Preparation method of heteroatom-doped silicon-carbon composite material and application thereof

By preparing heteroatom-doped silicon-carbon composite materials, the problems of high expansion rate and poor rate performance of silicon-carbon composite materials were solved, and the structural stability and conductivity of the materials were improved, thereby enhancing the performance of the battery.

CN118954481BActive Publication Date: 2026-11-24SICHUAN KUNTIAN NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411160957.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2026-11-24
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

Existing silicon-carbon composite materials have high expansion rates and poor rate performance, and their electronic conductivity and ionic conductivity have not been effectively improved.

Method used

Heteroatom-doped porous magnesium oxide was prepared using basic magnesium carbonate, heteroatom solution, and catalyst. Heteroatom-doped silicon-carbon composite material was formed through multiple gas deposition processes, which improved the structural stability and conductivity of the material.

Benefits of technology

It reduces the material's expansion rate, improves electronic conductivity and rate performance, and enhances initial efficiency and cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954481B_ABST
    Figure CN118954481B_ABST
Patent Text Reader

Abstract

The application relates to the technical field of lithium ion battery materials, and discloses a preparation method of a heteroatom-doped silicon-carbon composite material and application thereof, the preparation method of the heteroatom-doped silicon-carbon composite material comprising the following steps: S1, adding basic magnesium carbonate and a catalyst into a heteroatom solution, uniformly dispersing, spray drying, sintering, and obtaining a heteroatom-doped porous magnesium oxide; S2, passing in silane gas for first-time deposition, passing in a heteroatom mixed gas for second-time deposition, passing in halosilane gas for third-time deposition, passing in an oxidizing gas for fourth-time deposition, passing in a first carbon source gas for fifth-time deposition, and obtaining the heteroatom-doped silicon-carbon composite material. Through the technical scheme, the problems of high expansion rate and poor rate performance of the silicon-carbon composite material in the related art are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery materials technology, specifically to a method for preparing heteroatom-doped silicon-carbon composite materials and their applications. Background Technology

[0002] Currently, silicon-carbon composites mainly consist of porous carbon and nano-silicon deposited within its pores as the core, with amorphous carbon as the outer shell. Since the outer shell is composed of a single amorphous carbon coating layer, its ability to constrain the expansion of the nano-silicon core is limited. Furthermore, the outer shell's reliance solely on an amorphous carbon layer reduces the material's electronic conductivity, failing to improve its ionic conductivity, which severely hinders the rate performance enhancement of silicon-carbon composites. Therefore, to reduce the expansion of silicon-carbon composites and improve their rate performance, it is urgent to develop a novel method for preparing silicon-carbon composites. Summary of the Invention

[0003] This invention proposes a method for preparing heteroatom-doped silicon-carbon composite materials and their application, which solves the problems of high expansion rate and poor rate performance of silicon-carbon composite materials in related technologies.

[0004] The technical solution of the present invention is as follows: This invention proposes a method for preparing heteroatom-doped silicon-carbon composite materials, comprising the following steps: S1. Add basic magnesium carbonate and catalyst to the heteroatom solution, disperse evenly, spray dry, and sinter to obtain heteroatom-doped porous magnesium oxide; S2. Silane gas is introduced into the heteroatom-doped porous magnesium oxide for the first deposition, followed by the introduction of a heteroatom mixed gas, the second deposition, the introduction of halosilane gas, the third deposition, the introduction of an oxidizing gas, the fourth deposition, the introduction of a first carbon source gas, and the fifth deposition to obtain a heteroatom-doped silicon-carbon composite material.

[0005] As a further technical solution, in step S1, the mass ratio of the basic magnesium carbonate, heteroatom solution, and catalyst is 100:100~500:1~5.

[0006] As a further technical solution, the heteroatom solution is one of urea solution, melamine solution, hydrazine hydrate solution, boric acid solution, and phosphoric acid solution.

[0007] As a further technical solution, the mass fraction of the heteroatom solution is 1% to 10%.

[0008] As a further technical solution, the catalyst is one of bismuth isooctanoate, bismuth laurate, and bismuth neodecanoate.

[0009] As a further technical solution, in step S1, the sintering temperature is 600~1000℃ and the time is 1~3h.

[0010] As a further technical solution, in step S2, the silane gas is one of trichlorosilane, ethoxysilane, and dimethylsilane.

[0011] As a further technical solution, when introducing silane gas, the introduction rate is 50~200mL / min.

[0012] As a further technical solution, in step S2, the heteroatom mixed gas is a mixture of heteroatom gas and a second carbon source gas.

[0013] As a further technical solution, the heteroatom gas is one of ammonia, phosphine, hydrogen sulfide, and sulfur dioxide.

[0014] As a further technical solution, the second carbon source gas is one of methane, acetylene, and ethylene.

[0015] As a further technical solution, the volume ratio of the heteroatom gas to the second carbon source gas is 10:1~5.

[0016] As a further technical solution, when introducing the heteroatom mixed gas, the introduction rate is 50~200mL / min.

[0017] As a further technical solution, in step S2, the halosilane gas is one of tetrafluorosilane, trichlorofluorosilane, tetrachlorosilane, and hexafluorodisilane.

[0018] As a further technical solution, when introducing halosilane gas, the introduction rate is 50~200mL / min.

[0019] As a further technical solution, in step S2, the oxidizing gas is one of nitrous oxide, hydrogen peroxide, oxygen, ozone, nitric oxide, and nitrogen dioxide.

[0020] As a further technical solution, when introducing the oxidizing gas, the introduction rate is 50~200mL / min.

[0021] As a further technical solution, in step S2, the first carbon source gas is one of methane, acetylene, and ethylene.

[0022] As a further technical solution, when the first carbon source gas is introduced, the introduction rate is 100~200mL / min.

[0023] As a further technical solution, in step S2, the temperature during the first deposition is 450~650℃, and the time is 30~300min; and / or The second deposition is performed at a temperature of 600–900°C for a time of 10–60 min; and / or The third deposition was performed at a temperature of 500–800°C for 30–120 minutes; and / or The fourth deposition was performed at a temperature of 200-300°C for 30-300 minutes; and / or The fifth deposition was carried out at a temperature of 600-900℃ for 30-300 minutes.

[0024] The present invention also proposes the application of the heteroatom-doped silicon-carbon composite material prepared by the above-described method in lithium-ion battery materials.

[0025] The working principle and beneficial effects of this invention are as follows: 1. In this invention, heteroatom-doped porous magnesium oxide is prepared by sintering basic magnesium carbonate, heteroatom solution and catalyst. The heteroatom is used to improve the conductivity of porous magnesium oxide, and the catalyst is used to form a macroporous structure to facilitate the subsequent deposition of nano-silicon. At the same time, the porous magnesium oxide and nano-silicon form magnesium silicate to improve the structural stability of silicon-carbon composite material, reduce the expansion rate, and improve rate performance and first-pass efficiency.

[0026] 2. In this invention, nano-silicon, heteroatom materials, halogen-doped silicon oxide, and amorphous carbon are sequentially deposited in the pores and surface of porous magnesium oxide. The heteroatoms enhance the electronic conductivity of the silicon-carbon composite material; the halogen-doped silicon oxide reduces the expansion rate, improves rate performance and first-cycle efficiency; and the amorphous carbon isolates the core of the silicon-carbon composite material from the electrolyte, improving first-cycle efficiency and storage performance, and reducing gas production. As a result, the prepared heteroatom-doped silicon-carbon composite material has the advantages of good rate performance, low expansion rate, good cycle performance, and high first-cycle efficiency. Attached Figure Description

[0027] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.

[0028] Figure 1 The image shows a SEM image of the heteroatom-doped silicon-carbon composite material prepared in Example 1. Detailed Implementation

[0029] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0030] Example 1 A method for preparing heteroatom-doped silicon-carbon composite material includes the following steps: S1. Add 100g of basic magnesium carbonate and 3g of bismuth isooctanoate to 300g of urea solution with a mass fraction of 5%, disperse evenly, spray dry, and sinter at 850℃ for 2h to obtain heteroatom-doped porous magnesium oxide. S2. Add heteroatom-doped porous magnesium oxide to a fluidized bed. First, nitrogen gas is introduced to purge the air in the tube. Then, silane is introduced at a flow rate of 100 mL / min. After deposition at 550 °C for 120 min, a mixture of ammonia and methane (volume ratio of ammonia to methane is 10:3) is introduced at a flow rate of 100 mL / min. After deposition at 750 °C for 30 min, tetrafluorosilane is introduced at a flow rate of 100 mL / min. After deposition at 650 °C for 120 min, oxygen is introduced at a flow rate of 100 mL / min. After deposition at 250 °C for 120 min, methane is introduced at a flow rate of 100 mL / min. After deposition at 800 °C for 120 min, heteroatom-doped silicon-carbon composite material is obtained. The SEM images of the heteroatom-doped silicon-carbon composite material are shown below. Figure 1 As shown, by Figure 1 It can be seen that the heteroatom-doped silicon-carbon composite material exhibits a granular structure with a uniform size distribution and an average particle size of 7.5 μm.

[0031] Example 2 A method for preparing heteroatom-doped silicon-carbon composite material includes the following steps: S1. Add 100g of basic magnesium carbonate and 1g of bismuth laurate to 100g of 5% melamine solution, disperse evenly, spray dry, and sinter at 600℃ for 3h to obtain heteroatom-doped porous magnesium oxide. S2. Heteroatom-doped porous magnesium oxide was added to a fluidized bed. First, nitrogen gas was introduced to purge the air from the tube. Then, silane was introduced at a flow rate of 50 mL / min. After deposition at 450 °C for 300 min, a phosphine / acetylene mixture (phosphine to acetylene volume ratio of 10:1) was introduced at a flow rate of 50 mL / min. After deposition at 600 °C for 60 min, trichlorofluorosilane was introduced at a flow rate of 50 mL / min. After deposition at 500 °C for 60 min, nitric oxide was introduced at a flow rate of 50 mL / min. After deposition at 200 °C for 300 min, acetylene was introduced at a flow rate of 200 mL / min. After deposition at 600 °C for 300 min, a heteroatom-doped silicon-carbon composite material was obtained.

[0032] Example 3 A method for preparing heteroatom-doped silicon-carbon composite material includes the following steps: S1. Add 100g of basic magnesium carbonate and 5g of bismuth neodecanoate to 500g of 1% hydrazine hydrate solution, disperse evenly, spray dry, and sinter at 1000℃ for 1h to obtain heteroatom-doped porous magnesium oxide. S2. Heteroatom-doped porous magnesium oxide was added to a fluidized bed. First, nitrogen gas was introduced to purge the air in the tube. Then, silane was introduced at a flow rate of 200 mL / min. After deposition at 650 °C for 30 min, a hydrogen sulfide / ethylene mixture (volume ratio of hydrogen sulfide to ethylene is 10:5) was introduced at a flow rate of 200 mL / min. After deposition at 900 °C for 10 min, tetrachlorosilane was introduced at a flow rate of 200 mL / min. After deposition at 800 °C for 30 min, nitrogen dioxide was introduced at a flow rate of 200 mL / min. After deposition at 300 °C for 30 min, acetylene was introduced at a flow rate of 200 mL / min. After deposition at 900 °C for 30 min, a heteroatom-doped silicon-carbon composite material was obtained.

[0033] Comparative Example 1 The only difference between this comparative example and Example 1 is that, in this comparative example, heteroatom-doped porous magnesium oxide was not prepared, and the heteroatom-doped porous magnesium oxide was replaced with an equal amount of porous carbon.

[0034] Comparative Example 2 A method for preparing heteroatom-doped silicon-carbon composite material includes the following steps: S1. Add 100g of basic magnesium carbonate and 3g of bismuth isooctanoate to 300g of urea solution with a mass fraction of 5%, disperse evenly, spray dry, and sinter at 850℃ for 2h to obtain heteroatom-doped porous magnesium oxide. S2. Add heteroatom-doped porous magnesium oxide to a fluidized bed, introduce silane at a flow rate of 100 mL / min, and deposit at 550 °C for 120 min. Then, introduce ammonia / methane mixed gas (ammonia to methane volume ratio of 10:3) at a flow rate of 100 mL / min and deposit at 750 °C for 30 min to obtain heteroatom-doped silicon-carbon composite material.

[0035] Comparative Example 3 The only difference between this comparative example and Example 1 is that in step S2 of this comparative example, tetrafluorosilane was not introduced at a rate of 100 mL / min and deposited at 650°C for 120 min.

[0036] Experiment Example 1: Physicochemical Property Testing The specific surface area and tap density of the heteroatom-doped silicon-carbon composite materials prepared in Examples 1-3 and Comparative Examples 1-3 were tested according to the methods in GB / T 38823-2020 "Silicon-Carbon". The powder resistivity was tested using a powder resistivity tester (model ST2742B). The test results are shown in Table 1 below.

[0037] Table 1. Results of Physicochemical Properties Tests

[0038] Experiment Example 2: Button Battery Test The heteroatom-doped silicon-carbon composite materials prepared in Examples 1-3 and Comparative Examples 1-3 were used to prepare coin cells according to the following method: Each heteroatom-doped silicon-carbon composite material was used as the negative electrode material. LA132 binder, SP conductive agent, and NMP solvent were added respectively (heteroatom-doped silicon-carbon composite material:SP conductive agent:LA132 binder:NMP solvent = 95g:1g:4g:220mL). After stirring and slurry preparation, the mixture was coated onto copper foil, dried, and rolled to obtain the negative electrode sheets for each battery. The negative electrode sheets, along with the counter electrode (lithium metal sheet), electrolyte (1 mol / L LiPF6 solution, the solvent consisting of ethylene carbonate and diethyl carbonate in a 1:1 volume ratio), and separator (polypropylene membrane), were assembled into coin cells in an argon-filled glove box. The performance of the coin cells was tested using a Wuhan Landian Battery Tester (model CT2001A) as follows: ① Initial discharge specific capacity and initial efficiency: The test conditions were a charge / discharge voltage of 0.005V~2.0V and a charge / discharge rate of 0.1C; ② Rate performance: Test conditions are 1C / 0.1C; ③ Full charge expansion rate: Test the active material thickness D1 of the negative electrode of each battery, then fully charge the button cell to 100% SOC, dissect its negative electrode, test the active material thickness D2 of the negative electrode at this time, and calculate the full charge expansion rate according to the following formula: Full charge expansion rate = (D2-D1) ÷ D1 × 100%.

[0039] The test results are shown in Table 2 below.

[0040] Table 2. Test Results of Button Cells

[0041] As shown in Table 2, compared with Comparative Examples 1 to 3, the coin cell made from the heteroatom-doped silicon-carbon composite material in Example 1 has a higher initial discharge specific capacity and initial efficiency, and a lower full-charge expansion rate. The reason may be that the high electronic conductivity of porous magnesium oxide itself and the magnesium silicate formed by porous magnesium oxide and nano-silicon improve the initial discharge specific capacity and initial efficiency, and reduce the full-charge expansion rate.

[0042] Experiment Example 3: Soft Pack Battery Test The heteroatom-doped silicon-carbon composite materials prepared in Examples 1-3 and Comparative Examples 1-3 were used to prepare pouch cells according to the following method: each heteroatom-doped silicon-carbon composite material was doped with artificial graphite (the mass ratio of heteroatom-doped silicon-carbon composite material to artificial graphite was 1:9) as the negative electrode and the positive electrode ternary material LiNi. 1 / 3 Co 1 / 3 Mn 1 / 3 O2, electrolyte (1.3 mol / L LiPF6, solvent composed of ethylene carbonate and diethyl carbonate in a 1:1 volume ratio), and separator (Celegate 2400) were assembled into a 5 Ah pouch cell. The following performance tests were performed on each pouch cell: ① Liquid absorption capacity: Use a 1mL burette to draw 1mL of electrolyte, add one drop to the surface of the negative electrode, and time the process until the electrolyte is completely absorbed. Record the liquid absorption time. ② Electrode surface resistance test: An electrode surface resistance tester (model FT-551) is used to test the surface resistance of a 100cm² electrode. 2 The negative electrode is placed on the test bench, and its resistance is tested under a pressure of 500 kg. ③ Cyclic performance test: The test conditions are a charge / discharge voltage range of 2.5~4.2V, a temperature of 25±3.0℃, a charge / discharge rate of 1.0C / 1.0C, and 500 cycles; ④ Rate performance test: The capacity retention rate was tested at 0.5C, 1C, 2C and 3C respectively.

[0043] The test results are shown in Table 3 below.

[0044] Table 3 Test Results of Pouch Batteries

[0045] As shown in Table 3, compared with Comparative Examples 1 to 3, the soft-pack battery made from the heteroatom-doped silicon-carbon composite material in Example 1 has higher liquid absorption capacity and lower electrode surface resistance. This is because the heteroatom-doped silicon-carbon composite material prepared in Example 1 has a higher specific surface area and a lower powder resistivity.

[0046] Compared with Comparative Examples 1-3, the pouch cell prepared from the heteroatom-doped silicon-carbon composite material in Example 1 has better cycle performance. This is because the heteroatom-doped silicon-carbon composite material prepared in Example 1 has lower expansion and higher specific surface area, which improves the liquid retention performance, reduces the expansion of the pouch cell during cycling, and improves the cycle performance.

[0047] Compared with Comparative Examples 1-3, the pouch cell made from the heteroatom-doped silicon-carbon composite material in Example 1 has better rate performance. This is because the heteroatom-doped silicon-carbon composite material prepared in Example 1 has higher powder conductivity and larger specific surface area, thereby improving rate performance.

[0048] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a heteroatom-doped silicon-carbon composite material, characterized in that, Includes the following steps: S1. Add basic magnesium carbonate and catalyst to the heteroatom solution, disperse evenly, spray dry, and sinter to obtain heteroatom-doped porous magnesium oxide; The mass ratio of basic magnesium carbonate, heteroatom solution, and catalyst is 100:100~500:1~5. The heteroatom solution is one of urea solution, melamine solution, hydrazine hydrate solution, boric acid solution, and phosphoric acid solution. The mass fraction of the heteroatom solution is 1%~10%. The catalyst is one of bismuth isooctanoate, bismuth laurate, and bismuth neodecanoate. S2. Silane gas is introduced into the heteroatom-doped porous magnesium oxide for the first deposition, followed by the introduction of a heteroatom mixed gas, the second deposition, the introduction of halosilane gas, the third deposition, the introduction of an oxidizing gas, the fourth deposition, the introduction of a first carbon source gas, and the fifth deposition to obtain a heteroatom-doped silicon-carbon composite material. The heteroatom mixed gas is a mixture of heteroatom gas and a second carbon source gas, wherein the heteroatom gas is one of ammonia, phosphine, hydrogen sulfide, and sulfur dioxide. The first deposition was performed at a temperature of 450–650°C for 30–300 min; and / or The second deposition is performed at a temperature of 600–900°C for a time of 10–60 min; and / or The third deposition was performed at a temperature of 500–800°C for 30–120 minutes; and / or The fourth deposition was performed at a temperature of 200-300°C for 30-300 minutes; and / or The fifth deposition was carried out at a temperature of 600-900℃ for 30-300 minutes.

2. The method for preparing a heteroatom-doped silicon-carbon composite material according to claim 1, characterized in that, In step S1, the sintering temperature is 600~1000℃ and the time is 1~3h.

3. The method for preparing a heteroatom-doped silicon-carbon composite material according to claim 1, characterized in that, In step S2, the silane gas is one of trichlorosilane, ethoxysilane, and dimethylsilane; When introducing silane gas, the introduction rate is 50~200mL / min.

4. The method for preparing a heteroatom-doped silicon-carbon composite material according to claim 1, characterized in that, The second carbon source gas is one of methane, acetylene, and ethylene; The volume ratio of the heteroatom gas to the second carbon source gas is 10:1~5; When introducing the heteroatom mixed gas, the introduction rate is 50~200mL / min.

5. The method for preparing a heteroatom-doped silicon-carbon composite material according to claim 1, characterized in that, In step S2, the halosilane gas is one of tetrafluorosilane, trichlorofluorosilane, tetrachlorosilane, and hexafluorodisilane; When introducing halosilane gas, the introduction rate is 50~200mL / min.

6. The method for preparing a heteroatom-doped silicon-carbon composite material according to claim 1, characterized in that, In step S2, the oxidizing gas is one of nitrous oxide, hydrogen peroxide, oxygen, ozone, nitric oxide, and nitrogen dioxide. When introducing the oxidizing gas, the introduction rate is 50~200mL / min.

7. The method for preparing a heteroatom-doped silicon-carbon composite material according to claim 1, characterized in that, In step S2, the first carbon source gas is one of methane, acetylene, and ethylene; When the first carbon source gas is introduced, the introduction rate is 100~200mL / min.

8. The application of the heteroatom-doped silicon-carbon composite material prepared by the method according to any one of claims 1 to 7 in lithium-ion battery materials.

Citation Information

Patent Citations

  • Porous carbon doping induced silicon deposition silicon-carbon negative electrode material and preparation method thereof

    CN114122352A

  • Method for formation of crystalline boron-doped silicon carbide and amorphous boron silicon oxycarbide fibers from polymer blends containing siloxane and boron