Sulfonic acid group organic polymer, sulfonic acid group organic polymer / carbon nanotube composite material, and preparation method and application of sulfonic acid group organic polymer / carbon nanotube composite material

Through the composite material of sulfonic acid-based organic polymer and carbon nanotubes, the problems of low capacity and poor cycle stability of the positive electrode material of lithium-ion battery are solved, and the high capacity and excellent cycle performance are improved. It is suitable for high-performance lithium-ion batteries. development.

CN118994576AActive Publication Date: 2024-11-22CHANGZHOU UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411091226.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

Traditional lithium-ion battery positive electrode materials have problems such as low capacity, poor cycle stability and environmental pollution, and the low conductivity and poor solubility of organic materials limit their commercial applications.

Method used

The electrochemical performance is improved through specific structural units and composite methods by using sulfonic acid-based organic polymers and their composite materials with carbon nanotubes as the cathode material of lithium-ion batteries.

Benefits of technology

It achieves high specific capacity and excellent cycle stability, improves conductivity and material performance, overcomes the dissolution problem of organic materials, and has broad application prospects for lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994576A_ABST
    Figure CN118994576A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion battery positive electrode materials, and particularly relates to a sulfonic acid group organic polymer, a sulfonic acid group organic polymer / carbon nanotube composite material, and a preparation method and an application of the sulfonic acid group organic polymer / carbon nanotube composite material. The sulfonyl organic polymer is prepared by carrying out dehydration condensation reaction on 2, 5-diaminobenzene sulfonic acid and hexaazabenzene hexacarboxylic acid trianhydride, has relatively high specific capacity and excellent cycling stability when being used as the positive electrode material of the lithium ion battery, and overcomes the problem of dissolution of an organic positive electrode material in an electrolyte. After being compounded with the carbon nanotubes, the sulfonic organic polymer is applied to the positive electrode material of the lithium ion battery, so that the battery performance is remarkably improved, and the capacity is still kept stable after long circulation. The sulfonyl organic polymer and the sulfonyl organic polymer / carbon nanotube composite material are simple in synthesis method, rich in raw material source, good in reproducibility and suitable for industrial production, and have wide application prospects in the field of lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion battery positive electrode materials, and particularly relates to a sulfonic acid organic polymer, a sulfonic acid organic polymer / carbon nanotube composite material, and a preparation method and application thereof. Background Art

[0002] With the increase in industrial activities and the increase in energy consumption and demand, traditional rechargeable batteries are gradually losing their ability to meet current and future market needs. In order to meet this challenge, it is imperative to develop advanced, flexible and controllable energy technologies. At present, there are some safety issues and environmental hazards in lithium-ion batteries, so some alternatives need to be considered. One way to improve the efficiency of energy storage devices is to focus on the development and improvement of their components, such as electrode materials, diaphragms and other components. The positive electrode material plays an important role in the composition of lithium-ion batteries, not only because of its high cost, but also because the positive electrode material plays a key role in battery performance.

[0003] Traditional inorganic materials are not conducive to future green development needs because of their limited reserves in nature and the problem of heavy metal elements polluting the environment. In addition, when such inorganic materials are used as positive electrodes for lithium-ion batteries, their capacity is relatively low. For example, the theoretical specific capacity of LiCoO2 is 274mAh g -1 However, its actual specific capacity is only half of the theoretical capacity. For example, the theoretical capacity of LiMn2O4 is only 147 mAh g -1 . Organic materials are abundant in sources and have less environmental harm in extraction and synthesis processes. In recent years, the use of redox-active organic materials to replace the currently used inorganic materials as lithium-ion battery electrode materials has received increasing attention in the battery field. However, due to the low electrical conductivity of most organic electrode materials and the high solubility of many small molecule organic materials in electrolytes, the overall battery capacity is low and the cycle stability is poor. These factors limit the commercialization of organic lithium-ion batteries. However, research in recent decades has found that some organic positive electrode materials have the advantage of strong functional design, and the performance of the battery can be improved by introducing structural units with specific functions. In 2014, Wang et al. reported a group of sulfonated anthraquinone compounds (AQDS) and studied the effect of the presence or absence of sulfonic acid functional groups on the electrochemical performance of the positive electrode material. Although this material only has 130mAh g at 0.2C, it has a low electrochemical performance. -1 The specific capacity of the material is 2.347 W / m, but it has excellent cycle stability, which indicates that sulfonation modification plays a multifunctional role in solving the dissolution problem of the compound and regulating the lithium storage voltage (RSCA Advances, 2014, 4(38): 19878-19882). In addition, compounding the material with carbon nanotubes can also improve performance. For example, in 2022, Yao et al. TPDA-PMDAThe abundant triangular micropores and hexagonal mesopores in the structure greatly improve the electronic conductivity and mass transfer kinetics. -1 After 1800 cycles at a high current density, the battery still maintained 80 mAh g -1 high capacity and cycling stability (Journal of the American Chemical Society, 2022, 144(51): 23534-23542).

[0004] Therefore, the introduction of specific functional groups and the compounding with materials such as carbon nanotubes are considered to be an effective means to improve the performance of lithium-ion batteries. Therefore, such materials are studied as positive electrode materials for lithium-ion batteries, and it is expected that organic positive electrode materials with high capacity and excellent cycle performance will be discovered, thereby promoting the application and development of high-performance lithium batteries. Summary of the invention

[0005] The purpose of the present invention is to provide a sulfonic acid organic polymer, a sulfonic acid organic polymer / carbon nanotube composite material and a preparation method thereof, and to apply the sulfonic acid organic polymer and the sulfonic acid organic polymer / carbon nanotube composite material to lithium ion battery positive electrode materials.

[0006] The present invention provides a sulfonic acid organic polymer, the structural formula of which is:

[0007]

[0008] Furthermore, the sulfonic acid organic polymer (PSHT-polymer) is produced by the reaction of 2,5-diaminobenzenesulfonic acid and hexaazatriphenylene hexacarboxylic acid trianhydride, and the synthesis reaction equation is as follows:

[0009]

[0010] The specific steps are as follows:

[0011] Add 2,5-diaminobenzenesulfonic acid, hexaazatriphenylene hexacarboxylic acid trianhydride and an organic solvent into a thick-walled reaction bottle, and after fully dissolving and dispersing them evenly, carry out a dehydration condensation reaction by a solvent thermal method. After the reaction is completed, cool to room temperature and filter or centrifuge, wash with deionized water 2-3 times, and vacuum dry to obtain a product, which is a sulfonic acid organic polymer.

[0012] Furthermore, the molar ratio of the 2,5-diaminobenzenesulfonic acid to the hexaazatriphenylene hexacarboxylic acid trianhydride is 1.5:1-1.6:1.

[0013] Furthermore, the organic solvent is N,N-dimethylformamide or 1-methyl-2-pyrrolidone.

[0014] Furthermore, the concentration of the 2,5-diaminobenzenesulfonic acid in the organic solvent is 50-75 mmol / L.

[0015] Furthermore, the dehydration condensation reaction temperature is 120-165° C., and the time is 2-5 days.

[0016] The present invention also provides a sulfonic acid organic polymer / carbon nanotube composite material, which is in-situ composited by the sulfonic acid organic polymer and the carbon nanotubes, and the mass ratio of the sulfonic acid organic polymer to the carbon nanotubes is 1:1-3:1.

[0017] Furthermore, the preparation method of the sulfonic acid organic polymer / carbon nanotube composite material comprises the following steps: after uniformly mixing an organic solvent, hexaazatriphenylene hexacarboxylic acid trianhydride, carbon nanotubes and 2,5-diaminobenzenesulfonic acid, carrying out a dehydration condensation reaction by a solvent thermal method, after the reaction is completed and cooled to room temperature, filtering or centrifuging, washing and drying to obtain the sulfonic acid organic polymer / carbon nanotube composite material.

[0018] Furthermore, the molar ratio of 2,5-diaminobenzenesulfonic acid to hexaazatriphenylene hexacarboxylic acid trianhydride is 1.5:1-1.6:1;

[0019] The concentration of the 2,5-diaminobenzenesulfonic acid in the organic solvent is 50-75 mmol / L;

[0020] The organic solvent is N,N-dimethylformamide or 1-methyl-2-pyrrolidone.

[0021] The present invention also provides the use of the above-mentioned sulfonic acid organic polymer and sulfonic acid organic polymer / carbon nanotube composite material in a lithium ion battery positive electrode material, and the specific steps are:

[0022] The electrode sheet prepared by sulfonic acid organic polymer or sulfonic acid organic polymer / carbon nanotube composite material was used as the positive electrode, lithium foil was used as the negative electrode, porous polypropylene was used as the separator, and 1.0 mol L -1 LiTFSI and 1wt% LiNO3 were dissolved in DME (dimethoxyethane) and DOL (1,3-dioxolane) in a volume ratio of 1:1 as the electrolyte and assembled into a button cell;

[0023] The electrode sheet prepared from the sulfonic acid organic polymer or the sulfonic acid organic polymer / carbon nanotube composite material is prepared by mixing and grinding the sulfonic acid organic polymer or the sulfonic acid organic polymer / carbon nanotube composite material, a battery conductive agent, and an adhesive in a mass ratio of 30:60:10-60:30:10, adding a proper amount of a dispersant (such as 1-methyl-2-pyrrolidone), grinding it again, uniformly coating it on a current collector aluminum sheet, and vacuum drying it to form an electrode sheet.

[0024] Compared with the prior art, the present invention has the following characteristics:

[0025] The sulfonic acid organic polymer of the present invention has a simple synthesis process, is easy to operate, has low cost, is easy to obtain raw materials, has good reproducibility, and has excellent performance. When used as a positive electrode material for lithium ion batteries, it has a high specific capacity and excellent cycle stability. The sulfonic acid organic polymer has a high specific capacity and excellent cycle stability at 0.05Ag -1 156.2mAh g -1 The initial discharge capacity is 0.1A g -1 After 1000 cycles, it still retains 83.3mAh g -1 The capacity retention rate reaches 71.3%, showing excellent cycle stability.

[0026] The present invention obtains a sulfonic acid organic polymer / carbon nanotube composite material by compounding a sulfonic acid organic polymer with carbon nanotubes. The performance of the sulfonic acid organic polymer is significantly improved. -1 Under this condition, the capacity is increased to 216.3mAh g -1 Even at high current (2Ag -1 ) has a capacity increase of nearly 20 mAh g compared to sulfonic acid organic polymers. -1 . And after a long cycle, the capacity remains stable. The sulfonic acid organic polymer / carbon nanotube composite material of the present invention not only overcomes the dissolution problem of organic positive electrode materials in electrolytes, but also improves the conductivity and performance of the material by compounding with carbon nanotubes, and also has high stability. As a new type of lithium battery positive electrode material, the sulfonic acid organic polymer / carbon nanotube composite material of the present invention has high discharge specific capacity, long-term cycle stability, and good rate performance, and has broad application prospects in the field of lithium ion battery electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is the structural formula diagram of the material PSHT-polymer;

[0028] Figure 2 is the H NMR spectrum of the material PSHT-polymer;

[0029] Figure 3 is the C NMR spectrum of the material PSHT-polymer;

[0030] Figure 4 is the infrared spectrum of the material PSHT-polymer;

[0031] Figure 5 is the Raman spectrum of the material PSHT-polymer;

[0032] Figure 6is the thermogravimetric curve of the material PSHT-polymer;

[0033] Figure 7 It is the nitrogen adsorption-desorption and pore size distribution curve of the material PSHT-polymer;

[0034] Figure 8 The cyclic voltammograms of PSHT-polymer button cells at different scan rates;

[0035] Fig. 9 This is the rate performance diagram of the material PSHT-polymer button battery;

[0036] Fig.10 This is the charge and discharge curve of the PSHT-polymer button battery at different current densities;

[0037] Fig.11 PSHT-polymer button cell at 0.1Ag -1 Cycling stability diagram at different current densities;

[0038] Fig.12 This is the AC impedance diagram of the material PSHT-polymer button battery;

[0039] Fig.13 This is the infrared spectrum of the material PSHT-polymer / carbon nanotube;

[0040] Fig.14 Thermogravimetric curve of the material PSHT-polymer / carbon nanotube;

[0041] Fig.15 It is the nitrogen adsorption-desorption and pore size distribution curve of the material PSHT-polymer / carbon nanotube;

[0042] Fig.16 0.1 mV s for PSHT-polymer / carbon nanotube button cell -1 Cyclic voltammogram at scan rate;

[0043] Fig.17 This is the rate performance diagram of the PSHT-polymer / carbon nanotube button cell;

[0044] Fig.18 The charge and discharge curves of the material PSHT-polymer / carbon nanotube at different current densities;

[0045] Fig.19 PSHT-polymer / carbon nanotube button cell at 0.1A g -1 Cycling stability plot at different current densities. DETAILED DESCRIPTION

[0046] The present invention will be further described below by means of specific examples.

[0047] Example 1

[0048] Add 30 mL of N,N-dimethylformamide (DMF) to a 48 mL thick-walled reaction bottle, and add 2,5-diaminobenzenesulfonic acid (2.25 mmol, 0.423 g) and hexaazatriphenylene hexacarboxylic acid trianhydride (purchased from McLean, 1.5 mmol 0.6663 g) at the same time. After sufficient dissolution and dispersion, the thick-walled reaction bottle is vacuum-treated and kept warm at 125°C for 4 days. After the reaction is completed, wash it with deionized water 3 times, filter or centrifuge to collect the solid, and vacuum dry it at 100°C for 12 hours to obtain a sulfonic acid-based organic polymer material, namely PSHT-polymer, with a yield of 71%.

[0049] PSHT-polymer was used as the active material of the positive electrode material, and was mixed with acetylene black (Ningbo Veken Battery Co., Ltd.) and a binder (PVDF) in a certain proportion. PSHT-polymer: acetylene black: binder (PVDF) = 30%: 60%: 10% (mass ratio). After the three were mixed and ground for 2 hours, an appropriate amount of 1-methyl-2-pyrrolidone (NMP) was added and ground again for 0.5 hours. Then, the mixture was evenly coated on an aluminum foil sheet with an area of ​​1×1 cm, and vacuum dried at 80°C overnight to form an electrode sheet. The electrode sheet was used as the positive electrode, the lithium sheet as the negative electrode, porous polypropylene (PP, Hangzhou Chuangwei Rubber & Plastic Technology Co., Ltd., the same below) as the separator, and 1.0 mol L -1 LiTFSI and 1wt% LiNO3 were dissolved in DME (dimethoxyethane) and DOL (1,3-dioxolane) in a volume ratio of 1:1 as the electrolyte, assembled into a button cell, and its electrochemical performance was investigated. Figure 8 Cyclic voltammograms of button cells at different scan rates; Fig. 9 This is the rate performance diagram of button cell; Fig.10 The charge and discharge curves of button batteries at different current densities are shown in Figure 2. -1 The capacity can reach 140.8mAh g -1 , in 2Ag -1 The capacity is still 56.1mAh g -1 ; Fig.11 This is the cycle stability diagram of the button battery, and the capacity retention rate is 71.3%.

[0050] Example 2

[0051] 30 mL of N,N-dimethylformamide (DMF) was added to a 48 mL thick-walled reaction bottle, and 2,5-diaminobenzenesulfonic acid (2.25 mmol, 0.423 g), hexaazatriphenylene hexacarboxylic acid trianhydride (purchased from McLean, 1.5 mmol 0.6663 g), and carbon nanotubes (0.31 g) were added at the same time. After sufficient mixing and dispersion, the thick-walled reaction bottle was vacuum treated and kept at 125°C for 4 days. After the reaction was completed, it was washed with deionized water 3 times, and the solid was collected by suction filtration or centrifugation. It was vacuum dried at 100°C for 12 hours to obtain a sulfonic acid organic polymer / carbon nanotube material, namely PSHT-polymer / carbon nanotube, sulfonic acid organic polymer: carbon nanotube = 2:1 (mass ratio), and the yield was 75%.

[0052] The method of assembling button-type batteries using PSHT-polymer / carbon nanotubes as the active material of the positive electrode material is the same as in Example 1, that is, the PSHT-polymer is replaced by PSHT-polymer / carbon nanotubes, the electrode sheet preparation and battery preparation methods are exactly the same as in Example 1, and their electrochemical properties are examined.

[0053] Fig.16 0.1 mV s for PSHT-polymer / carbon nanotube button cell -1 Cyclic voltammogram at scan rate; Fig.17 The rate performance diagram of PSHT-polymer / carbon nanotube button cell is shown in Figure 2. -1 The capacity can reach 216.3mAh g -1 , at 2A g -1 The capacity is still 74.4mAh g -1 When the current density returns to 0.05 and 0.1 A g -1 The capacities recovered to 198.6 and 176.1 mAh g -1 , Fig.18 The charge and discharge curves of the material PSHT-polymer / carbon nanotube at different current densities; Fig.19 PSHT-polymer / carbon nanotube button cell at 0.05A g -1 Cycling stability diagram under current density. After 240 cycles, the capacity retention rate is close to 99.9%.

[0054] Example 3

[0055] The experimental method is the same as that of Example 1, except that the reaction conditions are changed from 125° C. for 4 days to 140° C. for 3 days, and the material PSHT-polymer is obtained with a yield of 70%.

[0056] Example 4

[0057] The experimental method was the same as that in Example 2, except that the reaction conditions were changed from 125° C. for 4 days to 140° C. for 3 days, to obtain the material PSHT-polymer / carbon nanotubes with a yield of 74%.

[0058] Example 5

[0059] The experimental method is the same as that of Example 2, except that the reaction conditions of sulfonic acid organic polymer: carbon nanotube = 2:1 (mass ratio) are changed to sulfonic acid organic polymer: carbon nanotube = 1:1 (mass ratio), and the material PSHT-polymer / carbon nanotube is obtained with a yield of 73%.

[0060] Example 6

[0061] The experimental method is the same as that of Example 2, except that the reaction conditions of sulfonic acid organic polymer: carbon nanotube = 2:1 (mass ratio) are changed to sulfonic acid organic polymer: carbon nanotube = 3:2 (mass ratio), and the material PSHT-polymer / carbon nanotube is obtained with a yield of 74%.

[0062] Example 7

[0063] The experimental method was the same as that of Example 1, except that the reaction conditions were changed from adding 30 mL of N,N-dimethylformamide (DMF) to adding 30 mL of 1-methyl-2-pyrrolidone (NMP), and the material PSHT-polymer was obtained with a yield of 69%.

[0064] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A sulfonic acid organic polymer, characterized in that The structural formula of the sulfonic acid organic polymer is as follows:

2. The method for preparing a sulfonic acid organic polymer according to claim 1, characterized in that: The method comprises the following steps: uniformly mixing an organic solvent, hexaazatriphenylene hexacarboxylic acid trianhydride and 2,5-diaminobenzenesulfonic acid, carrying out a dehydration condensation reaction by a solvent thermal method, cooling to room temperature after the reaction is completed, filtering or centrifuging, washing and drying to obtain a sulfonic acid organic polymer material.

3. The method for preparing a sulfonic acid organic polymer according to claim 2, characterized in that: The molar ratio of 2,5-diaminobenzenesulfonic acid to hexaazatriphenylene hexacarboxylic acid trianhydride is 1.5:1-1.6:1; The concentration of the 2,5-diaminobenzenesulfonic acid in the organic solvent is 50-75 mmol / L; The organic solvent is N,N-dimethylformamide or 1-methyl-2-pyrrolidone.

4. The method for preparing a sulfonic acid organic polymer according to claim 2, characterized in that: The reaction temperature of the dehydration condensation reaction is 120-165° C. and the reaction time is 2-5 days.

5. Use of the sulfonic acid organic polymer as claimed in claim 1 in positive electrode materials for lithium ion batteries.

6. A sulfonic acid organic polymer / carbon nanotube composite material, characterized in that: The sulfonic acid organic polymer / carbon nanotube composite material is formed by in-situ compounding of the sulfonic acid organic polymer according to claim 1 and carbon nanotubes, and the mass ratio of the sulfonic acid organic polymer to the carbon nanotubes is 1:1-3:

1.

7. The method for preparing the sulfonic acid organic polymer / carbon nanotube composite material according to claim 6, characterized in that: The method comprises the following steps: uniformly mixing an organic solvent, hexaazatriphenylene hexacarboxylic acid trianhydride, carbon nanotubes and 2,5-diaminobenzenesulfonic acid, carrying out a dehydration condensation reaction by a solvent thermal method, cooling to room temperature after the reaction is completed, filtering or centrifuging, washing and drying to obtain a sulfonic acid organic polymer / carbon nanotube composite material.

8. The method for preparing the sulfonic acid organic polymer / carbon nanotube composite material according to claim 7, characterized in that: The molar ratio of 2,5-diaminobenzenesulfonic acid to hexaazatriphenylene hexacarboxylic acid trianhydride is 1.5:1-1.6:1; The concentration of the 2,5-diaminobenzenesulfonic acid in the organic solvent is 50-75 mmol / L; The organic solvent is N,N-dimethylformamide or 1-methyl-2-pyrrolidone.

9. The method for preparing the sulfonic acid organic polymer / carbon nanotube composite material according to claim 7, characterized in that: The reaction temperature of the dehydration condensation reaction is 120-165° C. and the reaction time is 2-5 days.

10. Use of the sulfonic acid organic polymer / carbon nanotube composite material as claimed in claim 6 in positive electrode materials for lithium ion batteries.

Citation Information

Patent Citations

  • Sulfonated polyimide binder, electrode plate and lithium ion battery

    CN111777984A

  • Branched cross-linked polyamide acid solution, polyimide adhesive as well as preparation method and application of branched cross-linked polyamide acid solution and polyimide adhesive

    CN114805804A

  • Polycarbonyl hexaaza-naphthalene derivative type COF material as well as preparation method and application thereof

    CN114976297A

  • Polycarbonyl hexaazabenzophenanthrene derivative type COF for water-based zinc ion battery positive electrode material and preparation method of polycarbonyl hexaazabenzophenanthrene derivative type COF

    CN116425974A

  • Multi-active-site nitrogen-containing heterocyclic covalent organic framework material as well as preparation method and application thereof

    CN116925355A