An apparatus, method for processing a composite honeycomb panel and a composite honeycomb panel made by the processing method

By connecting conductive components to the side electrical blocks of the honeycomb layer, uniform heating and high-pressure pressing of the honeycomb panel are achieved, solving the problems of heat loss and uneven heating in hot pressing equipment, improving adhesive stability and processing efficiency, and saving energy.

CN118952817BActive Publication Date: 2026-11-24GUANGZHOU ZHIHUI TECHNOLOGY INNOVATION CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411325709.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2026-11-24
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

Existing composite honeycomb panels suffer from severe heat loss and uneven heating during hot pressing, resulting in insufficient adhesive stability. Furthermore, hot pressing equipment is energy-intensive and has low processing efficiency.

Method used

The conductive components are connected to the aluminum honeycomb junction blocks on the side of the honeycomb layer. The conductive components transmit electrical energy to make the honeycomb layer heat up evenly. Combined with the pressing mechanism, high pressure is applied to achieve uniform heating and curing of the adhesive layer.

Benefits of technology

It improves the adhesive stability of composite honeycomb panels, extends their service life, saves energy and processing costs, and enhances processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118952817B_ABST
    Figure CN118952817B_ABST
Patent Text Reader

Abstract

This invention discloses an apparatus, method, and composite honeycomb panel processing method, relating to the field of building honeycomb panel processing technology. The apparatus includes a pressing mechanism and conductive components. The pressing mechanism has a pressing station for placing and pressing the composite honeycomb panel. The composite honeycomb panel has a honeycomb layer, a face material layer disposed on the surface of the honeycomb layer, and a base material layer disposed on the bottom surface of the honeycomb layer. An adhesive layer is disposed between the honeycomb layer and the face material layer and the base material layer. The conductive components are disposed on the sides of the honeycomb layer and connected to each aluminum honeycomb cell on the side of the honeycomb layer. The conductive components are electrically connected to a heating source and conduct electrical energy to the honeycomb layer, so that the honeycomb layer heats up uniformly and the heat is evenly conducted to the adhesive layer. This achieves the purpose of simultaneously energizing and heating the honeycomb layers of multiple sets of composite honeycomb panels and uniformly and fully heating the adhesive layer, saving more than 30% of energy consumption and processing costs. Furthermore, by pressing multiple sets of composite honeycomb panels using the pressing mechanism, the processing efficiency is increased by more than 80%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building honeycomb panel processing technology, and in particular to a device, a processing method, and a composite honeycomb panel prepared by the processing method. Background Technology

[0002] Composite honeycomb panels used in prefabricated buildings are mainly composed of face material and substrate firmly bonded to both sides of a relatively thick honeycomb core material. Fiberglass is also interspersed between the face material, substrate, and honeycomb core material. The honeycomb core material is usually aluminum foil, the face material is usually ceramic tile or marble, and the face material is applied to the outer surface. The substrate is usually gypsum board, which is connected to the wall. Therefore, based on its structural composition and characteristics, composite honeycomb panels are widely used in kitchens, bedrooms, and bathrooms.

[0003] In the prior art, composite honeycomb panels are usually formed by hot pressing equipment. The two metal plates of the hot pressing equipment are heated to a high temperature by an induction furnace, and then the surface material, the base material and the honeycomb core material of the composite honeycomb panel are pressed under high temperature and high pressure. At the same time, the polyurethane between the material layers of the composite honeycomb panel is heated at high temperature to cure the polyurethane and fix the pressed material layers together.

[0004] Although existing composite honeycomb panels can be formed by high temperature and high pressure processing using hot pressing equipment, the following drawbacks still exist:

[0005] 1. When existing composite honeycomb panels are processed under high temperature and pressure using two metal plates in a hot pressing device, a large portion of the heat is lost to the surface and substrate layers of the composite honeycomb panel because the two metal plates only contact the surface and substrate layers. This results in significant heat loss for the polyurethane used for heating. As the polyurethane fails to cure sufficiently and evenly, the adhesive strength between the various material layers of the composite honeycomb panel, such as the surface layer, honeycomb layer, and substrate layer, is insufficient, making the composite honeycomb panel prone to detachment after a certain period of use.

[0006] Moreover, since the two metal plates are quite thick, it is often necessary to increase the power of the induction furnace to heat the two metal plates at high temperatures, which results in greater energy consumption and increased hot pressing processing costs.

[0007] 2. Since each set of composite honeycomb panels is separated by a face material layer and a base material layer, when existing hot pressing equipment hot presses multiple sets of laminated composite honeycomb panels, the polyurethane of each set of composite honeycomb panels cannot be heated evenly and fully. Therefore, the hot pressing equipment can only hot press one set of composite honeycomb panels at a time, and its processing efficiency cannot meet the requirements. Summary of the Invention

[0008] In order to overcome the shortcomings of the prior art, one of the objectives of the present invention is to provide an apparatus for processing composite honeycomb panels.

[0009] One objective of this invention is achieved through the following technical solution: a device for processing composite honeycomb panels, comprising a pressing mechanism and a conductive component. The pressing mechanism has a pressing station for placing and pressing several sets of composite honeycomb panels. The composite honeycomb panel has a honeycomb layer, a face material layer disposed on the surface of the honeycomb layer, and a base material layer disposed on the bottom surface of the honeycomb layer. An adhesive layer is disposed between the honeycomb layer and the face material layer and the base material layer. The conductive component is disposed on one or both sides of the honeycomb layer. The conductive component is connected to each aluminum honeycomb cell on the side of the honeycomb layer. The conductive component is electrically connected to a heating source and transmits electrical energy to the honeycomb layer. The honeycomb layer is energized and heats up, and the heat is uniformly conducted to the adhesive layer, so that the adhesive layer is heated and cured, and the pressed composite honeycomb panel is firmly bonded.

[0010] Furthermore, each aluminum honeycomb on both sides of the honeycomb layer is integrally formed with an equipotential contact block, and the conductive element is connected to the contact block of each aluminum honeycomb on the side of the honeycomb layer.

[0011] Furthermore, the electrical contact block is provided with a buckle member facing the same direction, and one side of the conductive member is integrally formed with a groove. The conductive member is fixedly connected to the buckle member through the groove, thereby fixing the conductive member on one side of the honeycomb layer.

[0012] Furthermore, the conductive component has a clamp and several sliders movably disposed on the clamp. Each slider is provided with a spring rod. The clamp and the sliders are connected by a screw. By rotating the screw, the slider slides on the clamp and drives the spring rod and the clamping arm on the clamp to clamp the contact block on the aluminum honeycomb.

[0013] Furthermore, a glass fiber layer is disposed between the honeycomb layer and the face material layer and the substrate layer, and an adhesive layer is disposed between the glass fiber layer and the honeycomb layer, the face material layer and the substrate layer.

[0014] Furthermore, a metal mesh layer is provided between the honeycomb layer and the face material layer and the substrate layer, and an adhesive layer is provided between the metal mesh layer and the honeycomb layer, the face material layer and the substrate layer;

[0015] Alternatively, a metal mesh layer and a glass fiber layer may be provided between the honeycomb layer and the face material layer and the substrate layer, and an adhesive layer may be provided between the honeycomb layer and the metal mesh layer, the glass fiber layer, the face material layer and the substrate layer;

[0016] The metal mesh layer is connected to the conductive component, and the metal mesh layer and the honeycomb layer heat up synchronously or independently.

[0017] To overcome the shortcomings of the prior art, the second objective of this invention is to provide a method for processing composite honeycomb panels.

[0018] The second objective of this invention is achieved by the following technical solution: a method for processing composite honeycomb panels, comprising the following processing steps, using the aforementioned equipment for processing composite honeycomb panels:

[0019] S1. A face material layer and a base material layer are respectively provided on the surface and bottom surface of the honeycomb layer, and an adhesive layer is provided between the honeycomb layer and the face material layer and the base material layer to form a honeycomb blank.

[0020] S2. In step S1, conductive components are assembled on one or both sides of the honeycomb layer of the honeycomb blank.

[0021] S3. After assembling the conductive components in step S2, several sets of stacked honeycomb blanks are transported to the pressing station of the pressing mechanism. The conductive components are connected to a heating source, and electrical energy is transmitted to the honeycomb layer through the conductive components, so that the honeycomb layer is energized and heated, and the heat is evenly conducted to the adhesive layer. While heating the adhesive layer, the pressing mechanism is driven to press the several sets of honeycomb blanks under high pressure, so that the adhesive layer is heated and cured and the composite honeycomb panel is formed by adhesive pressing.

[0022] Furthermore, in step S2, each aluminum honeycomb on both sides of the honeycomb layer is integrally formed with an equipotential grounding block, and the conductive component is connected to the grounding block by a snap-fit ​​or clamping method.

[0023] Furthermore, in step S3, the heating temperature of the honeycomb layer is 50-100°C, and the adhesive layer is heated in the order of first heating, then maintaining a constant temperature, and finally cooling.

[0024] To overcome the shortcomings of the prior art, the third objective of this invention is to provide a composite honeycomb panel.

[0025] The third objective of this invention is achieved by the following technical solution: a composite honeycomb panel, which is processed by the aforementioned composite honeycomb panel processing equipment or by the aforementioned processing method.

[0026] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0027] (1) The equipment for processing composite honeycomb panels provided in this application embodiment has a pressing mechanism that sets up pressing stations for placing and pressing several sets of composite honeycomb panels, and connects conductive parts to each aluminum honeycomb on the side of the honeycomb layer. When the heating source is connected through the conductive parts and the electrical energy is transmitted to the honeycomb layer, the honeycomb layer can be energized and heated, and the heat can be evenly conducted to the adhesive layer, thereby causing the adhesive layer to be heated and cured, and the honeycomb layer, surface layer and base layer after being pressed by the pressing mechanism under high pressure are firmly bonded.

[0028] Compared to previous methods that relied solely on high-temperature, high-pressure pressing of two metal plates in a hot-pressing device for composite honeycomb panels, this embodiment eliminates the need for heating the two metal plates of the pressing mechanism using an induction furnace. This avoids the problems associated with heating the metal plates during hot pressing of the composite honeycomb panel, which involves high energy consumption and significant heat loss to the face and substrate layers, resulting in insufficient and uneven heating of the adhesive layer. By implementing this embodiment, the conductive components are electrically connected to the contact blocks of each aluminum honeycomb in the honeycomb layer. This allows the conductive components to uniformly transmit electrical energy to the honeycomb layer, resulting in uniform heating of the honeycomb layer and uniform heat conduction to the adhesive layer. This ensures uniform and sufficient heat curing of the adhesive layer, improving the adhesive stability between the face, honeycomb, and substrate layers of the composite honeycomb panel, extending the service life of the composite honeycomb panel, and saving more than 30% in energy consumption and processing costs.

[0029] Moreover, by transmitting electrical energy to the honeycomb layer through conductive components, and then heating the adhesive layer through the honeycomb layer, multiple sets of composite honeycomb panels can be heated simultaneously. Furthermore, multiple sets of composite honeycomb panels can be pressed into shape under high pressure by a pressing mechanism. Compared with the previous hot pressing equipment, which could only hot press one set of composite honeycomb panels at a time, the hot pressing processing efficiency is increased by more than 80%.

[0030] (2) By setting a grounding block on each aluminum honeycomb on both sides of the honeycomb layer, the conductive component is connected to the grounding block on each aluminum honeycomb. Therefore, the conductive component connects to the heating source and transmits electrical energy to each aluminum honeycomb in the honeycomb layer, so that each aluminum honeycomb on the side of the honeycomb layer can be connected at the same potential. By ensuring that the entire honeycomb layer is heated evenly, the adhesive layer sprayed between the interlayers can also be heated and cured evenly, further improving the pressing and adhesive effect of the composite honeycomb panel.

[0031] (3) By setting a buckle with the same orientation on the power contact block, the conductive component can be snapped onto the buckle of the power contact block from the upper or lower side or left or right side of the honeycomb layer through the buckle groove, thereby quickly and securely installing the conductive component on the side of the honeycomb layer. The operation is simple and convenient.

[0032] (4) In addition to installing the conductive component on the side of the composite honeycomb panel by snap-fit, a conductive component consisting of a clamp, a slider, and a spring rod can also be provided. The slider and the clamp are connected by a screw. By simply rotating the screw, the slider and the spring rod can slide to the clamp arm of the clamp and clamp the contact block on the aluminum honeycomb together with the clamp arm. This achieves the purpose of quickly and stably installing the conductive component on the side of the honeycomb layer. Moreover, by rotating the screw in the opposite direction, the spring rod and the clamp arm can be released from the contact block, making it easy to remove the conductive component from the side of the composite honeycomb panel. There is no need to set a snap-fit ​​component on the contact block. The clamping width between the spring rod and the clamp arm can be adjusted by rotating the screw, which is suitable for clamping contact blocks of aluminum honeycomb of different thicknesses. The operation is simple and convenient.

[0033] (5) By setting metal mesh layers between the honeycomb layer and the face material layer and the substrate layer, and connecting the metal mesh layer with the conductive component, the metal mesh layer can be heated; the conductive component can be independently connected to the metal mesh layer and the honeycomb layer or simultaneously connected to the metal mesh layer and the honeycomb layer, thereby realizing the switching between independent heating and synchronous heating of the metal mesh layer and the honeycomb layer; the metal mesh layer is independently heated, and since the specifications of the metal mesh layer are determined, its current and resistance are also determined, eliminating the tedious operation of adjusting the heating current. In addition, when the metal mesh layer and the honeycomb layer are heated synchronously, the heating effect and heating efficiency are higher, thereby meeting the user's diverse heating processing needs for composite honeycomb panels.

[0034] (6) The method for processing composite honeycomb panels provided in this application involves assembling conductive components on the side of a pre-assembled honeycomb blank and conveying several stacked honeycomb blanks after the conductive components are assembled to the pressing station of the pressing mechanism; then the conductive components are connected to a heating source and transmit electrical energy to the honeycomb layer, so that the honeycomb layer is energized and heated and the heat is evenly conducted to the adhesive layer. While the adhesive layer is fully heated, the pressing mechanism is driven to press and form the honeycomb blank.

[0035] This invention eliminates the cumbersome operation of heating two metal plates in a hot-pressing device, avoiding the problems of high energy consumption and significant heat loss associated with heating metal plates, as well as insufficient and uneven heating of the adhesive layer. By implementing the embodiments of this application, the honeycomb layer can be heated evenly and the heat can be evenly conducted to the adhesive layer, resulting in uniform and sufficient heating and curing of the adhesive layer. This improves the adhesive stability between the face material layer, honeycomb layer, and substrate layer of the composite honeycomb panel, extends the service life of the composite honeycomb panel, and saves more than 30% in energy consumption and processing costs.

[0036] Furthermore, by transmitting electrical energy to the honeycomb layer through conductive components, the method of heating the honeycomb layer and the adhesive layer is overcome, which previously only allowed for the hot pressing of one composite honeycomb panel at a time on the hot pressing equipment. In this embodiment, multiple composite honeycomb panels can be stacked and transported to the pressing station of the pressing mechanism, and multiple composite honeycomb panels can be heated and pressed under high pressure at the same time, which improves the hot pressing processing efficiency by more than 80% compared with the previous hot pressing equipment. Attached Figure Description

[0037] Figure 1 This is a schematic diagram of the composite honeycomb panel connected to a heating source via a conductive element on its side, as shown in the first embodiment of the present invention.

[0038] Figure 2 This is an exploded view of the honeycomb layer and snap-on conductive component structure of the composite honeycomb panel in the first embodiment of the present invention;

[0039] Figure 3 for Figure 2 Enlarged view of point A in the middle;

[0040] Figure 4 This is a side view of the conductive component of the composite honeycomb panel connection snap-fit ​​type in the first embodiment of the present invention;

[0041] Figure 5 for Figure 4 Enlarged view of point B in the middle;

[0042] Figure 6 This is a schematic diagram of the composite honeycomb panel being conveyed to the pressing station of the pressing mechanism in the first embodiment of the present invention;

[0043] Figure 7 This is a schematic diagram of a honeycomb layer connection clamping conductive component in the second embodiment of the present invention;

[0044] Figure 8 for Figure 7 Enlarged diagram of point C in the middle.

[0045] In the picture:

[0046] 10. Honeycomb layer; 101. Aluminum honeycomb; 102. Electrical connector; 1021. Fastener;

[0047] 20. Surface material layer;

[0048] 30. Substrate layer;

[0049] 40. Fiberglass layer;

[0050] 50. Metal mesh layer;

[0051] 60. Conductive component; 601. Slot; 602. Electrical connection slot; 603. Clamp; 6031. Clamping arm; 604. Slider; 605. Spring rod; 606. Screw;

[0052] 70. Pressing mechanism; 701. Metal sheet; 702. Pressing station;

[0053] r, heating source. Detailed Implementation

[0054] The present invention will now be further described in conjunction with the accompanying drawings and specific embodiments. It should be noted that, without conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.

[0055] First Embodiment

[0056] like Figure 1-6 As shown in the embodiment of this application, an equipment for processing composite honeycomb panels is provided. The composite honeycomb panels processed by the equipment are typically used in building spaces such as kitchens, bedrooms, and bathrooms for decorative purposes.

[0057] The equipment for processing composite honeycomb panels includes a pressing mechanism 70 and a conductive component 60. The pressing mechanism 70 has two metal plates 701, one above the other, which together form a pressing station 702 for placing and pressing several sets of composite honeycomb panels. The conductive component 60 is located on the side of the composite honeycomb panel and is electrically connected to a heating source. The conductive component 60 transmits electrical energy to the composite honeycomb panel, causing it to heat up.

[0058] More specifically, the composite honeycomb panel has a honeycomb layer 10, a face material layer 20 disposed on the surface of the honeycomb layer 10, and a substrate layer 30 disposed on the bottom surface of the honeycomb layer 10. Furthermore, a fiberglass layer 40 and a metal mesh layer 50 are disposed between the honeycomb layer 10 and the face material layer 20 and substrate layer 30, or both the metal mesh layer 50 and the fiberglass layer 40 are disposed simultaneously. An adhesive layer (not shown in the figure) is disposed between each layer of the honeycomb layer 10, face material layer 20, substrate layer 30, metal mesh layer 50, and fiberglass layer 40. The adhesive layer can be disposed by spraying, coating, or filling. Polyurethane is preferably used as the adhesive layer, but other adhesives besides polyurethane are not excluded; in this embodiment, polyurethane is preferred.

[0059] The honeycomb layer 10 consists of several arrayed aluminum honeycomb cells 101. The cells in each aluminum honeycomb cell 101 are hexagonal or cylindrical, ensuring that the resistance, power, and potential difference of each aluminum honeycomb cell 101 in each honeycomb layer 10 are uniform. The face material layer 20 is made of materials such as ceramic tiles or marble, serving as the surface layer of the composite honeycomb panel and exposed on the wall. The base material layer 30 is made of materials such as gypsum board, serving as the wall-facing side of the composite honeycomb panel.

[0060] The metal mesh layer 50 is preferably made of iron. In actual use, the specifications of each metal mesh layer 50 can be set, such as the area, thickness and mesh size of the metal mesh layer 50, so as to determine its current carrying capacity and heating effect.

[0061] Each aluminum honeycomb 101 on one or both sides of the honeycomb layer 10 is integrally formed with a grounding block 102, and the grounding blocks 102 on each aluminum honeycomb 101 are set at the same potential. The grounding blocks 102 are provided with a fastening member 1021, and the fastening members 1021 on the grounding blocks 102 on each aluminum honeycomb 101 are all set with the same orientation.

[0062] The conductive element 60 is disposed on the side of the honeycomb layer 10. The conductive element 60 is generally in the shape of a long strip plate and is arranged along the length of the side of the honeycomb layer 10. One side of the conductive element 60 is integrally formed with a slot 601 that matches the fastener 1021. The other side of the conductive element 60 is provided with a receiving groove 602, and is electrically connected to an external heating source r through the receiving groove 602. The heating source r refers to a voltage source or a current source.

[0063] The conductive element 60 is electrically connected to the heating source r, and the conductive element 60 transmits electrical energy to the honeycomb layer 10, causing the honeycomb layer 10 to be energized and heated. The heating current is selected between 1KA and 10KA, and the power is between 1KW and 10KW, which can also be adjusted according to actual usage requirements. Therefore, when the conductive element 60 is installed on the side of the honeycomb layer 10, the conductive element 60 can be snapped into contact with the electrical contact block 102 of each aluminum honeycomb 101 on the side of the honeycomb layer 10 through the slot 601.

[0064] Therefore, when the conductive component 60 is connected to the honeycomb layer 10 and energized for heating, each aluminum honeycomb 101 on the side of the honeycomb layer 10 can be equipotentially connected, ensuring that the entire honeycomb layer 10, especially the honeycomb layer 10 and the polyurethane layer, is heated evenly. This allows the polyurethane layer sprayed between the interlayers to be heated and cured evenly, and removes the CO2 gas inside the polyurethane layer as cleanly as possible, further improving the pressing and bonding effect of the composite honeycomb panel.

[0065] During the pressing process of composite honeycomb panels, multiple sets of composite honeycomb panels can be stacked and transported together to the pressing station 702 of the pressing mechanism 70. The conductive parts 60 assembled on each set of composite honeycomb panels are electrically connected through a heating source r, and multiple sets of composite honeycomb panels are heated at the same time, thereby achieving the purpose of heating and pressing multiple sets of composite honeycomb panels simultaneously.

[0066] The specific installation method of the conductive component 60 is as follows: the buckle 1021 of each electrical block 102 is set towards the side length direction of the honeycomb layer 10, and the slot 601 of the conductive component 60 is opened along the length direction of the conductive component 60, and the slot opening of the slot 601 is set at the left and right ends of the conductive component 60; at this time, the conductive component 60 can be snapped onto the buckle 1021 in the left or right direction through the slot 601, thereby installing the conductive component 60 on the side of the honeycomb layer 10.

[0067] Alternatively, the latching member 1021 of each electrical contact block 102 is arranged in the direction of the face material layer 20 or the base material layer 30, and the slot 601 of the conductive member 60 is arranged perpendicular to the length direction of the conductive member 60, and the slot opening of the slot 601 is located on the upper or lower side of the conductive member 60; in this case, the conductive member 60 can be latched onto the fastener in the upward or downward direction, and then the conductive member 60 can be installed on the side of the honeycomb layer 10.

[0068] Therefore, by setting a snap fastener 1021 with the same orientation on the grounding block 102, the conductive element 60 can be snapped onto the snap fastener 1021 of the grounding block 102 from a certain direction, either from the upper or lower side or the left or right side of the honeycomb layer 10, through the snap slot 601, thereby quickly and securely installing the conductive element 60 on the side of the honeycomb layer 10, which is simple and convenient to operate.

[0069] In practical use, the conductive element 60 can be connected to the honeycomb layer 10 and the metal mesh layer 50, or connected to both the honeycomb layer and the metal mesh layer 50 simultaneously. The current is supplied to the conductive element 60 through the heating source r, and then the conductive element 60 transmits electrical energy to the honeycomb layer 10 and the metal mesh layer 50. Therefore, it is possible to choose to heat only the honeycomb layer 10 or the metal mesh layer 50, or heat both the honeycomb layer 10 and the metal mesh layer 50 simultaneously, thereby achieving the switching between synchronous heating of the metal mesh layer 50 and the honeycomb layer 10 or independent heating, and independent heating of the metal mesh layer 50.

[0070] Since the specifications of the metal mesh layer 50 are fixed, its current and resistance are also fixed, eliminating the cumbersome operation of adjusting the heating current for different specifications of the honeycomb layer 10. In addition, when the metal mesh layer 50 and the honeycomb layer 10 are heated simultaneously, the heating effect and heating efficiency are higher, thus meeting the user's diverse heating processing needs for composite honeycomb panels.

[0071] Thus, through the above optimization and improvement of the equipment for processing composite honeycomb panels, the embodiments of this application, compared with the previous implementation method of processing composite honeycomb panels by only using two metal plates 701 of a hot pressing equipment for high-temperature and high-pressure pressing, do not require heating the two metal plates 701 of the pressing mechanism 70 through an induction furnace. This eliminates the problem of high energy consumption in heating the metal plates when hot pressing the composite honeycomb panel by heating the two metal plates 701, and the problem of most of the heat being lost to the face material layer 20 and the substrate layer 30, resulting in insufficient and uneven heating of the polyurethane layer.

[0072] By implementing the embodiments of this application, the conductive element 60 is electrically connected to the contact block 102 of each aluminum honeycomb 101 of the honeycomb layer 10, so that the conductive element 60 uniformly transmits electrical energy to the honeycomb layer 10, the honeycomb layer 10 heats up uniformly and conducts the heat to the polyurethane layer uniformly, so that the polyurethane layer is uniformly and fully heated and cured, improving the adhesive stability between the surface layer 20, the honeycomb layer 10 and the substrate layer 30 of the composite honeycomb panel, extending the service life of the composite honeycomb panel, and saving more than 30% of energy consumption and processing costs.

[0073] Furthermore, by transmitting electrical energy to the honeycomb layer 10 through the conductive component 60, and heating the polyurethane layer through the honeycomb layer 10, multiple sets of composite honeycomb panels can be heated simultaneously. Moreover, the pressing mechanism 70 can press multiple sets of composite honeycomb panels under high pressure, which improves the hot pressing processing efficiency by more than 80% compared to the previous hot pressing equipment that could only hot press one set of composite honeycomb panels at a time.

[0074] The method for processing composite honeycomb panels provided in this application embodiment uses the aforementioned equipment for processing composite honeycomb panels to process the composite honeycomb panels, and includes the following processing steps:

[0075] S1. A face material layer 20 and a base material layer 30 are respectively provided on the surface and bottom surface of the honeycomb layer 10, and a polyurethane layer is provided between the honeycomb layer 10 and the face material layer 20 and the base material layer 30, thereby forming a honeycomb blank.

[0076] S2. In step S1, conductive components 60 are assembled on one or both sides of the honeycomb layer 10 of the honeycomb blank plate.

[0077] S3. After assembling the conductive component 60 in step S2, several sets of honeycomb blanks are transported to the pressing station 702 of the pressing mechanism 70. The conductive component 60 is connected to the heating source r, and electrical energy is transmitted to the honeycomb layer 10 through the conductive component 60, so that the honeycomb layer 10 is energized and heated, and the heat is evenly conducted to the polyurethane layer. While heating the polyurethane layer, the pressing mechanism 70 is driven to press the several sets of honeycomb blanks under high pressure, so that the polyurethane layer is heated, cured, and glued to form a composite honeycomb panel.

[0078] Preferably, in step S1, a metal mesh layer 50 is disposed between the honeycomb layer 10 and the face material layer 20 and the substrate layer 30, and a polyurethane layer is disposed between the metal mesh layer 50 and the honeycomb layer 10, the face material layer 20, and the substrate layer 30. Alternatively, a metal mesh layer 50 and a glass fiber layer 40 are disposed correspondingly between the honeycomb layer 10 and the face material layer 20 and the substrate layer 30, and a polyurethane layer is disposed between the honeycomb layer 10 and the metal mesh layer 50, the glass fiber layer 40, the face material layer 20, and the substrate layer 30.

[0079] The metal mesh layer 50 is connected to the conductive element 60, so when the conductive element 60 is energized, the conductive element 60 transmits electrical energy to the metal mesh layer 50 or the honeycomb layer 10. The metal mesh layer 50 or the honeycomb layer 10 can be heated, or both the metal mesh layer 50 and the honeycomb layer 10 can be heated simultaneously.

[0080] Preferably, in step S2, each aluminum honeycomb 101 on both sides of the honeycomb layer 10 is integrally formed with an equipotential contact block 102, and the conductive component 60 is connected to the contact block 102 by a snap-fit ​​or clamping method.

[0081] Preferably, the heating temperature of the honeycomb layer 10 in step S3 is 50-100℃. When the heating temperature is adjusted to 60-70℃, the curing time of the polyurethane layer is 60 minutes; when the heating temperature is adjusted to 80℃, the curing time of the polyurethane layer is 15-25 minutes. When other adhesives are selected, the heating temperature can be increased to accelerate the curing time of the adhesive. The honeycomb layer 10 is heated in the following sequence: first, heating up; then, maintaining a constant temperature; and finally, cooling down. For example, the first 1 / 5 of the curing time of the polyurethane layer is controlled by gradually increasing the temperature to the maximum curing temperature, then 3 / 5 of the curing time is controlled at the maximum curing temperature, and finally, the temperature is gradually reduced to room temperature and heating is stopped in the last 1 / 5 of the time. This allows the CO2 gas inside the polyurethane layer to be removed as much as possible, thereby achieving the best processing efficiency of the composite honeycomb panel.

[0082] Thus, through the above optimization and improvement of the method for processing composite honeycomb panels, the embodiments of this application save the cumbersome operation of heating two metal plates 701 in the previous hot pressing equipment, and eliminate the problems of high energy consumption and serious heat loss when heating the metal plates 701, as well as insufficient and uneven heating of the polyurethane layer.

[0083] By implementing the embodiments of this application, the honeycomb layer 10 can be heated uniformly and the heat can be uniformly conducted to the polyurethane layer, so that the polyurethane layer is heated and cured uniformly and fully, thereby improving the adhesive stability between the face material layer 20, the honeycomb layer 10 and the substrate layer 30 of the composite honeycomb panel, extending the service life of the composite honeycomb panel, and saving more than 30% of energy consumption and processing costs.

[0084] Furthermore, by transmitting electrical energy to the honeycomb layer 10 through the conductive component 60, the method of heating the honeycomb layer 10 and the polyurethane layer is overcome by overcoming the previous problem that only one set of composite honeycomb panels could be hot-pressed at a time on the hot pressing equipment. In this embodiment, multiple sets of composite honeycomb panels can be stacked and transported to the pressing station 702 of the pressing mechanism 70, and multiple sets of composite honeycomb panels can be heated and high-pressure pressed at the same time. Compared with the previous hot pressing equipment, the hot pressing processing efficiency is improved by more than 80%.

[0085] Second Embodiment

[0086] The difference between this embodiment and the first embodiment is that the structure of the conductive element 60 is different, the contact block 102 of the aluminum honeycomb 101 does not have a snap-fit ​​element 1021, and the connection method between the conductive element 60 and the contact block 102 is different. The rest are the same and will not be described again here.

[0087] like Figure 7-8 As shown, several conductive elements 60 are provided on the side of the honeycomb layer 10, and each aluminum honeycomb 101 on the side of the honeycomb layer 10 is connected to a conductive element 60.

[0088] More specifically, the conductive component 60 provided in this embodiment of the application includes a clamping base 603, a slider 604, and a spring rod 605. The clamping base 603 has a clamping arm 6031, and a groove is provided on the clamping base 603 on the same side as the clamping arm 6031. The slider 604 is movably disposed on the groove of the clamping base 603. A plurality of sliders 604 are connected to the clamping arm 6031 of the clamping base 603 by screws 606. The spring rod 605 passes through the slider 604 and extends along the direction of the groove of the clamping base 603.

[0089] Therefore, the movement of slider 604 can be achieved by rotating screw 606, direct drive of cylinder, etc. When screw 606 is rotated, spring rods 605 on several sliders 604 can slide along slider 604 on the groove of clamp 603. As one end of spring rod 605 gradually approaches clamp arm 6031 of clamp 603, spring rod 605 and clamp arm 6031 can clamp the electrical block 102 on aluminum honeycomb 101 together, thereby detachably assembling the entire conductive component 60 and electrical block 102.

[0090] Furthermore, by controlling the spring rods 605 on several sliders 604 simultaneously through the same screw 606, the conductive component and the electrical contact block 102 of each aluminum honeycomb 101 can be synchronously clamped, thereby improving the ease of operation.

[0091] Therefore, the conductive component 60 provided in this application can slide the slider 604 and the spring rod 605 to one side of the clamping arm 6031 of the clamping seat 603 by simply rotating the screw 606, and clamp the grounding block 102 on the aluminum honeycomb 101 together with the clamping arm 6031, thus achieving the purpose of quickly and stably installing the conductive component 60 on the side of the honeycomb layer 10.

[0092] Furthermore, by rotating the screw 606 in the opposite direction, the spring rod 605 and the clamping arm 6031 can be released from the contact block 102, making it easy to remove the conductive component 60 from the side of the composite honeycomb panel. It also eliminates the need to install the buckle 1021 on the contact block 102. Moreover, by rotating the screw 606, the clamping width between the spring rod 605 and the clamping arm 6031 can be adjusted, making it suitable for clamping contact blocks 102 with different thicknesses of aluminum honeycomb 101. The operation is simple and convenient.

[0093] The above embodiments are merely preferred embodiments of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-substantial changes and substitutions made by those skilled in the art based on the present invention shall fall within the scope of protection claimed by the present invention.

Claims

1. A device for processing composite honeycomb panels, characterized in that, The device includes a pressing mechanism and conductive components. The pressing mechanism has a pressing station for placing and pressing several sets of composite honeycomb panels. The composite honeycomb panel has a honeycomb layer, a face material layer disposed on the surface of the honeycomb layer, and a base material layer disposed on the bottom surface of the honeycomb layer. An adhesive layer is disposed between the honeycomb layer and the face material layer and the base material layer. The conductive components are disposed on one or both sides of the honeycomb layer. The conductive components are connected to each aluminum honeycomb on the side of the honeycomb layer. The conductive components are electrically connected to a heating source and transmit electrical energy to the honeycomb layer. The honeycomb layer is energized and heats up, and the heat is evenly conducted to the adhesive layer, so that the adhesive layer is heated and cured and adheres the pressed composite honeycomb panel. Each aluminum honeycomb on both sides of the honeycomb layer is integrally formed with an equipotential grounding block, and the conductive component is connected to the grounding block of each aluminum honeycomb on the side of the honeycomb layer. During the pressing process of composite honeycomb panels, multiple sets of composite honeycomb panels can be stacked and transported together to the pressing station of the pressing mechanism. The conductive components assembled on each set of composite honeycomb panels are electrically connected through a heating source, and multiple sets of composite honeycomb panels are heated and pressed at the same time.

2. The equipment for processing composite honeycomb panels as described in claim 1, characterized in that, The electrical contact block is provided with snap fasteners facing the same direction. One side of the conductive component is integrally formed with a slot. The conductive component is snapped and fixedly connected to the snap fastener through the slot, thereby fixing the conductive component to one side of the honeycomb layer.

3. The equipment for processing composite honeycomb panels as described in claim 1, characterized in that, The conductive component has a clamp and several sliders movably disposed on the clamp. Each slider is provided with a spring rod. The clamp and the sliders are connected by a screw. By rotating the screw, the slider slides on the clamp and drives the spring rod and the clamp arm on the clamp to clamp the contact block on the aluminum honeycomb.

4. The equipment for processing composite honeycomb panels as described in any one of claims 1-3, characterized in that, A glass fiber layer is disposed between the honeycomb layer and the face material layer and the substrate layer, and an adhesive layer is disposed between the glass fiber layer and the honeycomb layer, the face material layer and the substrate layer.

5. The equipment for processing composite honeycomb panels as described in any one of claims 1-3, characterized in that, A metal mesh layer is provided between the honeycomb layer and the face material layer and the substrate layer, and an adhesive layer is provided between the metal mesh layer and the honeycomb layer, the face material layer and the substrate layer. Alternatively, a metal mesh layer and a glass fiber layer may be provided between the honeycomb layer and the face material layer and the substrate layer, and an adhesive layer may be provided between the honeycomb layer and the metal mesh layer, the glass fiber layer, the face material layer and the substrate layer; The metal mesh layer is connected to the conductive component, and the metal mesh layer and the honeycomb layer heat up synchronously or independently.

6. A method for processing composite honeycomb panels, comprising processing the composite honeycomb panels using the equipment described in any one of claims 1-5, characterized in that, The processing steps include the following: S1. A face material layer and a base material layer are respectively provided on the surface and bottom surface of the honeycomb layer, and an adhesive layer is provided between the honeycomb layer and the face material layer and the base material layer to form a honeycomb blank. S2. In step S1, conductive components are assembled on one or both sides of the honeycomb layer of the honeycomb blank. S3. After assembling the conductive components in step S2, several sets of stacked honeycomb blanks are transported to the pressing station of the pressing mechanism. The conductive components are connected to a heating source, and electrical energy is transmitted to the honeycomb layer through the conductive components, so that the honeycomb layer is energized and heated, and the heat is evenly conducted to the adhesive layer. While heating the adhesive layer, the pressing mechanism is driven to press the several sets of honeycomb blanks under high pressure, so that the adhesive layer is heated, cured, and pressed into shape.

7. The method for processing composite honeycomb panels as described in claim 6, characterized in that, In step S2, each aluminum honeycomb on both sides of the honeycomb layer is integrally formed with an equipotential grounding block, and the conductive component is connected to the grounding block by a snap-fit ​​or clamping method.

8. The method for processing composite honeycomb panels as described in claim 6, characterized in that, In step S3, the heating temperature of the honeycomb layer is 50-100℃, and the adhesive layer is heated in the order of first heating up, then maintaining a constant temperature, and finally cooling down.

9. A composite honeycomb panel, processed by the composite honeycomb panel processing equipment according to any one of claims 1-5, or processed by the processing method according to any one of claims 6-8.

Citation Information

Patent Citations

  • Heat curing of thermosetting plastic film adhesives

    GB1087855A