A method for passivation of heavy metals and release of organic matter in coal gangue or gasification slag
By generating hydrotalcite-like materials with extremely low solubility product constants, heavy metals in coal gangue or gasification slag are fixed in the crystal lattice, solving the problems of high cost of heavy metal passivation and insufficient utilization of organic matter in existing technologies, and realizing low-cost and efficient heavy metal passivation and organic matter release.
Patent Information
- Application Number
- CN202411026820.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing technologies for removing heavy metals from coal gangue and gasification slag suffer from problems such as large consumption of mineral materials and washing agents, high energy consumption, high cost, and failure to effectively passivate heavy metals. At the same time, they fail to fully utilize the organic nutrients in coal gangue and gasification slag.
By mixing calcium oxide and ferric nitrate with coal gangue or gasification slag, a hydrotalcite-like substance with an extremely low solubility product constant is generated. This transforms heavy metals from a free state to a mineralized state, fixing them in the lattice of the hydrotalcite-like substance. At the same time, it breaks the dissolution process of coal gangue or gasification slag to release organic matter.
This method achieves low-cost and efficient passivation of heavy metals, reduces the content of available heavy metals, and releases organic nutrients that can be absorbed and utilized by plants, thereby enhancing the resource utilization value of coal gangue and gasification slag.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of effective utilization of solid waste resources, and in particular to a method for passivating heavy metals and releasing organic matter in coal gangue or gasification slag. Background Technology
[0002] Coal gangue contains various toxic and harmful heavy metals, such as lead, cadmium, nickel, chromium, and copper. When coal gangue is exposed to the atmosphere, water bodies, and soil, these heavy metals are released, polluting the surrounding environment and accumulating through the food chain, thus harming human health. Furthermore, the heavy metals in coal gangue pose a series of challenges to its resource utilization. For example, when using coal gangue for backfilling or soil reclamation, it is necessary to consider whether heavy metals will migrate and pollute surrounding land and crops. In addition to heavy metals, coal gangue also contains abundant organic matter. Therefore, it is necessary to develop a technology that fully utilizes the organic nutrients contained in coal gangue while removing heavy metals, thereby improving the resource utilization rate and ecological value of coal gangue.
[0003] Similarly, coal gasification slag is a solid waste generated during coal gasification technology, with annual emissions exceeding 33 million tons. However, the current disposal methods for coal gasification slag mainly involve landfilling and stockpiling, resulting in extremely low utilization value. Like coal gangue, coal gasification slag is rich in organic matter, but the heavy metals in it also hinder its resource utilization.
[0004] Currently, the most common methods for removing heavy metals from coal gangue or gasification slag are to passivate the heavy metals using microorganisms, mineral materials, and leaching agents.
[0005] Chinese patent CN116903421A discloses a method for passivating heavy metals in coal gangue using microorganisms. The method involves crushing the coal gangue into powder with a particle size of less than 115 μm, then cultivating the SK1 bacterium, which exhibits rapid and stable reproduction. The SK1 bacterium is then mixed with the coal gangue for fermentation. This method utilizes the metabolic products of the SK1 bacterium to convert insoluble phosphorus, potassium, and silicon in the coal gangue into available phosphorus, readily available potassium, and available silicon that can be absorbed and utilized by plants. Simultaneously, the three extracellular polymers and cell structure of the SK1 bacterium passivate lead and chromium in the coal gangue, achieving passivation rates of 91% and 86%, respectively.
[0006] Chinese patent CN114588579 A discloses a method for passivating heavy metals in coal gangue. This method uses maifanite and zeolite as individual passivating agents, and also mixes maifanite and zeolite in a 1:1 mass ratio as a composite passivating agent. This method can significantly reduce the effective state of heavy metals in coal gangue, achieving a passivation rate of over 40% for Cd, Cu, Ni, and Pb. Furthermore, the heavy metal content in the leachate from the passivated coal gangue is lower than the requirements for heavy metal content in surface water, groundwater, and drinking water.
[0007] Chinese patent CN118305172A discloses a method for harmlessly removing heavy metals from coal gangue. The method involves drying, pulverizing, and sieving the coal gangue, then mixing it with one or more passivating agents selected from magnesium oxide, calcium oxide, iron oxide, calcium phosphate, calcite, kaolin, and superphosphate at a ratio of 200:1 to 1:2. The mixture is kept at a certain temperature and time, and the effective state of heavy metals in the coal gangue is reduced through vibration. Simultaneously, the coal gangue is mixed with one or more leaching agents selected from formic acid, acetic acid, propionic acid, citric acid, succinic acid, and disodium EDTA at a ratio of 200:1 to 1:200, and filtered after maintaining a certain rotation speed and time to further reduce the heavy metal content in the coal gangue.
[0008] Chinese patent CN112430171A discloses a method for preparing an acidic soil conditioner and improving acidified soil using coal gasification slag. The method involves grinding and sieving the gasification slag to 85-90 μm, adding calcium oxide, calcining at 800-900℃ for 0.8-1.2 hours, and then mixing the calcined product with organic matter at a mass ratio of 6:4 to prepare the conditioner. This conditioner can transform acidic soil into neutral soil, enabling large-scale crop production. Although the total heavy metal content in this conditioner meets the T / CCEMA 0001-2019 standard "Soil Water Retention and Conditioning Agents (Fly Ash Based)," it does not address the changes in available heavy metals in the gasification slag.
[0009] The above-mentioned technologies are effective in removing heavy metals from coal gangue and gasification slag, but they require large quantities of mineral materials and leaching agents, resulting in high energy consumption and high costs associated with microbial fermentation. Most of the improved technologies rely on the precipitation reaction of heavy metals, failing to fundamentally passivate them, and neglecting the release and utilization of organic nutrients in coal gangue and gasification slag.
[0010] To address the aforementioned problems, this invention provides a method for passivating heavy metals and releasing organic matter in coal gangue or gasification slag. This method passivates heavy metals in coal gangue or gasification slag within a hydrotalcite-like crystal lattice (K2). spThe passivating agent (with extremely low concentration) transforms heavy metals from a free state to a mineralized state, fundamentally passivating them and reducing their effective content. Simultaneously, the generated heavy metal-containing hydrotalcite-like substance disrupts the dissolution equilibrium of coal gangue or gasification slag, releasing organic matter from them. This invention uses a small amount of passivating agent, is low in cost, and provides stable passivation results, offering a feasible technical approach for the harmless and resource-based utilization of coal gangue or gasification slag. Summary of the Invention
[0011] The purpose of this invention is to address the shortcomings of existing heavy metal passivation technologies for coal gangue or gasification slag, and the lack of research on the release of organic matter from coal gangue or gasification slag, by providing a method for heavy metal passivation and organic matter release from coal gangue or gasification slag. This method involves mixing calcium oxide and ferric nitrate separately with coal gangue or gasification slag. The heavy metals in the coal gangue or gasification slag can react with calcium or ferric ions to generate a solubility product constant (K). sp The extremely low concentration of hydrotalcite transforms heavy metals from a free state into a mineralized state within the hydrotalcite lattice, making them difficult to release. Simultaneously, the process of hydrotalcite formation disrupts the dissolution process of coal gangue or gasification slag, causing the coal gangue or gasification slag to continuously dissolve and release organic nutrients that can be absorbed and utilized by plants.
[0012] To address the aforementioned technical problems, this invention provides a method for passivating heavy metals and releasing organic matter in coal gangue or gasification slag, comprising the following steps:
[0013] A. Air dry the coal gangue or gasification slag naturally, grind and crush it, and then pass it through a 2-3cm sieve.
[0014] B. Apply calcium oxide to the coal gangue or gasification slag treated in step A and mix it evenly. The amount of calcium oxide applied is 0.8–4.8 g per kilogram of coal gangue or gasification slag; the preferred amount is 2.24–4.16 g per kilogram of coal gangue or gasification slag. Its function is to provide divalent metal cations for the formation of hydrotalcite-like materials and at the same time to break the dissolution process of coal gangue or gasification slag.
[0015] C. Apply ferric nitrate to the coal gangue or gasification slag treated in step B and mix thoroughly. The application amount is 2.665–7.995 g per kilogram of coal gangue or gasification slag; the preferred application amount is 3.731–6.929 g per kilogram of coal gangue or gasification slag. Its function is to provide trivalent metal cations for the formation of hydrotalcite-like materials and at the same time to break the dissolution process of coal gangue or gasification slag.
[0016] D. The amount of water sprayed should be 50% of the mass of the coal gangue or gasification slag. Afterward, replenish the water weekly according to the substrate's dryness to the original moisture content. The treatment period should be at least three months.
[0017] Every month, a five-point sampling method was used to sample the passivated coal gangue or gasification slag. After natural air drying, the contents of effective heavy metals and water-soluble organic carbon in the coal gangue or gasification slag were determined. The observation was carried out for a total of 3 months.
[0018] The beneficial effects of this invention are as follows:
[0019] (1) The amount of passivating agent used is small, the cost is low, and the passivation technology is simple and easy to implement.
[0020] (2) Calcium oxide and ferric nitrate react with heavy metals in coal gangue or gasification slag to form hydrotalcite-like minerals, which passivate the heavy metals in situ within the hydrotalcite-like mineral lattice, transforming the heavy metals from a free state to a mineralized state. Hydrotalcite-like minerals have extremely low solubility product constants, making it difficult for heavy metals to be released again, thereby reducing the content of available heavy metals.
[0021] (3) The hydrotalcite generated during the passivation process can break the dissolution process of coal gangue or gasification slag, allowing the coal gangue or gasification slag to release the rich organic matter contained therein. Attached Figure Description
[0022] Figure 1 Curve of heavy metal biomass content in coal gangue as a function of time in Example 1
[0023] Figure 2 Curve of heavy metal biomass content in coal gangue over time in Example 2
[0024] Figure 3 Curve of heavy metal biomass content in coal gangue over time in Example 3
[0025] Figure 4 Curves showing the change in water-soluble organic carbon content in coal gangue of Examples 1–3 over time.
[0026] Figure 5 Curve of heavy metal content in gasification slag as a function of time in Example 4
[0027] Figure 6 The curve showing the change of water-soluble organic carbon content in the gasification residue of Example 4 over time. Detailed Implementation
[0028] Example 1
[0029] This invention is applicable to coal gangue or gasification slag with consistent chemical composition and content. Examples 1-4, the passivation effect and organic matter release effect are based on Uxin Banner Town, Ordos City, Inner Mongolia Autonomous Region, but are not limited to this; they are applicable to coal gangue or gasification slag with consistent chemical composition and content in the local area.
[0030] Table 1 shows the chemical composition and content of coal gangue or gasification slag from Wushen Banner Town, Ordos City, Inner Mongolia Autonomous Region. Locally stockpiled coal gangue or gasification slag was selected, and calcium oxide and ferric nitrate were purchased locally. The implementation took place in early May, and the specific steps are as follows:
[0031] A. Crush and pulverize large pieces of coal gangue until they can pass through a 2–3 cm sieve.
[0032] B. Apply calcium oxide at a rate of 0.8g per kilogram of coal gangue to the coal gangue treated in step A and mix thoroughly.
[0033] C. Add ferric nitrate at a rate of 2.665 g per kilogram of coal gangue to the coal gangue treated in step B, and mix thoroughly.
[0034] D. The spraying water volume is 50% of the mass of coal gangue or gasification slag. Water is then added weekly to the original moisture content based on the substrate's dryness. Every month, a five-point sampling method is used to sample the passivated coal gangue or gasification slag. After natural air drying, the content of available heavy metals and water-soluble organic carbon in the coal gangue or gasification slag is determined. This observation is conducted for a total of 3 months. Figure 1 and Figure 4 ).Depend on Figure 1 and Figure 4 It can be seen that the passivation rate of heavy metals in coal gangue is 61.4%–66.9%, and the release of water-soluble organic carbon is 45.7 mg / kg.
[0035] Table 1 Chemical composition and content of coal gangue and gasification slag
[0036]
[0037]
[0038] Example 2
[0039] A. Crush and pulverize large pieces of coal gangue until they can pass through a 2–3 cm sieve.
[0040] B. Apply calcium oxide at a rate of 3.2g per kilogram of coal gangue to the coal gangue treated in step A and mix thoroughly.
[0041] C. Add ferric nitrate at a rate of 5.33g per kilogram of coal gangue to the coal gangue treated in step B, and mix thoroughly.
[0042] D. The spraying water volume is 50% of the mass of coal gangue or gasification slag. Water is then added weekly to the original moisture content based on the substrate's dryness. Every month, a five-point sampling method is used to sample the passivated coal gangue or gasification slag. After natural air drying, the content of available heavy metals and water-soluble organic carbon in the coal gangue or gasification slag is determined. This observation is conducted for a total of 3 months. Figure 2 and Figure 4 ).Depend on Figure 2 and Figure 4 It can be seen that the passivation rate of heavy metals in coal gangue is 80.4%–86.3%, and the release of water-soluble organic carbon is 98.4 mg / kg.
[0043] Example 3
[0044] A. Crush and pulverize large pieces of coal gangue until they can pass through a 2–3 cm sieve.
[0045] B. Apply calcium oxide at a rate of 4.8g per kilogram of coal gangue to the coal gangue treated in step A and mix thoroughly.
[0046] C. Add 7.995g of ferric nitrate per kilogram of coal gangue to the coal gangue treated in step B and mix thoroughly.
[0047] D. The spraying water volume is 50% of the mass of coal gangue or gasification slag. Water is then added weekly to the original moisture content based on the substrate's dryness. Every month, a five-point sampling method is used to sample the passivated coal gangue or gasification slag. After natural air drying, the content of available heavy metals and water-soluble organic carbon in the coal gangue or gasification slag is determined. This observation is conducted for a total of 3 months. Figure 3 and Figure 4 ).Depend on Figure 3 and Figure 4 It can be seen that the passivation rate of heavy metals in coal gangue is 72.0%–76.7%, and the release of water-soluble organic carbon is 62.5 mg / kg.
[0048] Example 4
[0049] A. Grind and sieve the gasification slag until it can pass through a 2-3 cm sieve.
[0050] B. Add calcium oxide at a rate of 3.2g per kilogram of gasification slag to the gasification slag treated in step A and mix thoroughly.
[0051] C. Add ferric nitrate at a rate of 5.33 g per kilogram of gasification slag to the gasification slag treated in step B, and mix thoroughly.
[0052] D. The spraying water volume is 50% of the mass of coal gangue or gasification slag. Water is then added weekly to the original moisture content based on the substrate's dryness. Every month, a five-point sampling method is used to sample the passivated coal gangue or gasification slag. After natural air drying, the content of available heavy metals and water-soluble organic carbon in the coal gangue or gasification slag is determined. This observation is conducted for a total of 3 months. Figure 5 and Figure 6 ).Depend on Figure 5 and Figure 6 It can be seen that the passivation rate of heavy metals in the gasification residue is 80.8%–85.2%, and the release of water-soluble organic carbon is 55.52 mg / kg.
[0053] Verification of the improvement effect:
[0054] This invention samples unpassivated coal gangue or gasification slag from the local area after 3 months, and tests the content of available heavy metals and water-soluble organic carbon. The results are compared with those of the coal gangue or gasification slag from the four examples after 3 months of passivation. The results are shown in Tables 2, 3, 4, and 5. Tables 2 and 3 show that after 3 months, the content of available heavy metals in the coal gangue of Examples 1, 2, and 3 decreased significantly, lower than that of the unpassivated coal gangue, indicating that the heavy metals had been passivated in the hydrotalcite-like crystal lattice. Simultaneously, the content of water-soluble organic carbon was also higher than that of the unpassivated coal gangue, indicating that the addition of the passivating agent can release more organic nutrients from the coal gangue. Tables 4 and 5 show that after 3 months, the content of available heavy metals in the gasification slag of Example 4 was lower than that of the control example, while the content of water-soluble organic carbon increased significantly. This invention has a significant and stable passivation effect on heavy metals in coal gangue or gasification slag, while releasing organic nutrients, greatly maximizing the value of coal gangue or gasification slag, and has broad application prospects.
[0055] Table 2 shows the active heavy metal content of coal gangue in different embodiments during the third month.
[0056]
[0057] Table 3. Water-soluble organic carbon content of coal gangue in different examples during the third month.
[0058]
[0059] Table 4 shows the active heavy metal content of gasification slag in different embodiments during the third month.
[0060]
[0061] Table 5 shows the water-soluble organic carbon content of the gasification slag in different embodiments during the third month.
[0062]
Claims
1. A method for passivating heavy metals and releasing organic matter in coal gangue or gasification slag, characterized in that: Follow these steps: A. Crush and grind the coal gangue or gasification slag so that it can pass through a sieve with a pore size of 2-3 cm; B. Add calcium oxide at a rate of 0.8–4.8 g per kilogram of coal gangue or gasification slag to the coal gangue or gasification slag treated in step A, and mix thoroughly. C. Apply ferric nitrate at a rate of 2.665–7.995 g per kilogram of coal gangue or gasification slag to the coal gangue or gasification slag treated in step B, and mix thoroughly. Through the reaction of calcium oxide and ferric nitrate with the heavy metals in the coal gangue or gasification slag, a hydrotalcite-like substance is generated, which passivates the heavy metals in situ in the lattice of the hydrotalcite-like substance, transforming the heavy metals from a free state to a mineralized state. D. The amount of water sprayed should be 50% of the mass of coal gangue or gasification slag. Afterward, water should be added weekly according to the dryness of the substrate to restore the original moisture content. The treatment time should be at least three months.
2. The method for passivation of heavy metals and release of organic matter in coal gangue or gasification slag according to claim 1, characterized in that, The amount of calcium oxide applied in step B is 2.24–4.16 g per kilogram of coal gangue or gasification slag.
3. The method for passivation of heavy metals and release of organic matter in coal gangue or gasification slag according to claim 1, characterized in that, The amount of ferric nitrate applied in step C is 3.731–6.929 g per kilogram of coal gangue or gasification slag.
Citation Information
Patent Citations
Method for improving acidified soil by utilizing coal gasification slag and acidified soil conditioner
CN112430171A
Method for passivating metals in coal gangue with abnormal heavy metals by using solid passivator
CN114588579A
Method for passivating heavy metals and activating fertilizer by using microorganisms
CN116903421A
Method and apparatus for synthesizing hydrotalcite-like material by using coal gasification furnace residue as aluminum source
CN105236454A
Method for harmlessly treating heavy metals in coal gangue
CN118305172A