Egg yolk shell type composite molecular sieve, preparation method thereof, hydrofining catalyst and preparation method and application thereof

By preparing a Ni and Mo supported catalyst using an eggshell-shaped composite molecular sieve, the problems of high energy consumption and low desulfurization efficiency in existing hydrorefining catalysts were solved, achieving a highly efficient hydrodesulfurization effect, which is suitable for deep desulfurization of diesel fuel.

CN118988394BActive Publication Date: 2026-11-24CHINA UNIV OF PETROLEUM (BEIJING)
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411083943.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2026-11-24
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

Existing hydrorefining catalysts suffer from high energy consumption, short catalyst life, and low throughput in deep desulfurization processes, and are particularly difficult to effectively remove sterically hindered sulfides such as 4,6-DMDBT.

Method used

Using yolk-shell type composite molecular sieve (Yolk-Shell SiO₂) as a support, a catalyst with controllable shell and core structure was synthesized by nano-self-assembly method, and Ni and Mo active metals were loaded to optimize the pore structure and acidity, forming NiMo/TS-1-Yolk-Shell SiO₂ catalyst.

Benefits of technology

It achieves a highly efficient hydrodesulfurization reaction, with a desulfurization rate of up to 98% for 4,6-DMDBT and a sulfur content of less than 10 ppm, meeting the China VI standard. It also improves catalytic activity and metal dispersion, and optimizes mass transfer capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988394B_ABST
    Figure CN118988394B_ABST
Patent Text Reader

Abstract

The application provides an egg yolk shell type composite molecular sieve and a preparation method thereof, a hydrorefining catalyst and a preparation method and application thereof. The egg yolk shell type composite molecular sieve has an inner core composed of TS-1 molecular sieve, a shell layer composed of silicon dioxide and a cavity between the inner core and the shell layer; the thickness of the shell layer is 3-26 nm, the diameter size of the inner core is less than or equal to 51 nm, and the size of the cavity is 24-75 nm. The egg yolk shell type composite molecular sieve has controllable shell layer thickness and inner core size, and the hydrorefining catalyst has good catalytic hydrodesulfurization activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalyst technology, and more specifically to an egg yolk shell type composite molecular sieve and its preparation method, a hydrorefining catalyst and its preparation method and application. Background Technology

[0002] Hydrorefining technology is an effective means of improving oil quality and producing clean oil products on a large scale in the petroleum refining industry. Increasing reaction temperature, decreasing reaction space velocity, and increasing reactor volume can improve the depth of hydrodesulfurization to some extent, but this increases energy consumption, reduces catalyst lifespan, and decreases feedstock throughput. In contrast, the most economical and convenient approach is to develop suitable, highly active hydrodesulfurization catalysts to achieve large-scale production of ultra-low sulfur and ultra-clean oil products.

[0003] In recent years, mesoporous-microporous composite molecular sieves have gradually become a research hotspot in the field of catalytic hydrogenation. Mesoporous-microporous composite technology combines the pore advantages of mesoporous molecular sieves with the tunable acidity and high hydrothermal stability of microporous molecular sieves, exhibiting a dual-template pore distribution of micropores and mesopores. Commonly used synthesis methods include in-situ synthesis, pore wall crystallization, and nano-assembly. Mesoporous-microporous composite technology not only broadens the pore size of zeolite molecular sieves, effectively reducing or avoiding diffusion resistance of macromolecular sulfides within the pores and accelerating mass transfer and reaction processes between reactants and products, but also provides more options for the hydrodesulfurization reaction pathway and selectivity due to its significantly enhanced acidity, demonstrating a synergistic effect not found in single-component molecular sieves.

[0004] CN113019440A discloses a method for preparing a hydrorefining catalyst for ultra-deep desulfurization of diesel fuel. The catalyst uses a Beta / Al-SBA-15 composite molecular sieve and alumina as supports. The method first synthesizes the Beta / Al-SBA-15 composite molecular sieve, then mixes it with alumina dry adhesive powder, shapes it, dries it, and calcines it. This method relies primarily on mechanical mixing, making it difficult to fully utilize the diffusion advantages of reactant molecules in the large-pore structure of the mesoporous molecular sieve, and to achieve adjustment of the acidity of the support material and optimization of the pore structure. Summary of the Invention

[0005] To address the problems in the prior art, the present invention aims to provide an egg yolk-shell type composite molecular sieve and its preparation method, a hydrorefining catalyst and its preparation method, and its applications. The egg yolk-shell type composite molecular sieve has controllable shell thickness and core size, and the hydrorefining catalyst exhibits good catalytic hydrodesulfurization activity.

[0006] To achieve the above objectives, according to a first aspect of the present invention, a yolk-shell type composite molecular sieve (Yolk-Shell SiO2) is provided, which has a core composed of TS-1 molecular sieve, a shell composed of silica, and a cavity between the core and the shell; the thickness of the shell is 3-26 nm, preferably 7-23 nm; the diameter of the core is ≤51 nm, preferably 3-41 nm; and the size of the cavity is 24-75 nm, preferably 30-65 nm.

[0007] The size of the cavity refers to the distance between the core and the shell.

[0008] The eggshell-type composite molecular sieve of the present invention has controllable shell size and core size, which is beneficial to the uniform loading of active metals and the free diffusion of macromolecular reactants.

[0009] In a preferred embodiment of the present invention, the specific surface area of ​​the egg yolk shell type composite molecular sieve is 500-700 m². 2 ·g -1 The preferred pore size is 520–650 nm; the average pore size is 4–9 nm, preferably 5–8 nm; and the pore volume is 0.5–1.4 cm³. 3 ·g -1 Preferably 0.6–1.2 cm 3 ·g -1 The superior pore structure, large specific surface area, and pore volume of this preferred method are more conducive to the uniform loading of active metals on the eggshell-type composite molecular sieve. In a preferred embodiment of the present invention, the eggshell-type composite molecular sieve contains micropores with a pore size of approximately 0.67 nm.

[0010] In a preferred embodiment of the present invention, the total acidity of the egg yolk shell-type composite molecular sieve is 35–96 μmol·g. -1 The preferred concentration is 48–84 μmol·g. -1 The acidity is 30–76 μmol·g. -1 The preferred concentration is 40–68 μmol·g. -1 The acidity of B is 5–20 μmol·g. -1 Preferably 8–16 μmol·g -1 Based on this optimized yolk-shell type composite molecular sieve with suitable acidity, it is more conducive to the uniform loading of active metals on the yolk-shell type composite molecular sieve, which changes the metal-support interaction force, improves the dispersion of active metals, and is beneficial to improving catalytic efficiency.

[0011] In a preferred embodiment of the present invention, the SiO2 / TiO2 molar ratio in the eggshell-type composite molecular sieve is 30–400. This preferred silicon-aluminum ratio is more conducive to improving the activity of the hydrodesulfurization reaction.

[0012] According to another aspect of the present invention, a hydrorefining catalyst, designated NiMo / TS-1-Yolk-Shell SiO2, is also provided. The catalyst is supported by the aforementioned yolk-shell type composite molecular sieve, on which oxides of Mo and Ni are loaded. The catalyst obtained by combining the yolk-shell type composite molecular sieve of the present invention with Mo and Ni exhibits excellent catalytic hydrogenation activity.

[0013] In a preferred embodiment of the invention, the proportion of Mo oxide in the hydrorefining catalyst is 10-20%, preferably 12-16%, by mass. The proportion of Ni oxide in the hydrorefining catalyst is 2-5%, preferably 3-4%. Such preferred loading amounts are more conducive to improving catalytic performance.

[0014] According to another aspect of the present invention, the application of the above-described hydrorefining catalyst in diesel desulfurization and hydrorefining is also provided.

[0015] In particular, it is used in hydrogenation purification with 4,6-DMDBT as a model compound.

[0016] The macromolecular sulfide 4,6-DMDBT has significant steric hindrance, making it difficult to directly perform deep desulfurization using existing technologies. However, the catalyst of this invention possesses a suitable pore structure, thus effectively eliminating diffusion effects. Furthermore, the catalyst structure can be further optimized, acidity adjusted, and the distribution of the active phase NiMoS-II optimized through the combination of mesoporous and microporous components and the modification of the pore structure by introducing Ni and Mo metals.

[0017] In a preferred embodiment of the present invention, the conditions for applying the catalyst of the present invention to the hydrorefining of 4,6-DMDBT are as follows: temperature 300–400°C, preferably 340–360°C; pressure 4–10 MPa, preferably 4–6 MPa; hydrogen-to-oil ratio 200–600:1, preferably 200–400:1; and liquid hourly space velocity 1–3 h⁻¹. -1 Preferably 1.5 to 2.5 hours -1 .

[0018] In a preferred embodiment of the present invention, the amount of the hydrorefining catalyst of the present invention relative to the catalytic substrate is calculated in a mass ratio of 1:200 to 400, preferably 1:350 to 390.

[0019] According to another aspect of the present invention, a method for preparing the above-mentioned egg yolk shell type composite molecular sieve is also provided, comprising:

[0020] Step S1: The first template agent, silicon source, titanium source, alcohol and water are prepared into a first mixed solution and crystallized to obtain TS-1 molecular sieve precursor emulsion.

[0021] Step S2: Prepare a second mixed solution by mixing the organosilane precursor, the second template agent, the pore-expanding agent, ammonia, and alcohol; the organosilane precursor includes at least one hydrophilic silicon source and at least one hydrophobic silicon source; the mass ratio of the second template agent to the pore-expanding agent is 1 to 0.25, preferably 0.8 to 0.3;

[0022] Step S3: Mix the TS-1 molecular sieve precursor emulsion and the second mixed solution, perform nano-self-assembly, and then perform a first calcination to obtain the egg yolk shell type composite molecular sieve.

[0023] In the preparation method of this invention, suitable reagents were selected, particularly silicon sources with different hydrophilicity / hydrophobicity, as well as appropriate amounts of pore-expanding agents and template agents, so that the obtained eggshell-type composite molecular sieve has a suitable structure. When the amount of pore-expanding agent is too large, the shell thickness and core size of the composite molecular sieve will be greatly reduced, the mechanical strength will be weakened, and the molecular sieve will break and its morphology will change; conversely, a thicker core and shell will be formed, which is not conducive to the free diffusion of macromolecular reactants.

[0024] In a preferred embodiment of the present invention, in step S1, the first template agent comprises tetrapropylammonium hydroxide (TPAOH). In a preferred embodiment of the present invention, in step S1, the silicon source comprises tetraethyl orthosilicate (TEOS) and / or tetramethyl orthosilicate (TMOS). In a preferred embodiment of the present invention, in step S1, the titanium source comprises tetrabutyl titanate (TBOT) and / or titanium tetrachloride (TiCl4). In a preferred embodiment of the present invention, in step S1, the alcohol comprises isopropanol (IPA).

[0025] In a preferred embodiment of the present invention, in step S1, the mass ratio of TPAOH to TEOS is 1.1–1.5:1, preferably 1.2–1.4:1; the mass ratio of IPA to TEOS is 1.1–1.4:1, preferably 1.2–1.3:1. In a preferred embodiment of the present invention, in step S2, the mass ratio of the organosilane precursor to TMB is 1:0.3–1.4, preferably 1:0.5–1.2; the mass ratio of the organosilane precursor to ammonia is 1:0.4–0.5, preferably 1:0.43–0.48; the mass ratio of the organosilane precursor to the alcohol is 1:12–13, preferably 1:12.5–12.8.

[0026] In a preferred embodiment of the present invention, the crystallization treatment is performed at a temperature of 140–180°C, preferably 160–170°C, for a duration of 3–4 days.

[0027] In a preferred embodiment of the present invention, in step S2, the alcohol includes ethanol and / or isopropanol.

[0028] In a preferred embodiment of the present invention, the hydrophilic silicon source includes TEOS and / or TMOS; the hydrophobic silicon source includes 1,2-bis(triethoxysilyl ethane) (BTSE) and / or 1,2-bis(trimethoxysilyl ethane) (BTME).

[0029] In a preferred embodiment of the present invention, the mass ratio of the hydrophilic silicon source to the hydrophobic silicon source is 0.9 to 1.2, preferably 0.94 to 1.0.

[0030] In a preferred embodiment of the present invention, in step S3, the temperature of the first calcination is 450–600°C, preferably 500–550°C, and the time is 4–6 hours. Preferably, before the first calcination, the nano-self-assembled material is washed and dried. More preferably, the washing is performed using an alcohol solvent filtration process to wash the obtained material until it is neutral. More preferably, after washing the nano-self-assembled material, it is incubated in water. Preferably, the incubation temperature is 70°C, the time is 10–14 hours, and the process is carried out under stirring. After incubation, the material is dried, and then the first calcination is performed.

[0031] In the preparation method of the egg yolk shell type composite molecular sieve of the present invention, the sol-gel method is adopted to synthesize the egg yolk shell type structure through water culture, which does not require etching and multiple deposition steps, thus saving the preparation process. Moreover, the obtained egg yolk shell type composite molecular sieve has excellent catalytic performance after being prepared as a catalyst.

[0032] According to another aspect of the present invention, a method for preparing the above-mentioned hydrorefining catalyst is also provided, comprising: loading a Mo precursor solution and a Ni precursor solution onto an eggshell-type composite molecular sieve using an equal-volume impregnation method, and then performing a second calcination treatment to obtain the hydrorefining catalyst. Preferably, the impregnation order of the Mo and Ni precursor solutions is as follows: first, the Mo precursor solution is impregnated, and then the Ni precursor solution is impregnated.

[0033] In a preferred embodiment of the present invention, the temperature of the second calcination is 400-600°C, preferably 500-550°C, and the time is 4-6 hours.

[0034] In a preferred embodiment of the present invention, the precursor solution of Mo includes an ammonium heptamolybdate solution and a sodium molybdate solution; the precursor solution of Ni includes a nickel nitrate solution and a nickel chloride solution. There are no particular requirements regarding the concentration of the precursor solutions.

[0035] This invention employs a nano-self-assembly method to synthesize a mesoporous-microporous composite molecular sieve. This composite material possesses controllable shell and core sizes, excellent pore structure, and a large specific surface area and pore volume, which facilitates uniform loading of active metals and free diffusion of macromolecular reactants. The mesoporous-microporous composite molecular sieve exhibits suitable acidity, altering the metal-support interaction forces and improving the dispersion of active metals, thus benefiting the hydrorefining reaction. The hydrorefining catalyst prepared from this composite molecular sieve demonstrates excellent catalytic performance. Using the catalyst and supporting process technology, the hydrorefining reaction of the macromolecular sulfide 4,6-DMDBT can achieve a desulfurization rate exceeding 98% and a sulfur content below 10 ppm, meeting the requirements of the China VI emission standard. Attached Figure Description

[0036] Figure 1 The image shows the wide-angle XRD pattern of the TS-1-Yolk-Shell SiO2 composite molecular sieve prepared in Example 1.

[0037] Figure 2 The N2- adsorption-desorption isotherm of the TS-1-Yolk-Shell SiO2 composite molecular sieve prepared in Example 1 is shown.

[0038] Figure 3 The pore size distribution of the TS-1-Yolk-Shell SiO2 composite molecular sieve prepared for Example 1 is shown.

[0039] Figure 4 The image shows the transmission electron microscopy (TEM) spectrum of the TS-1-Yolk-Shell SiO2 composite molecular sieve prepared in Example 1.

[0040] Figure 5 This is a high-magnification transmission electron microscope (HRTEM) image of the NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst (sulfided state) prepared in Example 1. Detailed Implementation

[0041] In order to provide a clearer understanding of the technical features, objectives and beneficial effects of the present invention, the technical solution of the present invention will now be described in detail below, but it should not be construed as limiting the scope of implementation of the present invention.

[0042] Unless otherwise specified in the embodiments, the conditions shall be performed under conventional conditions or conditions recommended by the manufacturer. Reagents, instruments, or methods used in the embodiments of this invention whose source is not specified are all commercially available products or obtainable from the applicant.

[0043] Example 1

[0044] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrogenation refining catalyst, the preparation process of which includes the following steps:

[0045] I. Preparation of Egg Yolk Shell Type Composite Molecular Sieves

[0046] Step S1: Under an ice-water bath, TEOS, TPAOH, TBOT, and H2O are mixed in a mass ratio of 17.7:15.2:1:4.4 and stirred continuously until homogeneous. After homogeneous dissolution, the water bath temperature is adjusted to 70℃, and stirring is continued for 3 hours. Then, 48g of isopropanol is added. The resulting solution is crystallized at 170℃ for 4 days to obtain TS-1 molecular sieve precursor emulsion for later use.

[0047] Step S2: At room temperature, add the template agent CTAB and the pore-expanding agent TMB to the ethanol aqueous solution at a mass ratio of 1:1 and stir until homogeneous; add 6.7g of ammonia water dropwise to the above solution and continue stirring for 0.5-1h; slowly add the organosilane precursor (a mixed solution of TEOS and BTSE, m... TEOS / m BTSE =6.7:7.1) Stir for 1-2 hours to obtain a second mixed solution;

[0048] Step S3: Mix the second mixed solution with the aforementioned TS-1 molecular sieve precursor emulsion, controlling the SiO2 / TiO2 molar ratio to be 50, and continue stirring until the mixture is homogeneous; centrifuge the mixed solution and wash it with ethanol filtration, and soak the obtained solid in 1000-1200g of water for incubation, while stirring slowly for 10-12h; stop stirring, wait for the solution to separate into layers, take off the lower layer of solid, dry it at 80℃ for 12h, calcine it at 550℃ for 6h, and then cool it to room temperature to obtain the TS-1-Yolk-Shell SiO2 composite support;

[0049] II. Preparation of Hydrorefining Catalysts

[0050] The catalyst loaded with Mo was prepared by dissolving 0.73 g of ammonium molybdate in deionized water using the equal volume impregnation method. The solution was used to impregnate 4 g of TS-1-Yolk-Shell SiO2 composite support, while the mixture was ultrasonically dispersed for 15 minutes. The catalyst was then dried at 100 °C for 12 h, calcined at 550 °C for 6 h, and cooled to room temperature.

[0051] 0.54 g of nickel nitrate was used to prepare an impregnation solution. Mo / TYS was impregnated with this solution. After impregnation, the mixture was ultrasonically dispersed for 15 minutes, dried at 100 °C for 12 h, and calcined at 550 °C for 6 h to obtain a NiMo supported hydrorefining catalyst, denoted as Cat-1.

[0052] Example 2

[0053] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrogenation refining catalyst, the preparation process of which is the same as that in Example 1, except that the ratio of CTAB to TMB is 0.5, and the catalyst is designated as Cat-2.

[0054] Example 3

[0055] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrogenation refining catalyst, the preparation process of which is the same as that in Example 1, except that the ratio of CTAB to TMB is 0.4, and the catalyst is designated as Cat-3.

[0056] Example 4

[0057] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrogenation refining catalyst, the preparation process of which is the same as that in Example 1, except that the ratio of CTAB to TMB is 0.3, and the catalyst is designated as Cat-4.

[0058] Example 5

[0059] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrogenation refining catalyst, the preparation process of which is the same as that in Example 1, except that the ratio of CTAB to TMB is 0.2, and the catalyst is designated as Cat-5.

[0060] Example 6

[0061] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrogenation refining catalyst, the preparation process of which is the same as that in Example 4, except that the SiO2 / TiO2 molar ratio is 30 and the catalyst is designated as Cat-6.

[0062] Example 7

[0063] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrogenation refining catalyst, the preparation process of which is the same as that in Example 4, except that the SiO2 / TiO2 molar ratio is 40 and the catalyst is designated as Cat-7.

[0064] Example 8

[0065] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrogenation refining catalyst, the preparation process of which is the same as that in Example 4, except that the SiO2 / TiO2 molar ratio is 100 and the catalyst is designated as Cat-8.

[0066] Example 9

[0067] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrogenation refining catalyst, the preparation process of which is the same as that in Example 4, except that the SiO2 / TiO2 molar ratio is 200 and the catalyst is designated as Cat-9.

[0068] Example 10

[0069] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrogenation refining catalyst, the preparation process of which is the same as that in Example 4, except that the SiO2 / TiO2 molar ratio is 400 and the catalyst is designated as Cat-10.

[0070] Comparative Example 1

[0071] The hydrorefining catalyst was prepared according to the method of Example 1, except that commercially available alumina was used as the support in the comparative example. The resulting NiMo / Al2O3 hydrorefining catalyst supported on molybdenum and nickel was designated Cat-11.

[0072] Comparative Example 2

[0073] The hydrorefining catalyst was prepared according to the method of Example 1, except that the comparative example used only TEOS as a single silicon source in step S3. The resulting hydrorefining catalyst supported on molybdenum and nickel was designated Cat-12.

[0074] Comparative Example 3

[0075] The hydrorefining catalyst was prepared according to the method of Example 1, except that the comparative example used only BTSE as a single silicon source in step S3. The resulting hydrorefining catalyst supported on molybdenum and nickel was designated Cat-13.

[0076] Comparative Example 4

[0077] The hydrorefining catalyst was prepared according to the method of Example 1, except that the comparative example only supported metallic nickel. The obtained nickel-supported hydrorefining catalyst was designated Cat-14.

[0078] Comparative Example 5

[0079] The hydrorefining catalyst was prepared according to the method of Example 1, except that the comparative example only supported molybdenum metal. The hydrorefining catalyst with only molybdenum loading was designated Cat-15.

[0080] The TS-1-Yolk-Shell SiO2 material prepared in Example 1 was tested and analyzed, and its wide-angle XRD results are as follows: Figure 1 As shown; its N2- adsorption-desorption isotherm is as follows: Figure 2 As shown; its aperture distribution is as follows Figure 3 As shown; the transmission electron microscopy (TEM) spectrum of the TS-1-Yolk-Shell SiO2 composite molecular sieve prepared in Example 1 is shown below. Figure 4 As shown, its transmission electron microscopy (TEM) spectrum is as follows: Figure 5 As shown.

[0081] From the aperture distribution map ( Figure 3 As can be seen, the composite molecular sieve synthesized in this invention exhibits three peaks at 2.2 nm, 10 nm, and 20–40 nm, respectively. The first peak is attributed to the self-assembly of CTAB; the second peak is attributed to the mesoporous channels formed by the assembly of CTAB micelles and further amplified by the pore-expanding agent TMB; and the third peak originates from the cavity formed by incubation with water. This indicates that the channels of the composite molecular sieve are radially ordered and three-dimensionally open.

[0082] The eggshell-type composite material synthesized in this invention has radially oriented ordered channels that are open and continuous, with openings on the shell surface and radially oriented to the surface of the sphere. Therefore, sulfur-containing compounds can effectively diffuse into or out of the hierarchical porous composite material, thus improving mass transfer capacity.

[0083] like Figure 5As shown, black filamentous stripes are clearly visible, which are the active phase. The NiMoS-II active phase has a high degree of sulfidation and exists in a form with a certain number of stacked layers, exhibiting better catalytic activity. When the proportion of the NiMoS-II active phase is high, it is more conducive to the hydrodesulfurization reaction.

[0084] The specific surface area, pore size, and pore volume of the hydrorefining catalysts prepared in the examples and comparative examples were determined, and the results are shown in Table 1 below.

[0085] As can be seen from the data in Table 1, in the technical solution of the present invention, the preferred SiO2 / TiO2 molar ratio is 100, and the preferred CTAB to TMB mass ratio is 0.3.

[0086] Table 1

[0087] Example <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Pore volume (cm 3 ·g -1 )]]> Aperture (nm) Cat-1 517 0.67 5.6 Cat-2 542 0.79 6.3 Cat-3 560 0.84 6.8 Cat-4 598 1.01 7.3 Cat-5 527 0.85 7.5 Cat-6 514 0.60 6.5 Cat-7 552 0.63 7.1 Cat-8 642 1.21 7.6 Cat-9 537 0.95 8.0 Cat-10 466 0.93 8.3 Cat-11 266 0.74 8.6 Cat-12 357 0.48 4.0 Cat-13 189 0.33 3.2 Cat-14 530 0.73 6.6 Cat-15 527 0.70 6.1

[0088] The shell thickness and core size of the hydrorefining catalysts prepared in the examples and comparative examples were determined, and the results are shown in Table 2 below.

[0089] Table 2

[0090]

[0091]

[0092] As can be seen from the data in Table 2, in the technical solution of this invention, as the mass ratio of CTAB / TMB decreases, that is, as the amount of TMB added increases, the shell thickness and core size of the synthesized eggshell-type hydrorefining catalyst gradually decrease. When the mass ratio of CTAB / TMB is too large, the shell thickness of the hydrorefining catalyst is relatively thick and the core size is relatively large; when the mass ratio of CTAB / TMB is too small, the core of the hydrorefining catalyst tends to disappear.

[0093] When the SiO2 / TiO2 molar ratio of the composite molecular sieve is too low, i.e., when the amount of TS-1 added is too high, the shell thickness increases significantly, while the core size remains almost unchanged. As the SiO2 / TiO2 molar ratio of the composite molecular sieve gradually increases, the shell size decreases, while the core size remains almost unchanged.

[0094] When TEOS is used as the silicon source alone, the synthesized hydrorefining catalyst is a hollow structure with no core; when BTSE is used as the silicon source alone, the synthesized hydrorefining catalyst is a solid sphere.

[0095] Using 4,6-DMDBT as a model compound, the hydrogenation purification reaction conditions were optimized, and the feed conversion, product distribution and yield were investigated. The results are shown in Table 3.

[0096] The reaction raw material is a 4,6-DMDBT-cyclohexane solution with a sulfur content of 500 ppm.

[0097] The specific testing methods for the catalyst are as follows:

[0098] (1) Catalyst loading: 14mL of quartz wool + quartz sand (20-40 mesh) + quartz wool + 1g of refining agent + 6mL of quartz wool + quartz sand;

[0099] (2) Pre-vulcanization process conditions: temperature 340℃, pressure 4MPa, vulcanizing liquid flow rate 3mL / h; stabilize for 4h;

[0100] (3) Evaluation process reaction conditions: reaction temperature 340℃, pressure 4MPa, mass hourly space velocity 1.5h -1 The hydrogen-to-oil ratio is 200:1.

[0101] Table 3

[0102]

[0103]

[0104] As shown in Table 3, the hydrogenation effect of Cat-1 to Cat-10 on 4,6-DMDBT is higher than that of Comparative Examples 1-5 (Cat-11 to Cat-15). Among them, Cat-8 has a desulfurization rate of over 98% for 4,6-DMDBT and a sulfur content of less than 10 ppm in the product.

Claims

1. A hydrorefining catalyst, characterized in that, The support for the hydrorefining catalyst is an egg yolk-shell type composite molecular sieve, on which oxides of Mo and oxides of Ni are loaded. This yolk-shell type composite molecular sieve has a core composed of TS-1 molecular sieve, a shell composed of silica, and a cavity between the core and the shell; the thickness of the shell is 9~26nm; the diameter of the core is 10~51nm; and the size of the cavity is 24~75nm. The total acid amount of the yolk-shell composite molecular sieve is 35-96 µmol·g -1 The L acid amount of the yolk-shell composite molecular sieve is 30-76 µmol·g -1 The B acid amount of the yolk-shell composite molecular sieve is 5-20 µmol·g -1 ; The molar ratio of SiO2 / TiO2 in the egg yolk shell type composite molecular sieve is 30~400; The preparation method of the egg yolk shell type composite molecular sieve includes: Step S1: The first template agent, silicon source, titanium source, alcohol and water are prepared into a first mixed solution and crystallized to obtain TS-1 molecular sieve precursor emulsion. Step S2: Prepare a second mixed solution by mixing the organosilane precursor, the second template agent, the pore-expanding agent, ammonia, and alcohol; the organosilane precursor includes at least one hydrophilic silicon source and at least one hydrophobic silicon source; the mass ratio of the second template agent to the pore-expanding agent is 0.3~1; Step S3: Mix the TS-1 molecular sieve precursor emulsion and the second mixed solution, perform nano-self-assembly, and then perform a first calcination to obtain the egg yolk shell type composite molecular sieve.

2. The hydrorefining catalyst according to claim 1, characterized in that, The specific surface area of the egg yolk shell type composite molecular sieve is 500-700 m 2 ·g -1 The average pore size of the egg yolk shell type composite molecular sieve is 4-9 nm, and the pore volume of the egg yolk shell type composite molecular sieve is 0.5-1.4 cm 3 ·g -1 .

3. The hydrorefining catalyst according to claim 2, characterized in that, The specific surface area of ​​the egg yolk shell-type composite molecular sieve is 520~650m². 2 ·g -1 .

4. The hydrorefining catalyst according to claim 2, characterized in that, The average pore size of the egg yolk shell type composite molecular sieve is 5~8 nm.

5. The hydrorefining catalyst according to claim 2, characterized in that, The pore volume of the egg yolk shell-type composite molecular sieve is 0.6~1.2 cm³. 3 ·g -1 .

6. The hydrorefining catalyst according to claim 1, characterized in that, The total acidity of the egg yolk shell-type composite molecular sieve is 48~84 µmol·g. -1 .

7. The hydrorefining catalyst according to claim 1, characterized in that, The L-acidity of the egg yolk shell-type composite molecular sieve is 40~68 µmol·g. -1 .

8. The hydrorefining catalyst according to claim 1, characterized in that, The Brønsted acid content of the egg yolk shell-type composite molecular sieve is 8~16 µmol·g. -1 .

9. The hydrorefining catalyst according to claim 1, characterized in that, The mass ratio of the second template agent to the pore-expanding agent is 0.3 to 0.

8.

10. The hydrorefining catalyst according to claim 1, characterized in that, The titanium source includes tetrabutyl titanate and / or titanium tetrachloride.

11. The hydrorefining catalyst according to claim 1, characterized in that, By mass percentage, the oxide of Mo accounts for 10-20% of the hydrorefining catalyst; the oxide of Ni accounts for 2-5% of the hydrorefining catalyst.

12. The hydrorefining catalyst according to claim 11, characterized in that, The oxide of Mo accounts for 12-16% of the total mass of the hydrorefining catalyst.

13. The hydrorefining catalyst according to claim 11, characterized in that, The oxide of Ni accounts for 3-4% of the total mass percentage in the hydrorefining catalyst.

14. A method for preparing a hydrorefining catalyst according to any one of claims 1-13, characterized in that, include: Mo precursor solution and Ni precursor solution were loaded onto eggshell-type composite molecular sieves using an equal-volume impregnation method, and then subjected to a second calcination treatment to obtain the hydrogenation refining catalyst.

15. The application of a hydrorefining catalyst according to any one of claims 1-13 in diesel desulfurization and hydrorefining.

16. The application according to claim 15, characterized in that, This includes the application of the aforementioned hydrorefining catalyst in hydrorefining using 4,6-DMDBT as a model compound.

Citation Information

Patent Citations

  • Carrier of hydrofining catalyst, hydrofining catalyst and preparation method of carrier and hydrofining catalyst

    CN113019440A

  • Hierarchical pore monolithic molecular sieve catalyst and preparation method and application thereof

    CN113813990A

  • Ordered mesoporous titanium-aluminum composite oxide coated TS-1 molecular sieve material and preparation method thereof

    CN114669287A