B1 can completely reduce Cr(VI) to Cr(III) within 9 minutes at pH = 1 and 2. Considering that the acidity is too strong at pH = 1, the catalyst may undergo a small amount of dissolution. Therefore, pH = 2 was chosen as the optimal acidity. Figure 8 (d) It can be seen that M2B1 has the best performance when TA = 2mM.

[0112] Based on the above performance test results, it can be seen that this invention successfully loaded BiVO4 onto the surface of MIL-88A(Fe), constructing a novel heterojunction composite material. This material exhibits good chemical stability. The results of the examples show that the MIL-88A(Fe) / BiVO4 composite photocatalyst has an excellent band gap value, which is beneficial for electron transitions and can greatly accelerate the photocatalytic reduction reaction of Cr(VI).

[0113] The above are merely preferred embodiments of this application, but the scope of protection of this application is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the scope of protection of this application. Therefore, the scope of protection of this application should be determined by the scope of the claims.

Claims

1. The application of MIL-88A(Fe) / BiVO4 composite photocatalyst in the treatment of Cr(VI)-containing wastewater, characterized in that, The MIL-88A(Fe) / BiVO4 composite photocatalyst is added to Cr(VI)-containing wastewater, and tartaric acid is added for photocatalytic reduction. The preparation method of the MIL-88A(Fe) / BiVO4 composite photocatalyst includes the following steps: Bismuth nitrate pentahydrate and ammonium metavanadate were dissolved in dilute nitric acid solution and sodium hydroxide solution, respectively, to obtain bismuth nitrate solution and ammonium metavanadate solution. The ammonium metavanadate solution was added dropwise to the bismuth nitrate solution under magnetic stirring to obtain BiVO4 solution. Then, MIL-88A(Fe) powder was added to the BiVO4 solution and the pH was adjusted to 1. The MIL-88A(Fe) / BiVO4 composite photocatalyst was obtained through hydrothermal reaction. The ratio of bismuth nitrate pentahydrate to dilute nitric acid solution is 1 mmol: 30 mL, and the ratio of ammonium metavanadate to sodium hydroxide solution is 1 mmol: 30 mL. The concentrations of both the dilute nitric acid solution and the sodium hydroxide solution are 2M. The mass ratio of MIL-88A(Fe) powder to BiVO4 is (2-3):1; The hydrothermal reaction was carried out at a temperature of 180°C for 15 hours. The method for preparing the MIL-88A (Fe) powder is as follows: fumaric acid and ferric chloride hexahydrate are stirred at 600 r / min for 30 min, and then placed in an oil bath at 100°C for 4 h to obtain MIL-88A (Fe). The MIL-88A (Fe) is washed with ultrapure water with an impedance greater than 18 Ω, dried at 60°C, and ground to 5-10 μm to obtain the MIL-88A (Fe) powder.

2. The application of the MIL-88A(Fe) / BiVO4 composite photocatalyst according to claim 1 in the treatment of Cr(VI)-containing wastewater, characterized in that, The MIL-88A(Fe) / BiVO4 composite photocatalyst is added at a concentration of 400-500 mg / L in Cr(VI)-containing wastewater, the tartaric acid is added at a concentration of 2 mM in Cr(VI)-containing wastewater, the Cr(VI) concentration in the Cr(VI)-containing wastewater is 10-20 mg / L, and the pH of the Cr(VI)-containing wastewater is 2-3.

Citation Information

Patent Citations

  • Semiconductor photocatalyst as well as preparation method and application thereof

    CN109999786A