Process for the preparation of a low palladium content high selectivity palladium catalyst for fixed bed anthraquinone hydrogenation

By preparing a low-palladium-content, high-selectivity palladium catalyst, the problem of catalyst instability in fixed-bed hydrogen peroxide production was solved, the selectivity and stability of the catalyst under high-temperature conditions were improved, the cost was reduced, and it is suitable for large-scale industrial production.

CN118976484BActive Publication Date: 2026-11-24YANTAI BAICHUAN HUITONG TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411054406.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2026-11-24
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

In the existing fixed-bed hydrogen peroxide production process, uneven distribution of working fluid due to catalyst loading problems or flow fluctuations leads to unstable catalyst hydrogenation, generating harmful degradation products, increasing costs, and the existing catalysts have insufficient selectivity under high-temperature conditions.

Method used

A low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation was prepared by controlling the pore structure and palladium distribution of the alumina sphere support, and by employing ultrasonic treatment and negative pressure spraying technology to ensure that palladium is uniformly loaded on the support surface, forming a large-pore mesoporous structure, thereby improving the stability and selectivity of the catalyst.

Benefits of technology

It achieves fewer anthraquinone byproducts under high-temperature conditions, reduces the problems of excessive hydrogenation and temperature deviation, lowers costs, has strong adaptability, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976484B_ABST
    Figure CN118976484B_ABST
Patent Text Reader

Abstract

This invention relates to a method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation, belonging to the technical field of palladium catalyst preparation methods. The method includes the following steps: Step S1: Preparing an alumina sphere support; Step S2: Sonicating the prepared alumina sphere support in deionized water, filtering to remove moisture until no obvious water stains remain, obtaining a wet support; Step S3: Transferring the wet support obtained in Step S2 to a palladium-supported device, spraying palladium solution onto the support, maintaining constant temperature and pressure for 2 hours, and then washing with hot water until the chloride ion content is within acceptable limits, obtaining the primary state of the palladium catalyst; Step S4: Drying and calcining the obtained palladium catalyst to finally obtain the desired palladium catalyst. The palladium catalyst prepared by this invention has a large-pore mesoporous structure, with palladium distributed on the surface. After anthraquinone hydrogenation, it can quickly detach from the palladium catalyst, avoiding over-hydrogenation and effectively mitigating the problems of palladium catalyst pore blockage and anthraquinone degradation caused by over-hydrogenation under special operating conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing a palladium catalyst, and more particularly to a method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation, which belongs to the technical field of palladium catalyst preparation methods. Background Technology

[0002] Currently, the main method for producing hydrogen peroxide worldwide is the anthraquinone process. The anthraquinone process involves the catalytic hydrogenation of alkyl anthraquinone in a solvent to produce hydrogen anthraquinone, which is then oxidized by air to produce alkyl anthraquinone and hydrogen peroxide. The generated hydrogen peroxide is extracted with deionized water and collected, while the raffinate is regenerated and recycled. Existing hydrogenation methods for producing H2O2 using the anthraquinone process generally employ fluidized bed and fixed bed methods. Currently, domestic H2O2 production enterprises commonly use fixed bed methods, with the working fluid composition consisting of 2-ethylanthraquinone (2-EAQ), tetrahydro-2-ethylanthraquinone (4H-2-EAQ), heavy aromatics, trioctyl phosphate, TBU, etc. Generally, the anthraquinone process mainly includes four steps: hydrogenation, oxidation, extraction, and post-treatment. Catalytic hydrogenation is the key step in the production of hydrogen peroxide using the anthraquinone process; highly active and selective catalysts can effectively improve hydrogenation efficiency and reduce anthraquinone degradation.

[0003] Currently, fixed-bed hydrogen peroxide plants dominate the market in my country. During production, uneven distribution of the working fluid due to catalyst loading issues or flow fluctuations can cause flow deviations, leading to unstable catalyst hydrogenation and the generation of other harmful degradation products. This damages the effective components of the working fluid, increasing the costs of anthraquinone and regenerated alumina. Therefore, to improve the catalyst's adaptability under extreme operating conditions, enhance production stability, and minimize operating costs, a higher-performance catalyst is urgently needed to meet market demands. Summary of the Invention

[0004] Technical Objective: To overcome the shortcomings of existing technologies, this invention provides a method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation. The prepared palladium catalyst not only exhibits excellent selectivity under normal operating conditions but also produces fewer anthraquinone byproducts at high temperatures. This significantly reduces the impact of problems such as excessive hydrogenation and large temperature deviations caused by short-term working fluid deviation in fixed-bed processes on the palladium catalyst and working fluid systems. The method is low-cost and suitable for large-scale industrial production.

[0005] Technical Solution: To achieve the above objectives, this invention discloses a method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation, comprising the following steps:

[0006] Step S1: After mixing aluminum raw materials and deionized water in a certain proportion, add a fixed proportion of acid solution dropwise, while controlling the reaction temperature and rotation speed. After a certain reaction time, a colloid is obtained. The colloid is acidic. Add a curing agent to the colloid, stir evenly, and then form it in an oil column. Finally, after aging, water washing, drying, and calcination processes, alumina ball carrier is obtained.

[0007] Step S2: The prepared alumina ball carrier is ultrasonically treated in deionized water, and the water is removed by filtration until there are no obvious water stains to obtain a wet carrier.

[0008] Step S3: Transfer the wet support obtained in step S2 to the palladium support device, set the rotation speed, spray the palladium liquid onto the support under a certain temperature and negative pressure, keep it at constant temperature and pressure for 2 hours, and then wash it with hot water until the chloride ion content is qualified to obtain the primary state of palladium catalyst.

[0009] Step S4: The palladium catalyst obtained in step S3 is dried and calcined to finally obtain the desired palladium catalyst.

[0010] Furthermore, in step S1, the mass ratio of the aluminum raw material, deionized water, acid solution, and curing agent is 1:2 to 20:1 to 7:0.2 to 5, which is optimized to 1:3 to 10:1.5 to 4:0.3 to 2.5.

[0011] Furthermore, in step S1, the reaction temperature of the material is 10–100℃, optimized to 25–95℃; the stirring rate is 50–400 rad / min, optimized to 100–180 rad / min; the stirring time is 0.1–12 h, optimized to 0.5–8 h; the oil column temperature is 60–110℃, optimized to 85–99℃; the aging temperature is 80–150℃, optimized to 85–140℃; the aging time is 1–30 h, optimized to 2–24 h; the water washing temperature is 10–100℃, preferably 10–70℃; the drying temperature is 70–120℃, optimized to 95–115℃; the drying time is 8–24 h, optimized to 14–18 h; the calcination temperature is 400–1100℃, optimized to 500–1000℃; and the calcination time is 1–8 h, optimized to 2–6 h.

[0012] Furthermore, in step S1, the aluminum raw material includes one or more of aluminum powder, boehmite, and aluminum nitrate; the acid solution includes one or more of hydrochloric acid, nitric acid, formic acid, and acetic acid; the curing agent includes one or more of hexamethylenetetramine, ammonia, and urea; and the oil in the oil column includes one or more of machine oil, hydraulic oil, gear oil, and white oil.

[0013] Furthermore, in step S2, the alumina sphere carrier is selected to have a specific surface area of ​​70–150 m². 2 / g, preferably 80-120m 2 / g; pore volume is 0.65–1.5 cc / g, preferably 0.7–0.9 cc / g; average pore size is 15–30 nm, preferably 18–25 nm; bulk density is 0.4–0.8 g / cm³. 3 The preferred concentration is 0.45–0.6 g / cm³. 3 The diameter of the alumina ball carrier is 1.8–2.5 mm, preferably 2.2–2.4 mm.

[0014] Furthermore, in step S2, the volume of the deionized water is 1.2 to 2 times the volume of the alumina ball carrier, preferably 1.5 to 1.8 times; the soaking time is 0.5 to 3 hours, preferably 1 to 2 hours; and the ultrasonic frequency is 20 to 50 kHz, preferably 30 to 40 kHz.

[0015] Furthermore, in step S3, the rotational speed of the palladium-carrying device is 2–10 rad / min, preferably 3–5 rad / min; the temperature is 70–99°C, preferably 80–90°C; the vacuum degree is 0–-1 bar, preferably -0.1–-0.4 bar; the palladium solution content is 0.2 wt%–0.8 wt%, preferably 0.3 wt%–0.7 wt%; the ratio of palladium solution volume to carrier volume is 1:2–4, preferably 1:2.5–3.5; and the hot water washing temperature is 30–80°C, preferably 40–60°C.

[0016] Furthermore, in step S3, the palladium solution includes one or more of palladium chloride solution, palladium nitrate solution, and palladium acetate solution.

[0017] Furthermore, in step S4, the drying conditions are as follows: drying under negative pressure, with a vacuum degree of 0 to -1 bar, preferably -0.4 to -0.6 bar; drying temperature of 90 to 140°C, optimized to 100 to 110°C; drying time of 0.5 to 24 h, optimized to 8 to 15 h; calcination temperature of 450 to 550°C, optimized to 480 to 520°C; and calcination time of 1 to 6 h, optimized to 2.5 to 4 h.

[0018] Furthermore, the palladium catalyst has an average pore size of 19–23 nm and a diameter of 2.21–2.38 mm.

[0019] The present invention has the following beneficial effects:

[0020] (1) The palladium catalyst prepared by this invention has an average pore size of 19-23 nm, has a large-pore mesoporous structure, and palladium is distributed on the surface. After hydrogenation, anthraquinone can quickly detach from the palladium catalyst, avoiding excessive hydrogenation and effectively mitigating the problems of palladium catalyst pore blockage and anthraquinone degradation caused by excessive hydrogenation under special working conditions. The diameter of the palladium catalyst is 2.21-2.38 mm, which can avoid the problem of large bed resistance caused by excessively small particle size, and also avoid the problem of reduced palladium catalyst utilization caused by excessively large particle size.

[0021] (2) The amount of palladium required for the preparation of palladium catalyst in this invention is about 50% of the amount of palladium required for the preparation of traditional palladium catalyst. The cost of precious metal is significantly reduced, while the activity can reach 95% of that. Furthermore, the selectivity of palladium catalyst is increased by more than 20% under high temperature conditions, which fully meets the production requirements.

[0022] (3) In the process of preparing alumina sphere carrier, the colloid as an intermediate product allows for more precise control of the pore structure and surface characteristics of the alumina sphere carrier. The size and shape of the colloidal particles can be controlled by adjusting the reaction conditions (such as acid amount, temperature, rotation speed, etc.), thereby precisely controlling the pore size and distribution of the final alumina product. Due to its highly dispersed characteristics, the colloid can uniformly mix the aluminum source and other components at the molecular level. This uniform dispersion ensures that the active centers can be uniformly distributed on the surface and inside of the alumina sphere carrier during subsequent molding and calcination. The thermal stability is improved. In high-temperature catalytic reactions, this highly thermally stable alumina sphere carrier can maintain its structure, thus maintaining catalytic activity and service life.

[0023] (4) In this invention, the ultrasonic treatment is used to clean the alumina powder attached to the surface of the carrier and the micropores, reduce the loss of palladium caused by the shedding of palladium-containing alumina powder during palladium adsorption, and at the same time ensure that the water in the micropores of the carrier is evenly wetted, thus ensuring the palladium adsorption stability of the product.

[0024] (5) The palladium catalyst prepared by the present invention controls the vaporization of water in the support and quickly sprays palladium liquid onto the surface of the support. Due to the high temperature of the support surface and the combined effect of water evaporation and negative pressure, palladium is loaded on the support surface, so the utilization rate of active metal is high.

[0025] (6) The palladium catalyst prepared by this invention not only has excellent selectivity under normal operating conditions, but also produces fewer anthraquinone byproducts under high temperature conditions. This greatly reduces the impact of problems such as excessive hydrogenation and large temperature deviation caused by short-term flow deviation of the working fluid in the fixed bed process on the palladium catalyst and working fluid system. It is low in cost and can be mass-produced industrially. Attached Figure Description

[0026] Figure 1 The attached figure shows the isothermal adsorption-desorption of the palladium catalyst prepared in Example 1 of this invention;

[0027] Figure 2 The accompanying figure shows the isothermal adsorption-desorption of palladium catalyst in the comparative example of this invention;

[0028] Figure 3 This is a schematic diagram of the pore radius of the palladium catalyst prepared in Example 1 of this invention;

[0029] Figure 4 This is a schematic diagram of the pore radius of the palladium catalyst in the comparative example of this invention;

[0030] Figure 5 The working solution was analyzed by liquid chromatography, and the effective anthraquinones and degradation products were chromatograms (I).

[0031] Figure 6 The working solution is analyzed by liquid chromatography, and the effective anthraquinones and degradation products are shown in the spectrum (II). Detailed Implementation

[0032] The following is in conjunction with the appendix Figure 1 To be continued Figure 6 The principles and features of the present invention are described, and the examples given are only for explaining the present invention and are not intended to limit the scope of the present invention.

[0033] Example 1:

[0034] A method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation includes the following steps:

[0035] Step S1: Add 100g of aluminum powder to 500g of deionized water and add 250g of 30% nitric acid dropwise at a rate of 20ml / min. Mix and stir in a reflux flask at a stirring rate of 80rad / min at 80℃ for 6 hours. After stirring, cool to room temperature to obtain a colloid. The colloid is acidic. Add 40g of ammonia and 10g of urea and mix and stir at a stirring rate of 150rad / min for 0.5 hours. Then, form it in a white oil column at 90℃. After reacting at 120℃ for 4 hours, wash to remove oil, dry at 110℃, and calcine at 900℃ for 4 hours to obtain alumina ball carrier.

[0036] Step S2: Take 100g of carrier, add 150ml of deionized water, sonicate at 40kHz for 30min, then filter until there is no obvious water to obtain wet carrier;

[0037] Step S3: Transfer the wet support to the palladium support device and heat it to 90°C. Weigh 0.234g of palladium chloride, add 20ml of water, 0.3g of hydrochloric acid and 0.5g of sodium chloride, heat to dissolve, cool and dilute with water to 70ml to obtain palladium solution. Rotate at 3rad / min. After the reactor is preheated to 90°C, spray the palladium solution onto the support. After completion, control the temperature at 80°C and the vacuum degree at -0.3bar. Continue to rotate for 2 hours and wash with 60°C deionized water until the chloride ion concentration is less than 10mg / L to obtain the primary state of palladium catalyst.

[0038] Step S4: Dry at 120℃ for 12 hours with a rotation speed of 4 rad / min and a vacuum of -0.8 bar. The calcination atmosphere is air. The temperature is increased to 450℃ at a rate of 5℃ / min and the calcination time is 3 hours to obtain a Pd / Al2O3 catalyst. The palladium content in the Pd / Al2O3 catalyst is 1.4 wt‰.

[0039] Example 2:

[0040] A method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation includes the following steps:

[0041] Step S1: Add 100g of aluminum powder to 400g of water, and add 340g of 30% hydrochloric acid dropwise at a rate of 3ml / min. Mix and stir at 100rad / min in a reflux flask at 80℃ for 6 hours. After stirring, cool to room temperature to obtain a colloid. The colloid is acidic. Add 30g of hexamethylenetetramine and 10g of urea, and mix and stir at a rate of 150rad / min for 0.5 hours. Then, form it in a white oil column at 92℃, react at 140℃ for 10 hours, wash to remove oil, dry at 110℃, and calcine at 900℃ for 4 hours to obtain alumina ball carrier.

[0042] Step S2: Take 100g of carrier, add 150ml of deionized water, sonicate at 40kHz for 30min, then filter until there is no obvious water to obtain wet carrier;

[0043] Step S3: Transfer the wet support to the palladium support device and heat it to 90°C. Weigh 0.268g of palladium chloride, add 20ml of water, 0.34g of hydrochloric acid and 0.57g of sodium chloride, heat to dissolve, cool and dilute with water to 75ml to obtain palladium solution. Rotate at 3rad / min. After the reactor is preheated to 90°C, spray the palladium solution onto the support. After completion, control the temperature at 80°C and the vacuum degree at -0.3bar. Continue to rotate for 2 hours and wash with 60°C deionized water until the chloride ion concentration is less than 10mg / L to obtain the primary state of palladium catalyst.

[0044] Step S4: Dry at 120℃ for 12 hours with a rotation speed of 4 rad / min and a vacuum of -0.8 bar. The calcination atmosphere is air. The temperature is increased to 450℃ at a rate of 5℃ / min and the calcination time is 3 hours to obtain a Pd / Al2O3 catalyst. The palladium content in the Pd / Al2O3 catalyst is 1.6 wt‰.

[0045] Example 3:

[0046] A method for preparing a low-palladium-content, high-selectivity palladium catalyst for fixed-bed anthraquinone hydrogenation includes the following steps:

[0047] Step S1: Add 300g of pseudoboehmite to 500g of deionized water, add 400g of 10% nitric acid, mix evenly, and then mix and stir at 150rad / min at 50℃ for 0.5h to obtain a colloid. The colloid is acidic. Add 28g of urea and 80g of hexamethylenetetramine, stir evenly for 30min, form in a white oil column at 88℃, react at 110℃ for 2h, then wash to remove oil, dry at 110℃, and calcine at 900℃ for 4h to obtain alumina ball carrier.

[0048] Step S2: Take 100g of carrier, add 150ml of deionized water, sonicate at 40kHz for 30min, then filter until there is no obvious water to obtain wet carrier;

[0049] Step S3: Transfer the wet support to the palladium support device and heat it to 90°C. Weigh 0.44g of palladium nitrate, add 20ml of water, add 1g of nitric acid and heat to dissolve. After cooling, dilute with water to 65ml to obtain palladium solution. Rotate at 3rad / min. After the reactor is preheated to 90°C, spray the palladium solution onto the support. After completion, control the temperature at 80°C and the vacuum degree at -0.3bar. Continue to rotate for 2 hours and wash with 60°C deionized water until the chloride ion concentration is less than 10mg / L to obtain the primary state of palladium catalyst.

[0050] Step S4: Dry at 120℃ for 12 hours under controlled rotation speed of 4 rad / min and vacuum degree of -0.8 bar, with air as the calcination atmosphere. Increase the temperature to 450℃ at 5℃ / min and calcinate for 3 hours. Obtain Pd / Al2O3 catalyst with a palladium content of 1.8 wt‰.

[0051] Comparative example: A commercially available palladium catalyst with a palladium content of 3 wt‰ was used.

[0052] The palladium catalysts in Examples 1-3 and the comparative example were tested using the following methods: 20g of palladium catalyst was loaded, and 200ml of working solution was circulated (the working solution components were Ar:TOP:TBU = 2:0.7:0.3, the solute was diethylanthraquinone, and the concentration was 60g / L). The operating temperature was 70℃, and the circulation rate was 1.8L / h. The activity value was obtained by taking 5ml of working solution every 3 hours, performing oxidative extraction, and titrating with potassium permanganate. The average value was then taken. Selectivity was evaluated by liquid chromatography. After 24 hours of operation, the components of the working solution were analyzed, and the degradation status was judged based on the anthraquinone content and impurity peaks. The specific data are shown in Table 1.

[0053] Table 1: Summary Table of Data from Examples 1-3 and Comparative Examples

[0054]

[0055]

[0056] in conclusion:

[0057] (1) As can be seen from the data in Table 1, the palladium catalyst activity in the three examples reached more than 95% of that in the comparative 3‰ palladium catalyst, the total anthraquinone content was more than 20% higher, and the anthraquinone degradation was less.

[0058] (2) Figure 1 and Figure 2 The figures shown are isothermal adsorption-desorption curves for the palladium catalyst prepared in Example 1 and the comparative palladium catalyst (red represents the desorption curve, black represents the adsorption curve). Since Examples 1-3 show the same trend, Example 1 is used for overall analysis. Figure 1 It can be seen that: Example 1 is a typical ordered mesoporous material, and the pressure at the tail end condensation section is relatively large, indicating that the palladium catalyst has a uniform mesoporous distribution and a large pore size. The comparative example is also a typical ordered mesoporous material, but the pressure at the tail end condensation section is relatively lower than that of the example, indicating that the palladium catalyst has a uniform mesoporous distribution but a smaller pore size.

[0059] (3) Figure 3 and Figure 4 The figures show the desorption pore area distribution of the palladium catalyst prepared in Example 1 and the comparative palladium catalyst, respectively. Since Examples 1-3 show the same trend, Example 1 is used for overall analysis. Figure 3 It can be seen that the pore size of the palladium catalyst in Example 1 is concentrated between 18 and 22 nm, while the pore size of the palladium catalyst in the comparative example is concentrated between 7 and 9 nm.

[0060] (4) Figure 5 and Figure 6After the working solutions in Examples 1 and the comparative example were run under specified conditions for a period of time, the effective anthraquinones and degradation products were analyzed by liquid chromatography. Since Examples 1-3 showed the same trend, Example 1 was used for overall analysis. According to the peak shape, after running at 70°C for 24 hours, the anthraquinones in the working solution of Example 1 were mainly diethylanthraquinone and tetrahydrodiethylanthraquinone, both of which are effective components. However, the working solution of the comparative example had two obvious impurity peaks. Combined with the total anthraquinone detection data, it can be concluded that the comparative example had more degradation products after running at high temperature, thus proving that the performance of Example 1 is more stable.

[0061] The palladium catalyst prepared by this invention not only exhibits excellent selectivity under normal operating conditions, but also produces fewer anthraquinone byproducts at high temperatures. This significantly reduces the impact of problems such as excessive hydrogenation and large temperature deviations caused by short-term working fluid deviation in fixed-bed processes on the palladium catalyst and working fluid systems. It is also low in cost and can be mass-produced industrially.

[0062] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. The application of a low-palladium-content, high-selectivity palladium catalyst in fixed-bed anthraquinone hydrogenation, characterized in that, The preparation of the low-palladium-content, high-selectivity palladium catalyst includes the following steps: Step S1: After mixing aluminum raw materials and deionized water in a certain proportion, add a fixed proportion of acid solution dropwise, while controlling the reaction temperature and rotation speed. After a certain reaction time, a colloid is obtained. The colloid is acidic. Add a curing agent to the colloid, stir evenly, and then form it in an oil column. Finally, after aging, water washing, drying, and calcination processes, alumina ball carrier is obtained. The acid solution includes one or more of hydrochloric acid, nitric acid, formic acid, and acetic acid; the curing agent includes one or more of hexamethylenetetramine, ammonia, and urea. Step S2: The prepared alumina ball carrier is ultrasonically treated in deionized water, and the water is removed by filtration until there are no obvious water stains to obtain a wet carrier. The specific surface area of ​​the alumina sphere carrier is 70–150 m². 2 / g, pore volume of 0.65–1.5cc / g, average pore size of 15–30nm, and bulk density of 0.4–0.8g / cm³. 3 The diameter of the alumina sphere carrier is 1.8–2.5 mm; Step S3: Transfer the wet support obtained in step S2 to the palladium support device, set the rotation speed, spray the palladium chloride solution onto the support at 70-99℃ and -0.1--0.4 bar vacuum, keep it at constant temperature and pressure for 2 hours, and then wash it with hot water until the chloride ion content is qualified to obtain the primary state of palladium catalyst. Step S4: The palladium catalyst obtained in step S3 is dried and calcined to finally obtain the desired palladium catalyst.

2. The application of the low palladium content, high selectivity palladium catalyst according to claim 1 in fixed-bed anthraquinone hydrogenation, characterized in that: In step S1, the mass ratio of the aluminum raw material, deionized water, acid solution, and curing agent is 1:2 to 20:1 to 7:0.2 to 5.

3. The application of the low palladium content, high selectivity palladium catalyst according to claim 1 in fixed-bed anthraquinone hydrogenation, characterized in that: In step S1, the reaction temperature of the material is 10-100℃, the stirring time is 0.1-12h, the oil column temperature is 60-110℃, the aging temperature is 80-150℃, the aging time is 1-30h, the water washing temperature is 10-100℃, the drying temperature is 70-120℃, the drying time is 8-24h, the calcination temperature is 400-1100℃, and the calcination time is 1-8h.

4. The application of the low palladium content, high selectivity palladium catalyst according to claim 1 in fixed-bed anthraquinone hydrogenation, characterized in that: In step S1, the aluminum raw material includes one or more of aluminum powder, boehmite, and aluminum nitrate; the oil in the oil column includes one or more of machine oil, hydraulic oil, gear oil, and white oil.

5. The application of the low palladium content, high selectivity palladium catalyst according to claim 1 in fixed-bed anthraquinone hydrogenation, characterized in that: In step S2, the volume of deionized water is 1.2 to 2 times the volume of the alumina ball carrier, the soaking time is 0.5 to 3 hours, and the ultrasonic frequency is 20 to 50 kHz.

6. The application of the low palladium content, high selectivity palladium catalyst according to claim 1 in fixed-bed anthraquinone hydrogenation, characterized in that: In step S3, the palladium chloride solution content is 0.2wt% to 0.8wt%, the volume ratio of palladium chloride solution to carrier is 1:2 to 4, and the hot water washing temperature is 30 to 80℃.

7. The application of the low palladium content, high selectivity palladium catalyst according to claim 1 in fixed-bed anthraquinone hydrogenation, characterized in that: In step S4, the drying conditions are as follows: drying under negative pressure, vacuum degree of 0 to -1 bar, drying temperature of 90 to 140°C, drying time of 0.5 to 24 h, calcination temperature of 450 to 550°C, and calcination time of 1 to 6 h.

8. The application of the low palladium content, high selectivity palladium catalyst according to claim 1 in fixed-bed anthraquinone hydrogenation, characterized in that: The palladium catalyst has an average pore size of 19–23 nm and a diameter of 2.21–2.38 mm.

Citation Information

Patent Citations

  • Supported catalyst and preparation method thereof

    CN104001557A

  • Palladium catalyst for producing hydrogen peroxide by anthraquinone process and preparation method of palladium catalyst

    CN110639512A