A nickel-nitrogen doped multi-walled carbon nanotube, a preparation method and application thereof, and a modified electrode
By preparing nickel-nitrogen-doped multi-walled carbon nanotubes and modifying the electrode, the problem of simultaneous detection of APAP and DA was solved, the electrochemical activity and chemical stability were improved, and the catalytic performance and anti-interference ability of the electrode were enhanced.
Patent Information
- Application Number
- CN202411112097.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-08-14
AI Technical Summary
Existing technologies are insufficient for the simultaneous detection of two bioactive molecules, acetaminophen (APAP) and dopamine (DA), and also lack sufficient electrochemical activity and chemical stability.
Nickel-nitrogen-doped multi-walled carbon nanotubes were prepared by self-polymerization and thermal decomposition, and then modified onto the electrode surface to improve electrochemical activity and chemical stability through the synergistic effect of nickel and nitrogen.
Simultaneous detection of APAP and DA was achieved, improving electrochemical activity and chemical stability, enhancing the anti-interference ability and repeatability of the modified electrode, and enabling simultaneous catalysis of different substances at different potentials.
Smart Images

Figure CN118993042B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of modified electrode technology, and in particular to a nickel-nitrogen-doped multi-walled carbon nanotube, its preparation method and application, and a modified electrode. Background Technology
[0002] Biologically active molecules such as acetaminophen (APAP) and dopamine (DA) share similar nitrogen-based aromatic structures and play a crucial role in human metabolism. APAP is the world's most widely used analgesic, often used interchangeably with aspirin, and its safety profile is narrow, balancing efficacy with potential toxicity. APAP abuse can lead to liver and kidney toxicity, and may even be fatal. On the other hand, DA plays essential roles in the central nervous system and renal system. It is involved in various daily activities and is closely related to the onset and progression of many diseases. Specifically, irregular DA levels in the body can lead to various neurodegenerative diseases, including schizophrenia and Alzheimer's disease. Therefore, accurate detection of APAP and DA is crucial for neurological and biomedical health diagnosis.
[0003] Currently, various techniques are available for detecting APAP and DA, such as spectrophotometry, chromatography, electrophoresis, chemiluminescence, and electrochemical analysis. Among these methods, electrochemical techniques have become a reliable method for detecting target substances, offering high sensitivity, speed, simplicity, and low cost. However, achieving simultaneous detection of both substances and simultaneously improving their electrochemical activity and chemical stability can be challenging, making the optimization of electrode material structure crucial. Summary of the Invention
[0004] The purpose of this invention is to provide a nickel-nitrogen-doped multi-walled carbon nanotube, its preparation method, applications, and electrode modification. The nickel-nitrogen-doped multi-walled carbon nanotubes prepared by the method can be effectively used for simultaneous detection of APAP and DA, and exhibit high electrochemical activity and chemical stability.
[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0006] The present invention provides a nickel-nitrogen-doped multi-walled carbon nanotube, comprising a multi-walled carbon nanotube and nickel and nitrogen elements doped in the multi-walled carbon nanotube.
[0007] Preferably, the nickel doping amount in the nickel-nitrogen-doped multi-walled carbon nanotubes is 0.5 at.% to 3 at.%, and the nitrogen doping amount is 0.5 at.% to 4 at.%.
[0008] The outer diameter of the nickel-nitrogen-doped multi-walled carbon nanotubes is 5–25 nm.
[0009] This invention also provides a method for preparing nickel-nitrogen-doped multi-walled carbon nanotubes as described in the above technical solution, comprising the following steps:
[0010] A buffer solution of multi-walled carbon nanotubes and dopamine hydrochloride were mixed and subjected to a self-polymerization reaction to obtain polydopamine-coated multi-walled carbon nanotubes.
[0011] The polydopamine-coated multi-walled carbon nanotubes were adsorbed in a soluble nickel salt solution and then thermally decomposed in an argon atmosphere to obtain the nickel-nitrogen-doped multi-walled carbon nanotubes.
[0012] Preferably, the concentration of multi-walled carbon nanotubes in the buffer solution is 0.2–5 mg / mL;
[0013] The solvent in the buffer solution for the multi-walled carbon nanotubes is Tris buffer.
[0014] Preferably, the mass ratio of multi-walled carbon nanotubes to dopamine hydrochloride in the buffer solution of the multi-walled carbon nanotubes is (1-5):(1-5).
[0015] Preferably, the pH of the mixture obtained after mixing is 6 to 11.
[0016] Preferably, the ratio of the polydopamine-coated multi-walled carbon nanotubes to the soluble nickel salt solution is (1-5) mg: (1-5) mL;
[0017] The concentration of the soluble nickel salt solution is 5–20 mol / L.
[0018] Preferably, the annealing temperature is 500–1000°C and the time is 1–5 hours.
[0019] The present invention also provides the application of nickel-nitrogen-doped multi-walled carbon nanotubes described in the above technical solutions or nickel-nitrogen-doped multi-walled carbon nanotubes prepared by the preparation method described in the above technical solutions in the preparation of modified electrodes.
[0020] The present invention also provides a modified electrode, comprising an electrode and nickel-nitrogen-doped multi-walled carbon nanotubes coated on the surface of the electrode;
[0021] The nickel-nitrogen-doped multi-walled carbon nanotubes are the nickel-nitrogen-doped multi-walled carbon nanotubes described in the above technical solution or the nickel-nitrogen-doped multi-walled carbon nanotubes prepared by the preparation method described in the above technical solution.
[0022] This invention provides a nickel-nitrogen-doped multi-walled carbon nanotube (MWC nanotube), comprising MWC nanotubes and nickel and nitrogen elements doped into the MWC nanotubes. Introducing nitrogen atoms into the MWC nanotubes allows the lone pairs of electrons on the nitrogen atoms to combine with the MWC nanotubes, resulting in more site defects and thus improving electrochemical activity and chemical stability. Furthermore, nitrogen doping into the MWC nanotubes can serve as a catalytic substrate for supporting active nanoparticles, adding active sites based on an interwoven network structure, and utilizing the strong activity, stability, and low cost of nickel to further enhance the material's activity. Therefore, this invention uses DA as the unit cell and a soluble nickel salt as the metal source, significantly improving the electrocatalytic activity and conductivity of the material by introducing nickel and nitrogen into the MWC nanotubes. This further improves the anti-interference ability, good repeatability, and stability of the modified electrode. Simultaneously, the nickel-nitrogen-doped MWC nanotubes can achieve simultaneous catalysis of different substances at different potentials, effectively enabling the simultaneous detection of APAP and DA in real samples. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of the preparation process of nickel-nitrogen-doped multi-walled carbon nanotubes in an embodiment of the present invention;
[0024] Figure 2 The results are for detecting 200.0 μM APAP solution and 30.0 μM DA solution using the modified electrodes described in Examples 2-7;
[0025] Figure 3 The images show SEM, TEM, HRTEM-EDS, XRD, and XPS images of the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1.
[0026] Figure 4 The images show SEM images of the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1 at different regions and magnifications.
[0027] Figure 5 The atomic percentage composition of various elements in the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1;
[0028] Figure 6 The Raman spectra of the multi-walled carbon nanotubes described in Example 1, the MWCNTs-PDA described in Example 1, the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1, and the MWCNT-N-PC described in Comparative Example 2, as well as I D and I G The strength ratio;
[0029] Figure 7 XPS full spectrum (a) and C of the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1. 1s High-resolution XPS spectrum (b);
[0030] Figure 8 The MWCNTs-PDA-GCE described in Comparative Example 1, the MWCNT-N-PC-GCE described in Comparative Example 2, the MWCNTs-GCE prepared in Comparative Example 3, and the Ni / NiC described in Example 5 are all examples of MWCNTs-PDA-GCE prepared in Comparative Example 1. X -N-MWCNTs-GCE and bare GCE in a 0.1 MPa solution consisting of 200.0 μM APAP solution and 5.0 mM [Fe(CN)6] containing 0.1 M KCl. 3- / 4- CV curves in solution, and in 0.1 M PB solution composed of 50.0 μM DA solution and 5.0 mM [Fe(CN)6] containing 0.1 M KCl. 3- / 4- CV curve in solution;
[0031] Figure 9 The MWCNTs-PDA-GCE described in Comparative Example 1, the MWCNT-N-PC-GCE described in Comparative Example 2, and the Ni / NiC described in Example 5 are examples of these. X -N-MWCNTs-GCE and naked GCE in 5.0 mM Fe(CN)6 solution containing 0.1 M KCl 3- / 4- EIS diagram in (1:1);
[0032] Figure 10 To use the Ni / NiC described in Example 5 in PB solution (pH 7.0). X CV curves of APAP(a) and DA(b) obtained by the -N-MWCNT-GCE modified electrode at different scan rates; SWV curves of APAP(c) and DA(d) in 0.1M PB at different pH values under Ni / NiCX-N-MWCNTs / GCE; Effect of pH value on oxidation peak current and peak potential of APAP(e) and DA(f);
[0033] Figure 11 The graph shows the linear fit between the peak current of APAP(a) and DA(b) and the square root of the scan rate, and the relationship between the peak potential of APAP(c) and DA(d) and the natural logarithm of the scan rate.
[0034] Figure 12 The current response curves (a) and linear curves (b) of APAP at different concentrations are shown in the system with 50 μM DA; the current response curves (c) and linear curves (d) of DA at different concentrations are shown in the system containing 50.0 μM DA; the Ni / NiC described in Example 5. XCurrent response curves and linear curves of APAP and DA(f) variations on the -N-MWCNT-GCE modified electrode; Ni / NiC as described in Example 5 X The current-it curve (g) of the -N-MWCNT-GCE modified electrode, used for the sequential addition of APAP aminophenol and impurities in PB (impurities ak correspond to APAP, DA, magnesium chloride, copper nitrate, potassium chloride, ferric chloride, sodium sulfate, glucose, L-tyrosine, and glycine, respectively); and the bar charts of reproducibility (h) and repeatability (i) tests. Detailed Implementation
[0035] The present invention provides a nickel-nitrogen-doped multi-walled carbon nanotube, comprising a multi-walled carbon nanotube and nickel and nitrogen elements doped in the multi-walled carbon nanotube.
[0036] In this invention, the nickel doping amount in the nickel-nitrogen-doped multi-walled carbon nanotubes is preferably 0.5 at.% to 3 at.%, more preferably 1.5 at.% to 2.5 at.%, and most preferably 2.07 at.%; the nitrogen doping amount is preferably 0.5 at.% to 4 at.%, more preferably 1 at.% to 2 at.%, and most preferably 1.71 at.%.
[0037] In this invention, the outer diameter of the nickel-nitrogen-doped multi-walled carbon nanotubes is preferably 5-25 nm, more preferably 7-20 nm.
[0038] This invention also provides a method for preparing nickel-nitrogen-doped multi-walled carbon nanotubes as described in the above technical solution, comprising the following steps:
[0039] A buffer solution of multi-walled carbon nanotubes and dopamine hydrochloride were mixed and subjected to a self-polymerization reaction to obtain polydopamine-coated multi-walled carbon nanotubes.
[0040] The polydopamine-coated multi-walled carbon nanotubes were adsorbed in a soluble nickel salt solution and then thermally decomposed in an argon atmosphere to obtain the nickel-nitrogen-doped multi-walled carbon nanotubes.
[0041] In this invention, unless otherwise specified, all raw materials used in the preparation are commercially available products well known to those skilled in the art.
[0042] This invention involves mixing a buffer solution of multi-walled carbon nanotubes with dopamine hydrochloride and performing a self-polymerization reaction to obtain polydopamine-coated multi-walled carbon nanotubes.
[0043] In this invention, the concentration of multi-walled carbon nanotubes in the buffer solution of the multi-walled carbon nanotubes is preferably 0.2-5 mg / mL, more preferably 0.5-2 mg / mL, and most preferably 1 mg / mL; the solvent in the buffer solution of the multi-walled carbon nanotubes is preferably Tris buffer solution.
[0044] In this invention, the mass ratio of the multi-walled carbon nanotubes in the buffer solution to the dopamine hydrochloride is preferably (1-5):(1-5), more preferably (1-2):(1-2), and most preferably 1:1.
[0045] The present invention does not impose any special limitations on the mixing process, and adopts a process well known to those skilled in the art to ensure that the pH of the mixed solution obtained is 6 to 11, more preferably 8 to 9, and most preferably 8.5.
[0046] In this invention, the self-polymerization reaction is preferably carried out under ultrasonic conditions; the frequency of the ultrasound is preferably 20-200 kHz, more preferably 20-80 kHz, and most preferably 40 kHz; the duration of the ultrasound is preferably 5-120 min, more preferably 5-100 min, and most preferably 10 min.
[0047] After the ultrasound is completed, the present invention preferably includes sequential stirring, centrifugation, washing, and drying. In this invention, the stirring temperature is preferably room temperature; the stirring speed is preferably 100–1000 rpm, more preferably 100–500 rpm, and most preferably 200 rpm; the stirring time is preferably 2–10 h, more preferably 3–5 h, and most preferably 4 h. The present invention does not impose any special limitations on the centrifugation, washing, and drying processes; processes well known to those skilled in the art can be used.
[0048] After obtaining the polydopamine-coated multi-walled carbon nanotubes, the present invention adsorbs the polydopamine-coated multi-walled carbon nanotubes in a soluble nickel salt solution and then thermally decomposes them in an argon atmosphere to obtain the nickel-nitrogen-doped multi-walled carbon nanotubes.
[0049] This invention does not impose any particular limitation on the type of soluble nickel salt solution; any type well-known to those skilled in the art can be used. In a specific embodiment of this invention, the soluble nickel salt solution is specifically a nickel chloride solution.
[0050] In this invention, the concentration of the soluble nickel salt solution is preferably 5-20 mmol / L, more preferably 8-12 mmol / L, and most preferably 10.0 mmol / L.
[0051] In this invention, the preferred ratio of the polydopamine-coated multi-walled carbon nanotubes to the soluble nickel salt solution is (1-5) mg:(1-5) mL, more preferably 1 mg:(1-3) mL, and most preferably 1 mg:2 mL.
[0052] In this invention, the adsorption is preferably carried out under stirring conditions. The adsorption time is preferably 3–15 hours, more preferably 6–10 hours, and most preferably 8 hours. This invention does not impose any special limitation on the stirring speed; any speed well-known to those skilled in the art can be used to ensure uniform adsorption of nickel ions on the surface of the multi-walled carbon nanotubes.
[0053] After the adsorption is completed, the present invention preferably includes centrifugation, washing, and drying in sequence. The present invention does not impose any special limitations on the centrifugation and washing processes; any process well-known to those skilled in the art can be used. In the present invention, the drying is preferably vacuum drying; the vacuum drying temperature is preferably 60°C; the present invention does not impose any special limitations on the vacuum drying time; any time well-known to those skilled in the art can be used, ensuring sufficient drying.
[0054] In this invention, the temperature of the thermal decomposition is preferably 500-1000℃, more preferably 700-900℃, and most preferably 800℃; the time is preferably 1-5h, more preferably 1-3h, and most preferably 2h.
[0055] The present invention also provides the application of nickel-nitrogen-doped multi-walled carbon nanotubes described in the above technical solutions or nickel-nitrogen-doped multi-walled carbon nanotubes prepared by the preparation method described in the above technical solutions in the preparation of modified electrodes.
[0056] The present invention also provides a modified electrode, comprising an electrode and nickel-nitrogen-doped multi-walled carbon nanotubes coated on the surface of the electrode;
[0057] The nickel-nitrogen-doped multi-walled carbon nanotubes are the nickel-nitrogen-doped multi-walled carbon nanotubes described in the above technical solution or the nickel-nitrogen-doped multi-walled carbon nanotubes prepared by the preparation method described in the above technical solution.
[0058] In this invention, the method for preparing the modified electrode preferably includes the following steps:
[0059] A nickel-nitrogen-doped multi-walled carbon nanotube suspension was coated onto the surface of the electrode and dried to obtain the modified electrode.
[0060] In this invention, the concentration of the nickel-nitrogen-doped multi-walled carbon nanotube suspension is preferably 0.5 mg·mL. -1 In this invention, the coating amount of the nickel-nitrogen-doped multi-walled carbon nanotube suspension is preferably 4–9 μL.
[0061] The following detailed description, in conjunction with embodiments, illustrates the nickel-nitrogen-doped multi-walled carbon nanotubes provided by the present invention, their preparation methods, applications, and modified electrodes. However, these descriptions should not be construed as limiting the scope of protection of the present invention.
[0062] Example 1
[0063] like Figure 1 As shown, 50.0 mg of dopamine hydrochloride was dissolved in 50.0 mL of Tris buffer containing 50.0 mg of multi-walled carbon nanotubes and the pH was maintained at 8.5. After sonication for 10 min (sonication frequency of 40 kHz), the resulting mixture was stirred at room temperature for 4 h (stirring speed of 200 rpm), and then centrifuged, washed and dried in sequence to obtain polydopamine (PDA) coated multi-walled carbon nanotubes (MWCNTs-PDA).
[0064] 50.0 mg of the MWCNTs-PDA was dispersed in 100 mL of nickel chloride solution (concentration 10.0 mmol / L), and stirred continuously (stirring speed 200 rpm) for 8 h. After centrifugation, washing, and vacuum drying at 60 °C for 12 h, the mixture was annealed at 800 °C for 2 h in an argon atmosphere to obtain nickel-nitrogen-doped multi-walled carbon nanotubes (Ni / NiC). x -N-MWCNTs).
[0065] Examples 2-7
[0066] A glassy carbon electrode (GCE electrode) was polished sequentially with alumina powder with particle sizes of 1.00 μm, 0.30 μm and 0.05 μm, then rinsed with ultrapure water, and then subjected to ultrasonic treatment in anhydrous ethanol and ultrapure water, and dried at room temperature to obtain a pretreated GCE electrode.
[0067] The surface of the pretreated GCE electrode was coated with a nickel-nitrogen-doped multi-walled carbon nanotube suspension (concentration of 0.5 mg·mL⁻¹) as shown in Example 1. -1 The coating amounts were successively 4 μL (Example 2), 5 μL (Example 3), 6 μL (Example 4), 7 μL (Example 5), 8 μL (Example 6), and 9 μL (Example 7), and after drying, modified electrodes (denoted as Ni / NiC) were obtained. X -N-MWCNTs-GCE).
[0068] Comparative Example 1
[0069] 50.0 mg of dopamine hydrochloride was dissolved in 50.0 mL of Tris buffer containing 50.0 mg of multi-walled carbon nanotubes and the pH was maintained at 8.5. After sonication for 10 min (sonication frequency of 40 kHz), the resulting mixture was stirred at room temperature for 4 h (stirring speed of 200 rpm), and then centrifuged, washed and dried to obtain polydopamine (PDA) coated multi-walled carbon nanotubes (MWCNTs-PDA).
[0070] A glassy carbon electrode (GCE electrode) was polished sequentially with alumina powder with particle sizes of 1.00 μm, 0.30 μm and 0.05 μm, then rinsed with ultrapure water, and then subjected to ultrasonic treatment in anhydrous ethanol and ultrapure water, and dried at room temperature to obtain a pretreated GCE electrode.
[0071] The MWCNTs-PDA suspension (concentration of 0.5 mg·mL⁻¹) was coated on the surface of the pretreated GCE electrode. -1 The coating amount was 7 μL, and the electrode was dried to obtain the modified electrode (denoted as MWCNTs-PDA-GCE).
[0072] Comparative Example 2
[0073] Preparation of MWCNT-N-PC-GCE:
[0074] 50.0 mg of dopamine hydrochloride was dissolved in 50.0 mL of Tris buffer containing 50.0 mg of multi-walled carbon nanotubes and the pH was maintained at 8.5. After sonication for 10 min (sonication frequency of 40 kHz), the resulting mixture was stirred at room temperature for 4 h (stirring speed of 200 rpm), and then centrifuged, washed and dried to obtain polydopamine (PDA) coated multi-walled carbon nanotubes (MWCNTs-PDA).
[0075] Then, 50.0 mg of MWCNTs-PDA powder was annealed at 800 °C for 2 hours (argon flow) to form MWCNT-N-PC nanostructures.
[0076] A glassy carbon electrode (GCE electrode) was polished sequentially with alumina powder with particle sizes of 1.00 μm, 0.30 μm and 0.05 μm, then rinsed with ultrapure water, and then subjected to ultrasonic treatment in anhydrous ethanol and ultrapure water, and dried at room temperature to obtain a pretreated GCE electrode.
[0077] The MWCNT-N-PC suspension (concentration of 0.5 mg·mL⁻¹) was coated on the surface of the pretreated GCE electrode. -1 The coating amount was 7 μL, and the electrode was dried to obtain the modified electrode (denoted as MWCNT-N-PC-GCE).
[0078] Comparative Example 3
[0079] Preparation of MWCNTs-GCE:
[0080] A glassy carbon electrode (GCE electrode) was polished sequentially with alumina powder with particle sizes of 1.00 μm, 0.30 μm and 0.05 μm, then rinsed with ultrapure water, and then subjected to ultrasonic treatment in anhydrous ethanol and ultrapure water, and dried at room temperature to obtain a pretreated GCE electrode.
[0081] The MWCNTs suspension (concentration of 0.5 mg·mL⁻¹) was coated on the surface of the pretreated GCE electrode. -1 The coating amount was 7 μL, and the electrode was dried to obtain the modified electrode (denoted as MWCNTs-GCE).
[0082] Test Example 1
[0083] The modified electrodes described in Examples 2-7 were used to detect 200.0 μM APAP solution and 30.0 μM DA solution. The detection results are as follows: Figure 2 As shown, by Figure 2 It can be seen that when the amount of catalyst (nickel-nitrogen-doped multi-walled carbon nanotube suspension) coated is 7 μL (Example 5), the current change is the largest, and the simultaneous detection performance of APAP and DA is the best.
[0084] The modified electrode described in Example 5 was characterized using cyclic voltammetry (CV) and square wave voltammetry (SWV): CV measurements were performed in 10 mL of 0.1 mol / L PB solution (CV measurement conditions were: in 10 mL of 0.1 mol / L PB solution). -1 CV measurements were performed in PB solution; SWV measurements were performed in 0.1 mol / L phosphate buffer solution (PB, pH = 7.0) containing different concentrations of APAP (0, 1, 2, 5, 10, 20, 30, 50, 80, 100, 120, 150 μm), with a potential range of 0.1–0.6 V, and amplitude, frequency, and increment E of 0.025 V, 10 Hz, and 0.004 V, respectively.
[0085] The nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1 were subjected to SEM, TEM, HRTEM-EDS, XRD, and XPS tests. The test results are as follows: Figures 3-4 As shown, Figure 3 In the image, (a) is a SEM image of the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1, (b) is a TEM image of the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1, (c) to (f) are HRTEM-EDS images of the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1, (g) is an XRD pattern of the multi-walled carbon nanotubes described in Example 1, the MWCNTs-PDA described in Example 1, the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1, and the MWCNT-N-PC described in Comparative Example 2, and (h) is an XRD pattern of the N-type multi-walled carbon nanotubes described in Example 2. 1s The high-resolution XPS spectrum of the nickel-nitrogen-doped multi-walled carbon nanotubes, (i) is the Ni 2p High-resolution XPS spectra; Figure 4The images are SEM images of the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1 at different regions and at different magnifications. (a), (d), and (g) are SEM images of the same region at different magnifications, (b), (e), and (h) are SEM images of the same region at different magnifications, and (c), (f), and (i) are SEM images of the same region at different magnifications. Figure 5 The atomic percentage composition of various elements in the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1; by Figures 3-5 It is evident that the nanotubes in the nickel-nitrogen-doped multi-walled carbon nanotubes are interwoven, exhibiting a loose and porous macroscopic morphology. This morphology exposes more active sites, increases the specific surface area, and enhances electrocatalytic activity. Simultaneously, the typical morphology of multi-walled carbon nanotubes exhibits a relatively smooth and flat surface, with carbon nanotubes of different lengths arranged in an alternating pattern. After carbonization with the PDA and nickel source, the surface becomes rough due to the formation of a carbon layer on the surface of the multi-walled carbon nanotubes, while the nanowire array remains intact. TEM images of the nickel-nitrogen-doped multi-walled carbon nanotubes show that nitrogen and nickel are uniformly distributed within the internal structure. HRTEM-EDS elemental mapping confirms the coexistence and uniform distribution of C, N, and Ni elements in the nickel-nitrogen-doped multi-walled carbon nanotubes. The elemental percentages of C, N, and Ni are 96.20%, 1.71%, and 2.07%, respectively. XRD patterns demonstrate that for multi-walled carbon nanotubes, there are predominant hexagonal graphite characteristic diffraction peaks at 25.9° and 44.1°, attributed to the (002) and (101) crystal planes of the multi-walled carbon nanotubes (JCPDS No. 26-1077), respectively. It can also be seen that the hexagonal graphite characteristic peaks are still retained in MWCNTs-PDA and MWCNT-N-PC (Comparative Example 2), with the decrease in peak intensity attributed to the polydopamine coating. Notably, for nickel-nitrogen-doped multi-walled carbon nanotubes, there is an additional characteristic diffraction peak at 44.5°, which points to the (011) plane of Ni (JCPDS No. 45-1027). More specifically, while retaining the characteristic peaks of multi-walled carbon nanotubes, diffraction peaks at 29.4°, 36.1°, 39.9°, 43.2°, and 47.7° can be indexed as NiCx peaks (JCPDS No. 45-0979). Therefore, these results indicate that nickel-nitrogen-doped multi-walled carbon nanotubes have been successfully prepared. Furthermore, Raman spectroscopy was used to reveal the level of graphitization in the carbon-based material. Figure 6 (a) Raman spectra of the multi-walled carbon nanotubes described in Example 1, the MWCNTs-PDA described in Example 1, the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1, and the MWCNT-N-PC described in Comparative Example 2; two characteristic spectral lines with different chemical structures are located at 1360 and 1580 cm⁻¹. -1The vicinity corresponds to the D and G bands, respectively. Compared to multi-walled carbon nanotubes, the higher peak value at D in the nickel-nitrogen-doped multi-walled carbon nanotubes is characterized by a decrease in order and graphitization degree. D and I G The strength ratio indicates the degree of graphitization of carbon materials. Figure 6 In (b), (b) refers to the multi-walled carbon nanotubes described in Example 1, the MWCNTs-PDA described in Example 1, the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1, and the MWCNT-N-PC described in Comparative Example 2. D and I G (strength ratio), obviously, I D / I G The value increased from 1.43 to 1.539, and the nickel-nitrogen-doped multi-walled carbon nanotubes showed more defects and disordered structures, which is beneficial for providing more catalytic active centers; the XRD and EDS results were consistent with the Raman spectroscopy results.
[0086] Figure 7 XPS full spectrum (a) and C of the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1. 1s The high-resolution XPS spectrum (b) is obtained from... Figure 3 (h) and (i) in the middle and Figure 7 It can be seen that the peaks at 844.6, 392.6, and 279.6 eV correspond to Ni 2p, N 1s, and C 1s, respectively, confirming the presence of C, N, and Ni. High-resolution XPS Ni 2p spectroscopy shows a weak peak at 852.7 eV attributed to metallic Ni, and three XPS peaks at 853.5, 854.1, and 855.5 eV attributed to divalent Ni 2p³ / ². The Ni 2p³ / ² peak at 853.5 eV can be attributed to NiCx. Meanwhile, the peaks at 861.8 and 873.5 eV are attributed to Ni, respectively. 2+ and Ni 3+ This also confirms the existence of multivalent Ni carbides, and two weak peaks corresponding to the satellite peaks of metallic Ni were observed at 878.6 and 858.1 eV. Furthermore, characteristic peaks of carbon-carbon double bonds (284.1 eV), N-2p2C (284.6 eV), and N-2p3C (288.3 eV) were observed in the high-resolution deconvolution C1s spectrum; in addition, the deconvolution N1s spectrum showed three peaks at 398.3, 400.4, and 402.9 eV, which are connected to pyridine-type N, pyrrole-type N, and graphitic N, respectively, indicating that N was successfully doped into the carbon material. XPS results show that the nanohybrid contains metallic Ni and NC materials, which further confirms the correctness of the XRD and EDS results.
[0087] Test Example 2
[0088] Cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS) were used to analyze the results of different modified electrodes (MWCNTs-PDA-GCE described in Comparative Example 1, MWCNT-N-PC-GCE described in Comparative Example 2, MWCNTs-GCE prepared in Comparative Example 3, and Ni / NiC described in Example 5). X -N-MWCNTs-GCE and bare GCE) in a 0.1M PB solution consisting of 200.0 μM APAP solution and 50.0 μM DA solution, and 5.0 mM [Fe(CN)6] containing 0.1 M KCl. 3- / 4- The CV curve in the solution, the test results are as follows: Figure 8 As shown, (a) is a 0.1 M PB solution composed of 200.0 μM APAP solution and 5.0 mM [Fe(CN)6] containing 0.1 M KCl. 3- / 4- The CV curves in the solutions, (b) are for a 0.1 M PB solution composed of 50.0 μM DA solution and a 5.0 mM [Fe(CN)6] solution containing 0.1 M KCl. 3- / 4- CV curve in solution; by Figure 8 It can be seen that Ni / NiC X The redox peaks of -N-MWCNTs are significantly higher than those of other electrodes, indicating that they have a more efficient electron transfer capability. Figure 9 The MWCNTs-PDA-GCE described in Comparative Example 1, the MWCNT-N-PC-GCE described in Comparative Example 2, and the Ni / NiC described in Example 5 are examples of these. X -N-MWCNTs-GCE and naked GCE in 5.0 mM Fe(CN)6 solution containing 0.1 M KCl 3- / 4- The EIS plot in (1:1) (frequency range from 100kHz to 0.1Hz, initial voltage of 0.22V, amplitude of 0.005V), is derived from... Figure 9 It can be seen that the EIS spectrum consists of two parts: a high-frequency semicircle representing the confined electron transfer process and a low-frequency linear region representing the diffusion-limited process. In the EIS plot, MWCNTs-N-PC-GCE does not have a clear semicircle in the high-frequency region, indicating high charge transfer resistance. However, in the high-frequency region, there are obvious semicircles of exposed GCE, MWCNTs, and MWCNTs PDA, which are much larger than those of the fitted Ni / NiC. X The Rct value of 75Ω obtained from the -N-MWCNTs equivalent circuit indicates that Ni / NiC X -N-MWCNTs exhibit excellent electrocatalytic behavior;
[0089] Figure 10 To prepare the coating in PB solution (pH 7.0), a coating volume of 7.0 μL (concentration 0.5 mg·mL) was used.-1 Ni / NiC X CV curves of APAP(a) and DA(b) obtained at different scan rates using the -N-MWCNT-GCE modified electrode; SWV curves of APAP(c) and DA(d) in 0.1M PB at different pH values under Ni / NiCX-N-MWCNTs / GCE; the effect of pH value on the oxidation peak current and peak potential of APAP(e) and DA(f); by Figure 10 It was found that when 100.0 μMAPAP or DA was present in PB (pH = 7.0), the CV of the scan rate varied between 5 and 10 mV / s to reflect interface control factors. It was clearly observed that the peak current increased with increasing scan rate, and that the oxidation and reduction peaks shifted slightly towards their respective potentials during this process. The redox peak current showed a linear correlation with the square root of the scan rate (e.g., ...). Figure 11 As shown in (a) and (b) in the figure, and accompanied by the subsequent linear regression equations (as shown in Equations 1 to 4);
[0090] I pa (APAP)(μA)=3.42ν 1 / 2 (mV / s)-6.92(R=0.9989) Formula 1,
[0091] I pc (APAP)(μA)=-2.24ν 1 / 2 (mV / s)+5.04(R=0.9965) Formula 2,
[0092] I pa (DA)(μA)=0.54ν 1 / 2 (mV / s)+0.012(R=0.9964) Formula 3,
[0093] I pc (DA)(μA)=-1.08ν 1 / 2 (mV / s)+1.22(R=0.9978) Formula 4;
[0094] Among them, I pa For peak anode current, I pc ν is the peak cathode current, and v is the scan rate (mV / s).
[0095] The above-described good linearity indicates that the electro-oxidation of APAP or DA on the modified electrode is a representative diffusion-controlled process. The correlation between the peak potential of APAP and DA and the logarithm of the scan rate is shown in the figure. Figure 11 As shown in (c) and (d) in the figure, the linear fitting equation is:
[0096] Epa (APAP)(V)=0.015lnν(mV / s)+0.36(R=0.9996) Equation 5,
[0097] E pc (APAP)(V)=-0.0092lnν(mV / s)+0.38(R=0.9969) Equation 6,
[0098] E pa (DA)(V)=0.013lnν(mV / s)+0.19(R=0.9899) Formula 7,
[0099] E pc (DA)(V)=-0.013lnν(mV / s)+0.18(R=0.9956) Formula 8,
[0100] The electron transfer coefficient (α) and the number of electrons transferred (n) can be calculated using the Lavilon equation as shown in Equations 9-10:
[0101]
[0102] Where R, T, and F represent the molar gas constant, thermodynamic temperature, and Faraday constant, respectively. Based on the slope of Ep with respect to ln, the electro-oxidation n of APAP and DA under Ni / NiCX-n-MWCNTs / GCE can be calculated to be approximately 2, indicating that in Ni / NiC X The electrode processes of APAP and DA on -n-MWCNTs / GCE are reversible, which is consistent with... Figure 10 The CV curves for APAP and DA in (a) and (b) are consistent. Based on this result, we derive the oxidation mechanism of APAP and DA, as shown in Equation 11.
[0103]
[0104] Figure 10 (c) and (d) show the results of square wave stripping voltammetry (SWV) tests conducted in PB solutions with a pH range of 5.0–9.0. The results indicate that the voltage increase was 0.004 V, the amplitude was 0.025 V, and the frequency was 10 Hz. The peak current reached its maximum value at pH 7.0. Figure 10 In the figure, (e) and (f) represent the peak potential and current fitting for pH. From the above results, it can be seen that as pH increases, Ep shifts to a lower potential, indicating that protons participate in the electrochemical reaction. The linear regression equation between Ep and pH is fitted as Equation 12-13:
[0105] Ep(APAP) / V = -0.0532pH + 0.7484 (R = 0.9992) Equation 12,
[0106] Ep(DA) / V = -0.0576pH + 0.5765 (R = 0.9963) Equation 13;
[0107] The absolute values of their slopes (-53.2 mV / pH and -57.6 mV / pH, respectively) are in excellent agreement with the theoretical value of -59 mV / pH, indicating a balance of electrons and protons in the redox reaction. The graph shows that the current initially increases steadily with increasing pH, then decreases, reaching a maximum at pH 7.0. Furthermore, the peak potential decreases with further increases in pH. These results indicate that H+ ions participate in the reactions during the electrochemical determination process.
[0108] Figure 12 The current response curves (a) and linear curves (b) of APAP at different concentrations are shown in the system with 50 μM DA; the current response curves (c) and linear curves (d) of DA at different concentrations are shown in the system containing 50.0 μM DA; the Ni / NiC described in Example 5. X Current response curves and linear curves of APAP and DA(f) variations on the -N-MWCNT-GCE modified electrode; Ni / NiC as described in Example 5 X The current-it curve (g) of the -N-MWCNT-GCE modified electrode, used for the sequential addition of impurities from APAP (aminophenol) and PB (impurities ak correspond to APAP, DA, magnesium chloride, copper nitrate, potassium chloride, ferric chloride, sodium sulfate, glucose, L-tyrosine, and glycine, respectively); reproducibility (h) and repeatability (i) test bar charts; as shown in (a), keeping the concentration of one substance constant and continuously changing the concentration of another substance, when the DA concentration is kept at 50 μmol / L, the peak current of APAP increases linearly with the increase of concentration; as shown in (b), the peak current of APAP is linearly correlated with the concentration in the range of 1–150 μmol / L. The linear regression equation is shown in Equation 14:
[0109] I p (APAP)(μA)=0.2236C / μM+1.1617(R=0.9969) Equation 14;
[0110] As shown in (c) and (d), when APAP is maintained at a certain concentration (1–150 μmol / L), the peak current of DA also shows a linear relationship with the concentration. The regression equation in the range of 0–80 μmol / L is shown in Equation 15:
[0111] I p (DA)(μA)=0.7420C / μM+1.6320(R=0.9928) Equation 15;
[0112] As shown in (e), with the increase of the concentration of the two target molecules (APAP and DA), the peak responses of APAP and DA can be detected simultaneously;
[0113] As shown in (f), the peak responses of APAP and DA in the range of 1–150 μmol / L exhibit a good linear relationship, and the regression equations are shown in Equations 16–17:
[0114] I p (APAP)(μA)=0.2418C / μM-0.2383(R=0.9994) Equation 16
[0115] I p (DA)(μA)=0.7146C / μM+2.6486(R=0.9983) Equation 17;
[0116] The limit of detection (LOD) is derived from the slope (M) of the calibration curve, as shown in Equation 18:
[0117] LOD = 3S / M (Formula 18);
[0118] Where S is the standard deviation of the blank ampere signal, and the detection limits for APAP and DA are 0.56 and 0.19 μmol / L, respectively (S / N = 3). The results show that, compared with some reported sensors for detecting APAP and DA, nickel-nitrogen-doped multi-walled carbon nanotubes exhibit good selectivity for detecting APAP or DA, and perform well in terms of detection range and detection limit.
[0119] As shown in (g), even though the concentrations of interfering substances such as p-aminophenol, dopamine, magnesium chloride, copper nitrate, potassium chloride, ferric chloride, sodium sulfate, glucose, L-tyrosine, and glycine are 100 times higher than those of APAP, the current response remains unchanged after adding these interfering substances every 50 seconds between two APAP additions. This means that the nickel-nitrogen-doped multi-walled carbon nanotube modified electrode has excellent selectivity and anti-interference ability for the trace detection of APAP and DA.
[0120] As shown in (h), the peak current value of the nickel-nitrogen-doped multi-walled carbon nanotube-modified electrode can be maintained at 90.66% of the original peak current value after being stored at room temperature for 7 days, which shows good stability.
[0121] As shown in (i), the relative standard deviation (RSD) of the nickel-nitrogen-doped multi-walled carbon nanotube modified electrode is 2.01%, indicating that the nickel-nitrogen-doped multi-walled carbon nanotube modified electrode has good repeatability.
[0122] In summary, the nickel-nitrogen-doped multi-walled carbon nanotube-modified electrode exhibits excellent stability, repeatability, and selectivity.
[0123] The nickel-nitrogen-doped multi-walled carbon nanotube-modified electrode was used to detect APAP and DA in acetaminophen tablets and dopamine injections, with actual concentrations of 10.0, 20.0, and 50.0 μM, respectively. The experimental results are shown in Table 2: the detected concentrations by the nickel-nitrogen-doped multi-walled carbon nanotube-modified electrode showed little difference from the actual concentrations, with recoveries ranging from 94.85% to 110.20% and relative standard deviations between 1.35% and 4.88%. This indicates that the modified electrode can be effectively used for the simultaneous detection of APAP and DA, and has practical application potential.
[0124] Table 2. Determination of actual APAP and dopamine content in acetaminophen tablets and dopamine injection.
[0125]
[0126]
[0127] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. The application of a modified electrode in the simultaneous detection of acetaminophen and dopamine, characterized in that, The modified electrode includes an electrode and nickel-nitrogen-doped multi-walled carbon nanotubes coated on the surface of the electrode. The nickel-nitrogen-doped multi-walled carbon nanotubes comprise multi-walled carbon nanotubes and nickel and nitrogen elements doped into the multi-walled carbon nanotubes; the nickel doping amount in the nickel-nitrogen-doped multi-walled carbon nanotubes is 0.5 at.%~3 at.%, and the nitrogen doping amount is 0.5 at.%~4 at.%. The method for preparing the nickel-nitrogen-doped multi-walled carbon nanotubes includes the following steps: A buffer solution of multi-walled carbon nanotubes and dopamine hydrochloride were mixed and subjected to a self-polymerization reaction to obtain polydopamine-coated multi-walled carbon nanotubes. The polydopamine-coated multi-walled carbon nanotubes were adsorbed into a soluble nickel salt solution and then thermally decomposed in an argon atmosphere to obtain the nickel-nitrogen-doped multi-walled carbon nanotubes; the soluble nickel salt solution was a nickel chloride solution.
2. The application as described in claim 1, characterized in that, The outer diameter of the nickel-nitrogen-doped multi-walled carbon nanotubes is 5~25 nm.
3. The application as described in claim 1, characterized in that, The concentration of multi-walled carbon nanotubes in the buffer solution is 0.2~5 mg / mL; The solvent in the buffer solution for the multi-walled carbon nanotubes is Tris buffer.
4. The application as described in claim 1, characterized in that, The mass ratio of multi-walled carbon nanotubes to dopamine hydrochloride in the buffer solution of the multi-walled carbon nanotubes is (1~5):(1~5).
5. The application as described in claim 1, characterized in that, The pH of the mixture obtained after mixing is 6~11.
6. The application as described in claim 1, characterized in that, The ratio of the polydopamine-coated multi-walled carbon nanotubes to the soluble nickel salt solution is (1~5) mg: (1~5) mL; The concentration of the soluble nickel salt solution is 5~20 mol / L.
7. The application as described in claim 1, characterized in that, The pyrolysis temperature is 500~1000℃, and the time is 1~5h.