Process for purifying phosphoric acid

By combining ionic liquid-loaded resin with steam fumigation and infrared laser irradiation activation treatment, the problems of insufficient selectivity and recycling performance in the wet phosphoric acid purification process were solved, achieving efficient purification and recovery of phosphoric acid, reducing the MER value, and improving the recovery rate of phosphoric acid and the stability of the resin.

CN118992996BActive Publication Date: 2026-11-20WUHAN UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411009166.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2026-11-20
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

In existing wet phosphoric acid purification processes, liquid-liquid extraction is complex, has poor selectivity, low ion separation efficiency, and the extractant is volatile, leading to difficulties in phase separation and poor circulation performance.

Method used

Phosphoric acid was adsorbed using an ionic liquid-supported resin. The ionic liquid-supported resin was prepared by reacting glycine with chloromethylated polystyrene resin. The resin’s adsorption capacity and selectivity were improved by combining steam fumigation and infrared laser irradiation activation treatment. Phosphoric acid was then desorbed using sulfuric acid.

Benefits of technology

It achieves highly efficient purification of phosphoric acid, with an adsorption capacity of 260 mg/g, a phosphoric acid recovery rate of 90%, and a MER value of less than 1. It avoids emulsification and solvent loss, is environmentally friendly, and has good cycle stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118992996B_ABST
    Figure CN118992996B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of phosphoric acid purification, and particularly relates to a phosphoric acid purification process, which uses ion liquid loaded resin to adsorb and treat phosphoric acid, and comprises the following steps: S1, pretreatment, S2, resin adsorption, and S3, sulfuric acid desorption; the present application uses glycine ion liquid loaded resin to purify and clean crude phosphoric acid, and compared with the traditional liquid-liquid extraction process, the adsorption amount of the phosphoric acid reaches 260 mg / g, the phosphoric acid recovery rate can reach 90%, the MER value of the phosphoric acid after desorption is lower than 1, the emulsification phenomenon can be avoided, the solvent loss is reduced, the environment is friendly, and the recyclability is also good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of phosphoric acid purification technology, specifically to a phosphoric acid purification process. Background Technology

[0002] Phosphorus resource processing mainly includes thermal and wet processes. Among these, the sulfuric acid process in wet phosphoric acid production is simple. It involves acid leaching phosphate rock powder with sulfuric acid, producing phosphoric acid as a liquid phase and calcium sulfate as a byproduct, a solid phase with very low solubility. Crude phosphoric acid can be obtained through simple solid-liquid separation. This process is adaptable to various ores and suitable for large-scale industrial production, making it the mainstream technology in wet phosphoric acid production. Purified phosphoric acid is then extracted from the crude phosphoric acid using organic matter. However, conventional liquid-liquid extraction processes are complex, have poor selectivity, low ion separation efficiency, and are prone to emulsification of the extractant, leading to difficulties in phase separation. Furthermore, the organic reagents are volatile and lost during extraction and back-extraction, resulting in poor recycling performance. Using ionic liquid-supported resins to adsorb phosphorus from wet phosphoric acid avoids these problems associated with liquid-liquid extraction. Studies have shown that ionic liquid-supported resins prepared by chemically grafting glycine with chloromethylated polystyrene resin exhibit good selectivity for phosphate, with phosphorus adsorption exceeding 260 mg / g. Desorption yields purified phosphoric acid with a MER value below 1. Based on this, the purification of wet phosphoric acid using ionic liquid-supported resin is a new process that combines cleanliness and production efficiency.

[0003] Ionic liquid-supported resins are environmentally friendly and exhibit high cycling stability and excellent selectivity. They avoid the volatilization of organic solvents and do not cause turbidity or emulsification of the solution phase. Selectivity can be altered by incorporating ionic liquids with different functional groups, allowing for the design of ionic liquid-supported resins with varying selectivities. Strong chemical bonds form between the ionic liquid and the resin in ionic liquid-supported resins, preventing the loss of ionic liquid during adsorption and desorption processes and ensuring cycling stability. Previous studies have used anionic ionic liquid-supported resins to adsorb vanadium in anionic form, achieving adsorption capacities exceeding 300 mg / g. Desorption with hydrochloric acid yields a desorption rate exceeding 99%, and after 10 cycles, the adsorption capacity remains above 96%, demonstrating excellent selectivity, stability, and cycling performance. Summary of the Invention

[0004] To address the aforementioned problems, this invention provides a phosphoric acid purification process that uses an ionic liquid-supported resin to adsorb phosphoric acid, comprising the following steps:

[0005] S1, Preprocessing

[0006] At 20–30°C, 18–22 g of ionic liquid-loaded resin was added to a 1 cm × 30 cm resin exchange column, and the top of the resin exchange column was stuffed with degreased cotton.

[0007] S2, resin adsorption

[0008] 18–22 mL of crude phosphoric acid was pumped into the resin exchange column at a rate of 0.4–0.6 mL / min. The crude phosphoric acid was adsorbed by the ionic liquid-supported resin. The adsorption was completed when all the crude phosphoric acid was added.

[0009] S3, sulfuric acid desorption

[0010] Continue to pump 8–12 mL of dilute phosphoric acid at a rate of 1–1.5 mL / min to clean the resin exchange column. After cleaning, continue to pump 18–22 mL of sulfuric acid with a concentration of 4.8–5.2 mol / L at a flow rate of 0.4–0.6 mL / min to desorb the phosphorus adsorbed on the ionic liquid-loaded resin. Collect the desorbed solution, which is the desorbed phosphoric acid.

[0011] Note: The purification of phosphoric acid using ionic liquid-supported resin achieves an adsorption capacity of 260 mg / g, a phosphoric acid recovery rate of up to 90%, and a MER value of less than 1 for the desorbed phosphoric acid.

[0012] Furthermore, the ionic liquid-supported resin is synthesized from glycine solution and chloromethylated polystyrene resin at a solid-liquid ratio of 1g:20-60mL;

[0013] Note: The ionic liquid-supported resin synthesized under the above ratio exhibits good adsorption of phosphoric acid and also has a good desorption effect.

[0014] Furthermore, in step S1, the ionic liquid-supported resin is activated.

[0015] The activation treatment method is as follows: Immerse the ionic liquid-loaded resin in anhydrous ethanol and sonicate for 4-6 minutes. After removal, rinse with ultrapure water 3-4 times. Then pour it into a sealable filter chamber. Place the sealable filter chamber horizontally above boiling water at 98-100°C and fumigate with water vapor for 15-20 minutes. Then turn the sealable filter chamber over and continue fumigating for 15-20 minutes. Finally, transfer the sealable filter chamber to a pyridine solution and immerse it for 15-20 minutes. After immersion, pour it out, wash with ultrapure water 2-4 times, and dry until the relative humidity of the ionic liquid-loaded resin is 30-40%RH to obtain the activated ionic liquid-loaded resin.

[0016] The sealable filter chamber is equipped with a filter cloth; the water vapor fumigation rate is 120–180 mL / min, and the steam density is 20–28 μg / cm³. 3During the ultrasonic treatment, the ultrasonic frequency is 60-80 kHz, the temperature is 23-27℃, and the ultrasonic power is 200-300 W; the pyridine solution is composed of pyridine, 0.4-1 mg / L of tetrahydrofuran derivative, and 94-96% ethanol solution in a volume ratio of 1:1:1-3.

[0017] Explanation: Ultrasonic treatment of ionic liquid-loaded resin with anhydrous ethanol can remove organic impurities and surface contaminants from the resin, thereby enhancing its purity and activity and further improving its adsorption of phosphoric acid. Steam fumigation can further open the resin's pore structure, increasing its specific surface area and porosity, thus enhancing its adsorption capacity. At the same time, the heating effect of steam helps the effective loading of pyridine solution. In the interaction between pyridine, tetrahydrofuran derivatives, ethanol, and phosphoric acid, the electronegative atoms such as nitrogen and oxygen in these molecules may form hydrogen bonds with hydrogen atoms in phosphoric acid, further improving the adsorption effect of ionic liquid-loaded resin on phosphoric acid. Ionic liquid-loaded resin exhibits better adsorption performance and structural integrity under the above relative humidity conditions.

[0018] Furthermore, the fumigation process is combined with infrared laser irradiation, which is performed in an alternating intermittent manner and consists of three stages.

[0019] First stage: The wavelength of the infrared laser is 810-850nm. After irradiation for 25-40 seconds, the infrared laser irradiation is stopped for 1-3 minutes.

[0020] Second stage: Adjust the wavelength of the infrared laser to 780-800nm, irradiate for 5-8 seconds, and then stop the infrared laser irradiation for 1-3 minutes.

[0021] Third stage: Adjust the wavelength of the infrared laser to 860-900nm, irradiate for 10-15s, and then stop the infrared laser irradiation for 1-3min.

[0022] Explanation: The first stage of infrared laser can generate a moderate thermal effect, which helps to activate the functional groups on the resin surface and increase the affinity with phosphoric acid. The second stage of infrared laser is used for local rapid heating. The third stage of infrared laser is used to maintain the temperature of the resin surface and maintain adsorption activity. The alternating intermittent irradiation mode allows the resin to recover after infrared laser irradiation, which helps to reduce excessive changes or damage to the resin structure that may be caused by continuous irradiation, thereby ensuring the desorption capacity of the ionic liquid resin.

[0023] Furthermore, the drying method is as follows: first, centrifuge the resin at a speed of 450-550 r / min for 2-4 min to achieve a relative humidity of 60-70% RH; then, allow it to dry naturally at room temperature of 20-25℃ for 1-1.5 h to achieve a relative humidity of 45-55% RH; finally, purge the surface of the ionic liquid-supported resin with dry air at a flow rate of 6-10 m / s at a temperature of 30-35℃ for 10-20 min to obtain an ionic liquid-supported resin with a relative humidity of 30-40% RH.

[0024] Note: Centrifugal drying at an appropriate speed can remove some moisture. At the same time, using a step-by-step drying method can avoid excessive damage to the resin structure and help maintain the resin's adsorption capacity. The natural drying stage at room temperature allows the resin to gradually adapt to the ambient humidity, reducing internal stress and thus improving its overall performance. Under the above humidity conditions, the adsorption of phosphoric acid by the resin is relatively reversible, thereby improving its desorption performance.

[0025] Further, in step S1, the crude phosphoric acid is crude phosphoric acid with a MER < 9 and a mass concentration of 40-50%;

[0026] Note: The initial untreated phosphoric acid is crude phosphoric acid with a mass concentration of 40-50%.

[0027] Further, in step S3, the mass concentration of the dilute phosphoric acid is 10-15%;

[0028] Note: The dilute phosphoric acid at the above mass concentration can wash away the crude phosphoric acid and impurity ions adhering to the column, thereby effectively improving the recovery rate of phosphoric acid.

[0029] Furthermore, the ionic liquid-loaded resin after desorption treatment is recovered and returned to step S2 for recycling;

[0030] Note: The experimental results show that the desorption solution obtained by the phosphoric acid purification process of this invention can still achieve good phosphorus recovery after multiple adsorption cycles, indicating that the process can be recycled multiple times and the adsorption effect is still good.

[0031] Furthermore, the purification effect of phosphoric acid is measured after step S3 by using ICP-OES to determine the concentration of each element in the desorption solution.

[0032] Note: ICP-OES refers to inductively coupled plasma optical emission spectrometry, which can be used for qualitative and quantitative analysis of metallic and some non-metallic elements in various samples. It features high efficiency, stability, high accuracy, and the ability to continuously and rapidly determine multiple elements, including all metallic elements and some non-metallic elements.

[0033] Compared with the prior art, the beneficial effects of the present invention are:

[0034] (1) This invention uses glycine solution and ionic liquid-supported resin to purify crude phosphoric acid. Compared with the traditional liquid-liquid extraction process, it has a high recovery rate, a low MER value, avoids emulsification, reduces solvent loss, is environmentally friendly, and has good recyclability. The traditional liquid-liquid extraction process for phosphoric acid has a low recovery rate and poor selectivity, with a recovery rate of only 60%. The ionic liquid-supported resin prepared in this invention has an adsorption capacity of 260 mg / g for phosphoric acid, a phosphoric acid recovery rate of up to 90%, and a MER value of less than 1 for phosphoric acid after desorption.

[0035] (2) This invention utilizes steam fumigation in conjunction with pyridine solution impregnation to activate ionic liquid resin, giving it more active sites that facilitate the loading of phosphoric acid. The addition of tetrahydrofuran derivatives and ethanol can synergistically swell the resin with pyridine solution. At the same time, pyridine solution itself also has an adsorption effect on phosphoric acid, which can further improve the purification effect of phosphoric acid. Furthermore, under the above environment, it is not easy for the components to form ionic bonds with phosphoric acid, so it will not affect the desorption effect of the resin. The synergistic effect between infrared laser and fumigation treatment can further improve the activation of functional groups on the resin surface, enhance its adsorption activity, and improve the purification effect of phosphoric acid. Attached Figure Description

[0036] Figure 1 This is a process flow diagram of Embodiment 1 of the present invention;

[0037] Figure 2 This is a comparison chart of the phosphoric acid adsorption amounts of Examples 1 to 11 and Comparative Examples 1 to 3 of the present invention;

[0038] Figure 3 This is a comparison chart of phosphorus recovery rates of the primary desorption solutions of Examples 1 to 11 and Comparative Examples 1 to 3 of the present invention;

[0039] Figure 4 This is a comparison chart of the MER values ​​of the desorption solutions of Examples 1 to 11 and Comparative Examples 1 to 3 of the present invention.

[0040] Figure 5 This is a comparison chart of the phosphoric acid adsorption amounts of Examples 1, 12 to 26, and Comparative Examples 4 to 7 of the present invention;

[0041] Figure 6 This is a comparison chart of phosphorus recovery rates of the primary desorption solutions of Examples 1, 12-26, and Comparative Examples 4-7 of the present invention;

[0042] Figure 7This is a comparison chart of the MER values ​​of the desorption solutions of Examples 1, 12 to 26, and Comparative Examples 4 to 7 of the present invention. Detailed Implementation

[0043] To further illustrate the methods and effects of this invention, the technical solution of this invention will be clearly and completely described below in conjunction with experiments.

[0044] Example 1: A phosphoric acid purification process, wherein the purification involves adsorption of phosphoric acid using an ionic liquid-supported resin, comprising the following steps:

[0045] S1, Preprocessing

[0046] At 25℃, 20g of ionic liquid-loaded resin was added to a 1cm×30cm resin exchange column, and the top of the resin exchange column was plugged with degreased cotton. The ionic liquid-loaded resin was synthesized from glycine solution and chloromethylated polystyrene resin at a solid-liquid ratio of 1g:40mL.

[0047] The synthesis method is as follows: chloromethylated polystyrene resin is added to a 15% glycine solution and stirred at 90°C for 10 hours. Then, solid-liquid separation is performed using quantitative medium-speed filter paper to obtain a pre-ionic liquid-loaded resin. Finally, the resin is vacuum dried at 55°C for 4.5 hours to obtain the ionic liquid-loaded resin.

[0048] S2, resin adsorption

[0049] 20 mL of crude phosphoric acid was pumped into the resin exchange column at a rate of 0.5 mL / min. The crude phosphoric acid was adsorbed by the ionic liquid-supported resin. The adsorption was completed when all the crude phosphoric acid was added. The crude phosphoric acid was 45% by mass with a MER of 8.17.

[0050] S3, sulfuric acid desorption

[0051] Continue to pump 10 mL of 13% phosphoric acid at a rate of 1.2 mL / min to clean the resin exchange column. After cleaning, continue to pump 20 mL of 5.0 mol / L sulfuric acid at a flow rate of 0.5 mL / min to desorb the phosphorus adsorbed on the ionic liquid-supported resin. Collect the desorption solution, which is the desorbed phosphoric acid. The purification effect of phosphoric acid is measured by determining the concentration of each element in the desorption solution using ICP-OES. The desorbed ionic liquid-supported resin is recovered and returned to step S2 for recycling.

[0052] Example 2: Unlike Example 1, the ionic liquid-loaded resin was synthesized from glycine solution and chloromethylated polystyrene resin at a solid-liquid ratio of 1g:20mL. The synthesis method was as follows: chloromethylated polystyrene resin was added to a 10% glycine solution according to the above ratio, stirred at 80°C for 12h, and then the solid and liquid were separated by quantitative medium-speed filter paper to obtain the pre-ionic liquid-loaded resin. Finally, it was vacuum dried at 50°C for 5h to obtain the ionic liquid-loaded resin.

[0053] Example 3: Unlike Example 1, the ionic liquid-supported resin was synthesized from glycine solution and chloromethylated polystyrene resin at a solid-liquid ratio of 1g:60mL. The synthesis method was as follows: chloromethylated polystyrene resin was added to a 20% glycine solution according to the above ratio, stirred at 95°C for 8 hours, and then the solid and liquid were separated by quantitative medium-speed filter paper to obtain the pre-ionic liquid-supported resin. Finally, it was vacuum dried at 60°C for 4 hours to obtain the ionic liquid-supported resin.

[0054] Example 4: Unlike Example 1, in step S1, 18g of ionic liquid-loaded resin was added to a 1cm×30cm resin exchange column at 20°C, and degreased cotton was inserted into the upper part of the resin exchange column.

[0055] Example 5: Unlike Example 1, in step S1, 22g of ionic liquid-loaded resin was added to a 1cm×30cm resin exchange column at 30°C, and degreased cotton was inserted into the upper part of the resin exchange column.

[0056] Example 6: Unlike Example 1, 18 mL of crude phosphoric acid was pumped into the resin exchange column at a rate of 0.4 mL / min.

[0057] Example 7: Unlike Example 1, 22 mL of crude phosphoric acid was pumped into the resin exchange column at a rate of 0.6 mL / min.

[0058] Example 8: Unlike Example 1, the resin exchange column was cleaned by pumping 8 mL of 10% phosphoric acid at a rate of 1 mL / min.

[0059] Example 9: Unlike Example 1, the resin exchange column was cleaned by pumping 12 mL of 15% phosphoric acid at a rate of 1.5 mL / min.

[0060] Example 10: Unlike Example 1, after cleaning, 18 mL of 4.8 mol / L sulfuric acid was pumped in at a flow rate of 0.4 mL / min.

[0061] Example 11: Unlike Example 1, after cleaning, 22 mL of 5.2 mol / L sulfuric acid was pumped in at a flow rate of 0.6 mL / min.

[0062] Example 12: Unlike Example 1, in step S1, the ionic liquid-supported resin is activated.

[0063] The activation treatment method is as follows: Immerse the ionic liquid-loaded resin in anhydrous ethanol and sonicate for 5 minutes. After taking it out, rinse it three times with ultrapure water. Then pour it into a sealable filter chamber and place the sealable filter chamber horizontally above boiling water at 99°C. Use water vapor to fumigate for 18 minutes. Then turn the sealable filter chamber over and continue to fumigate for 18 minutes. Finally, transfer the sealable filter chamber to pyridine solution and immerse it for 18 minutes. After immersion, pour it out, wash it three times with ultrapure water, and dry it until the relative humidity of the ionic liquid-loaded resin is 35%RH. The activated ionic liquid-loaded resin is obtained.

[0064] The enclosed filter chamber is equipped with a filter cloth; the steam fumigation rate is 150 mL / min, and the steam density is 24 μg / cm³. 3 During the ultrasonic treatment, the ultrasonic frequency was 70kHz, the temperature was 25℃, and the ultrasonic power was 250W. The pyridine solution was composed of pyridine, 0.6mg / L tetrahydrofuran derivative, and 95% ethanol solution in a volume ratio of 1:1:2. In this embodiment, the tetrahydrofuran derivative was an α-pyrrolidone solution.

[0065] The fumigation process is combined with infrared laser irradiation, which is performed in alternating intermittent stages.

[0066] Phase 1: The wavelength of the infrared laser is 830nm. After irradiation for 30 seconds, the infrared laser irradiation is stopped for 2 minutes.

[0067] Second stage: Adjust the wavelength of the infrared laser to 790nm, irradiate for 6 seconds, and then stop the infrared laser irradiation for 2 minutes.

[0068] Third stage: Adjust the wavelength of the infrared laser to 880nm, irradiate for 13s, and then stop the infrared laser irradiation for 2min.

[0069] The drying method is as follows: First, centrifuge at 500 r / min for 3 min to achieve a relative humidity of 65% RH for the ionic liquid-loaded resin. Then, allow it to dry naturally at room temperature of 22℃ for 1.3 h to achieve a relative humidity of 50% RH. Finally, purge the surface of the ionic liquid-loaded resin with dry air at 33℃ at a flow rate of 8 m / s for 15 min to obtain an ionic liquid-loaded resin with a relative humidity of 35% RH.

[0070] Example 13: Unlike Example 12, the ionic liquid-loaded resin was immersed in anhydrous ethanol and ultrasonically treated for 4 minutes, then rinsed 3 times with ultrapure water.

[0071] Example 14: Unlike Example 12, the ionic liquid-loaded resin was immersed in anhydrous ethanol and sonicated for 6 minutes, then rinsed 4 times with ultrapure water.

[0072] Example 15: Unlike Example 12, the sealable filter chamber was placed horizontally above boiling water at 98°C and fumigated with water vapor for 15 minutes. Then the sealable filter chamber was turned over and fumigated for another 15 minutes.

[0073] Example 16: Unlike Example 12, the sealable filter chamber was placed horizontally above boiling water at 100°C and fumigated with water vapor for 20 minutes. Then the sealable filter chamber was turned over and fumigated for another 20 minutes.

[0074] Example 17: Unlike Example 12, the sealable filter chamber was finally transferred to a pyridine solution for immersion for 15 minutes.

[0075] Example 18: Unlike Example 12, the sealable filter chamber was finally transferred to a pyridine solution for immersion for 20 minutes.

[0076] Example 19: Unlike Example 12, the pyridine solution was composed of pyridine, 0.4 mg / L tetrahydrofuran derivative, and 94% ethanol solution in a volume ratio of 1:1:1.

[0077] Example 20: Unlike Example 12, the pyridine solution was composed of pyridine, 1 mg / L of tetrahydrofuran derivative, and 96% ethanol solution in a volume ratio of 1:1:3.

[0078] Example 21: Unlike Example 12, the steam fumigation rate was 120 mL / min, and the steam density was 20 μg / cm³. 3 .

[0079] Example 22: Unlike Example 12, the steam fumigation rate was 180 mL / min, and the steam density was 28 μg / cm³. 3 .

[0080] Example 23: Unlike Example 12, the ultrasonic frequency during ultrasonic treatment was 60kHz, the temperature was 23℃, and the ultrasonic power was 200W.

[0081] Example 24: Unlike Example 12, the ultrasonic frequency was 80kHz, the temperature was 27℃, and the ultrasonic power was 300W during the ultrasonic treatment.

[0082] Example 25: Unlike Example 12, the drying method is as follows: First, the resin is centrifuged at 450 r / min for 2 min to achieve a relative humidity of 60% RH. Then, it is naturally dried at room temperature of 20°C for 1 h to achieve a relative humidity of 45% RH. Finally, the surface of the resin is purged with dry air at 30°C at a flow rate of 6 m / s for 10 min to obtain an ionic liquid-loaded resin with a relative humidity of 30% RH.

[0083] Example 26: Unlike Example 12, the drying method was as follows: First, the resin was centrifuged at 550 r / min for 4 min to achieve a relative humidity of 70% RH. Then, it was naturally dried at room temperature of 25°C for 1.5 h to achieve a relative humidity of 55% RH. Finally, the surface of the resin was treated with dry air at 35°C at a flow rate of 10 m / s for 20 min to obtain an ionic liquid-supported resin with a relative humidity of 40% RH.

[0084] Experimental Example: The description of this experimental example is based on the scheme described in Example 1, and aims to illustrate the practical application effect of the present invention.

[0085] The method for determining the concentration of each element in the desorption solution using ICP-OES was as follows: The desorption solution was sent to the Materials Research and Testing Center of Wuhan University of Technology for testing, and the results are as follows:

[0086] Table 1. Concentrations of various elements in the primary and secondary desorption solutions obtained from the phosphoric acid purification process in Example 1.

[0087] element P Fe Al Mg MER crude phosphoric acid 138.17g / L 1.82g / L 6.19g / L 6.89g / L 8.17 Primary desorption solution 127.87g / L 0.24g / L 0.26g / L 0.29g / L 0.45 Secondary desorption solution 127.32g / L 0.25g / L 0.25g / L 0.31g / L 0.46

[0088] As shown in Table 1, the phosphorus recovery rate in the primary desorption solution was 92.55%, and the MER value decreased from 8.17 to 0.45. This indicates that the purification of crude phosphoric acid using this process has a higher recovery rate and a lower MER value compared to the traditional liquid-liquid extraction process. It also avoids emulsification, reduces solvent loss, and is environmentally friendly. Furthermore, the data from the secondary desorption solution show that the adsorption of the ionic liquid-supported resin can still reach 99.56% of the original adsorption capacity, and the recovery rate is 92.14%, indicating good recycling performance. The MER value is still relatively low, allowing for multiple recycling cycles.

[0089] 1. Investigate the effects of resin and desorbent on the purification effect of phosphoric acid in the purification process.

[0090] Comparative Example 1: Unlike Example 1, phosphoric acid was replaced with dilute hydrochloric acid.

[0091] Comparative Example 2: Unlike Example 1, phosphoric acid was replaced with water.

[0092] Comparative Example 3: Unlike Example 1, the glycine ionic liquid-supported resin was replaced with an ionic liquid-supported resin prepared from pyridine and N,N-dimethylformamide.

[0093] Conclusion: From Figures 2-4 A comparison of the data from Examples 1 to 11 shows that the changes in parameters within the scope of this application during the phosphoric acid purification process have little impact on the purification effect. Considering adsorption and desorption, MER value, and economic efficiency, Example 1 is selected as the optimal solution. In contrast, Control Examples 1 and 2 used dilute hydrochloric acid or water for desorption, and the desorption effect was not as good as that of sulfuric acid in Example 1. Moreover, the industrial phosphoric acid process is carried out in a sulfuric acid system, and the use of sulfuric acid will not introduce too many other impurities. The ionic liquid-supported resin prepared in Control Example 3 has a high adsorption capacity for phosphorus, reaching 420 mg / g, and better adsorption performance, but poor desorption effect and a high MER value (around 3).

[0094] 2. Investigate the effect of activation treatment methods on the purification effect of phosphoric acid.

[0095] Comparative Example 4: Unlike Example 12, the ionic liquid-loaded resin after rinsing with ultrapure water was directly placed in a heating furnace at a temperature of 99°C for heating treatment.

[0096] Comparative Example 5: Unlike Example 12, the addition of a tetrahydrofuran derivative was absent in the pyridine solution.

[0097] Comparative Example 6: Unlike Example 12, infrared laser irradiation was not performed during the fumigation process.

[0098] Comparative Example 7: Unlike Example 12, the drying method was direct drying at room temperature to a relative humidity of 35% RH.

[0099] Conclusion: From Figures 5-7It can be seen that the activation treatment methods in Examples 12 to 26, compared with Example 1, without activation treatment, do indeed improve the adsorption and desorption capacity of ionic liquid-supported resin for phosphoric acid. Furthermore, the adjustment of the above parameters has little impact on the phosphoric acid adsorption and desorption effect of ionic liquid-supported resin. Considering the overall economic efficiency, Example 12 is selected as the further optimization scheme. Moreover, the comparison between Example 12 and Comparative Example 4 shows that the fumigation activation of ionic liquid-supported resin using water vapor is more effective than direct heating in a heating furnace. This is mainly because water vapor can penetrate and heat the resin more uniformly. Since the diffusion capacity of steam is generally better than that of dry hot air, this uniform heating helps to avoid changes in resin properties caused by local overheating or rapid heating. Steam heating can usually provide a gentler heating rate, which helps to control the polymerization and cross-linking process of the resin, thereby obtaining a resin with better activation effect and further improving the phosphoric acid purification effect.

[0100] The comparison between Example 12 and Comparative Example 5 shows that α-pyrrolidone may act as a hydrophilic additive, helping to improve the hydrophilicity of the resin, making it easier for the resin to contact water vapor, thereby promoting the penetration and adsorption of water vapor. Adding α-pyrrolidone also changes the internal structure of the resin, increasing its swelling capacity, making the resin more likely to expand under the action of water vapor, which helps to increase the resin's loading capacity for phosphoric acid. However, a weakened swelling capacity of the resin may directly affect its loading capacity for glycine ionic liquid, because insufficient swelling will reduce the resin's internal space's ability to accommodate phosphoric acid. At the same time, the lack of α-pyrrolidone as a stabilizer makes the resin more prone to chemical changes during the swelling process, thereby reducing the overall stability. In Comparative Example 6, the lack of infrared laser irradiation during fumigation also weakens the resin activation effect, thus reducing the purification efficiency of phosphoric acid. In Comparative Example 7, direct drying at room temperature to a relative humidity of 35% also weakens the resin's phosphoric acid adsorption and desorption properties. In this solution, by precisely controlling the humidity, the pore structure of the resin can be optimized, thereby increasing its adsorption capacity for phosphoric acid. The staged drying process can reduce the damage to the resin caused by rapid changes in temperature or humidity, extend the service life of the resin, and help maintain the structural stability of the resin, thereby improving its reusability.

Claims

1. A phosphoric acid purification and refining process, characterized in that, The adsorption treatment of phosphoric acid using an ionic liquid-supported resin includes the following steps: S1, Preprocessing At 20~30℃, take 18~22g of ionic liquid-loaded resin and add it into a 1cm×30cm resin exchange column, and stuff the top of the resin exchange column with degreased cotton. The ionic liquid-supported resin is activated by immersing it in anhydrous ethanol and sonicating it for 4-6 minutes. After rinsing it with ultrapure water 3-4 times, the resin is poured into a sealable filter chamber. The sealable filter chamber is placed horizontally above boiling water at 98-100°C and steamed for 15-20 minutes. The sealable filter chamber is then turned over and steamed for another 15-20 minutes. Finally, the sealable filter chamber is transferred to a pyridine solution and immersed for 15-20 minutes. After immersion, the resin is poured out, washed with ultrapure water 2-4 times, and dried until the relative humidity of the ionic liquid-supported resin is 30-40% RH. The activated ionic liquid-supported resin is then obtained. S2, resin adsorption 18-22 mL of crude phosphoric acid was pumped into the resin exchange column at a rate of 0.4-0.6 mL / min. The crude phosphoric acid was adsorbed by the ionic liquid-supported resin. The adsorption was completed when all the crude phosphoric acid was added. The ionic liquid-supported resin was synthesized by glycine solution and chloromethylated polystyrene resin at a solid-liquid ratio of 1 g: 20-60 mL. S3, sulfuric acid desorption Continue to pump 8-12 mL of dilute phosphoric acid at a rate of 1-1.5 mL / min to clean the resin exchange column. After cleaning, continue to pump 18-22 mL of sulfuric acid with a concentration of 4.8-5.2 mol / L at a flow rate of 0.4-0.6 mL / min to desorb the phosphorus adsorbed on the ionic liquid-supported resin. Collect the desorbed solution, which is the desorbed phosphoric acid.

2. The phosphoric acid purification process as described in claim 1, characterized in that, The synthesis method is as follows: chloromethylated polystyrene resin is added to a glycine solution with a mass concentration of 10-20% according to the above proportion, stirred at 80-95℃ for 8-12 hours, and then the solid-liquid separation is performed using quantitative medium-speed filter paper to obtain the pre-ionic liquid-loaded resin. Finally, the resin is vacuum dried at 50-60℃ for 4-5 hours to obtain the ionic liquid-loaded resin.

3. The phosphoric acid purification process as described in claim 1, characterized in that, In step S1, the sealable filter chamber is equipped with a filter cloth; the water vapor fumigation rate is 120~180mL / min, and the steam density is 20~28μg / cm³. 3 During the ultrasonic treatment, the ultrasonic frequency is 60~80kHz, the temperature is 23~27℃, and the ultrasonic power is 200~300W; the pyridine solution is composed of pyridine, 0.4~1mg / L of tetrahydrofuran derivative, and 94~96% ethanol solution in a volume ratio of 1:1:1~3.

4. The phosphoric acid purification process as described in claim 3, characterized in that, The fumigation process is combined with infrared laser irradiation, which is performed in alternating intermittent stages. The first stage: the wavelength of the infrared laser is 810~850nm, and the infrared laser irradiation is stopped 1~3min after irradiation treatment for 25~40s. Second stage: Adjust the wavelength of the infrared laser to 780~800nm, irradiate for 5~8s, and then stop the infrared laser irradiation for 1~3min. Third stage: Adjust the wavelength of the infrared laser to 860~900nm, irradiate for 10~15s, and then stop the infrared laser irradiation for 1~3min.

5. The phosphoric acid purification process as described in claim 3, characterized in that, The drying method is as follows: First, centrifuge the resin at a speed of 450~550 r / min for 2~4 min to achieve a relative humidity of 60~70RH%. Then, allow it to dry naturally at room temperature of 20~25℃ for 1~1.5 h to achieve a relative humidity of 45~55RH. Finally, purge the surface of the ionic liquid-supported resin with dry air at a flow rate of 6~10 m / s and a temperature of 30~35℃ for 10~20 min to obtain an ionic liquid-supported resin with a relative humidity of 30~40RH%.

6. The phosphoric acid purification process as described in claim 1, characterized in that, In step S1, the crude phosphoric acid is crude phosphoric acid with a MER < 9 and a mass concentration of 40-50%.

7. The phosphoric acid purification process as described in claim 1, characterized in that, In step S3, the mass concentration of the dilute phosphoric acid is 10-15%.

8. The phosphoric acid purification process as described in claim 1, characterized in that, The ionic liquid-loaded resin after desorption treatment is recovered and returned to step S2 for recycling.

Citation Information

Patent Citations

  • Method for preparing novel epoxidation catalyst of cyclohexene

    CN102527436A

  • Method for extraction and oxidative desulfurization of fuel oil by solid acid coupled ionic liquid

    CN110229693A