Substrate slice processing method
Through grinding, chamfering treatment, chemical mechanical polishing and aqueous ammonia solution corrosion, the surface defects and roughness problems of the substrate sheet are solved, and the pass rate and processing efficiency of the substrate sheet are improved.
Patent Information
- Application Number
- CN202410945569.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-22
AI Technical Summary
During the processing of existing substrate sheets, the surface is prone to many defects and the roughness does not meet the requirements, resulting in a low pass rate and additional time and expenses to improve.
Using the steps of grinding, chamfering treatment, chemical mechanical polishing and aqueous ammonia solution corrosion, the composition and concentration of the abrasive liquid and polishing liquid are controlled to ensure surface quality by cleaning by sodium hypochlorite polishing liquid and methanol or ethylene glycol.
Effectively reduce surface defects, improve the quality of surface roughness, improve the pass rate of substrate sheet, reduce subsequent improvement costs, and improve processing efficiency.
Smart Images

Figure CN119008377A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of wafer processing, and specifically relates to a substrate processing method. Background Art
[0002] Cadmium zinc telluride crystal is a new type of ternary compound semiconductor. Due to its excellent performance, it has high resistivity, large bandgap (with the change of zinc doping content, the bandgap changes continuously from 1.4eV to 2.26eV), and has very good resolution for X-rays and gamma rays. It can be used in various detectors and other equipment in the fields of astronomy, medicine, and military. At the same time, because its structure is very compatible with mercury cadmium telluride (MCT), it is the best substrate material for MCT.
[0003] Currently, substrates are usually surface treated by chemical mechanical polishing. However, after chemical mechanical polishing, it is still easy for the substrate to have many surface defects and the roughness does not meet the requirements, resulting in a low pass rate of the substrate. At the same time, in order to improve the surface defects of the substrate, a lot of time and additional costs are required, resulting in relatively low benefits. Summary of the invention
[0004] The technical problem to be solved by the present application is that in the existing substrate sheet processing process, the substrate sheet surface is prone to many surface defects and the roughness does not meet the requirements. A substrate sheet processing method is provided that can reduce surface defects and ensure that the surface roughness meets the requirements.
[0005] The technical solution proposed in this application is: A substrate processing method comprises the steps of: S110, grinding the upper and lower surfaces of the substrate sheet; S120, performing chamfering processing on the edge of each of the upper and lower surfaces of the substrate sheet; S130, performing chemical mechanical polishing on the upper and lower surfaces of the substrate; S140, chemically etching the substrate sheet using an ammonia solution; Wherein, the mass concentration of the ammonia solution is 2.2~3.3%.
[0006] Furthermore, in step S140, the chemical etching time is 10 to 20 seconds.
[0007] Furthermore, the substrate sheet processing method further comprises the steps of: S150, cleaning the substrate sheet.
[0008] Furthermore, in step S150, the substrate is cleaned with a methanol solution or an ethylene glycol solution.
[0009] Furthermore, in step S150, the substrate sheet is cleaned 5 to 8 times.
[0010] Furthermore, in step S110, the substrate sheet is ground using a grinding disc and a grinding liquid.
[0011] Furthermore, the volume ratio of abrasive to pure water in the grinding liquid is 2-5:8-12, the abrasive is one of aluminum oxide and diamond, and the particle size is 3-5 μm.
[0012] Further, in step S130, polishing is performed using a sodium hypochlorite polishing liquid.
[0013] Furthermore, the abrasive in the sodium hypochlorite polishing liquid is cerium oxide, and the particle size of the cerium oxide is 0.1-0.3 μm.
[0014] The above substrate processing method is adopted to remove mechanical damage and defects on the surface of the substrate during the grinding process through chemical mechanical polishing, reduce scratches, pits and orange peel on the surface of the substrate, and then chemically corrode the substrate with an ammonia solution to remove the damage layer generated during the chemical mechanical polishing process and the residual stress on the surface, so that the surface is free of scratches, pits and orange peel, improve the problem of many surface defects of the substrate, ensure that the surface roughness of the substrate meets the requirements, and improve the qualified rate of the substrate. At the same time, there is no need to spend a lot of time and extra costs to improve the surface later, which increases the economic benefits of substrate processing. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The accompanying drawings are used to provide further understanding of the present application and constitute a part of the specification. They are used to explain the present application together with the embodiments of the present application and do not constitute a limitation of the present application.
[0016] Figure 1 A flow chart of a substrate processing method provided in one embodiment of the present application; Figure 2 is a surface morphology image of the substrate sheet obtained in Example 1 under bright field; Figure 3 is the surface roughness value of the substrate sheet obtained in Example 1; Figure 4 is the surface roughness value of the substrate sheet obtained in Example 2; Figure 5 is the surface roughness value of the substrate sheet obtained in Example 3; Figure 6 is the surface roughness value of the substrate sheet obtained in Comparative Example 1; Figure 7 is the surface roughness value of the substrate sheet obtained in Comparative Example 2; Figure 8is the surface roughness value of the substrate sheet obtained in Comparative Example 3. DETAILED DESCRIPTION
[0017] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0018] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicating orientations or positional relationships are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0019] The present application provides a substrate sheet processing method, which is applied to the processing of cadmium zinc telluride substrate sheets to reduce surface defects of the substrate sheets, ensure that the surface roughness and VVT of the substrate sheets can meet the requirements, thereby improving the qualified rate of the substrate sheets and improving the economic benefits of substrate sheet processing.
[0020] like Figure 1 As shown, the processing method of the substrate sheet specifically includes the steps of: S110, grinding the upper and lower surfaces of the substrate sheet.
[0021] Specifically, the substrate sheet is ground with a grinding disc and a grinding liquid for 20 to 30 minutes to grind the substrate sheet to a thickness of 1000 μm ± 10 μm. During the grinding process, the grinding pressure is 100 to 120 g / cm 2 , the grinding speed is 25~30rpm, and the flow rate of the grinding liquid is 10~15ml / min.
[0022] Optionally, the grinding disc is a grooved glass disc. In addition, the volume ratio of abrasive to pure water in the grinding liquid is 2-5:8-12, the abrasive is at least one of aluminum oxide and diamond, and the particle size of the abrasive is 3-5 μm.
[0023] S120, chamfering the edges of each of the upper and lower surfaces of the substrate to prevent chipping and breaking of the edges of the substrate during the subsequent chemical mechanical polishing process, thereby avoiding a large number of scratches, pits and other defects on the surface of the substrate and reducing surface defects.
[0024] Specifically, the substrate sheet is placed on a chamfering machine platform and then subjected to a 45° chamfering process.
[0025] During the chamfering process, the grinding line speed is 600~800m / min, the chamfering time is 5~10s, and the chamfering amount is 0.1~0.2mm.
[0026] S130, chemical mechanical polishing is performed on the upper and lower surfaces of the substrate sheet to remove mechanical damage and defects on the surface of the substrate sheet during the grinding process, thereby reducing scratches, pits and orange peel on the surface of the substrate sheet.
[0027] Specifically, the polishing is performed using a sodium hypochlorite polishing liquid, wherein cerium oxide is used as an abrasive in the sodium hypochlorite polishing liquid, and the particle size of the cerium oxide is 0.1-0.3 μm.
[0028] During the chemical mechanical polishing process, a black flannel polishing pad is used with a polishing pressure of 50-80 g / cm 2 , the polishing speed is 30~40rpm, the polishing liquid flow rate is 8~12ml / min. In addition, the chemical mechanical polishing time is 30~60min.
[0029] S140, chemically etching the substrate sheet with an ammonia solution to further remove surface defects, and at the same time remove the damage layer generated during the chemical mechanical polishing process and the residual stress on the surface, so that the surface is free of scratches, pits and orange peel.
[0030] Specifically, the chemical etching time is 10 to 20 seconds. In addition, the mass concentration of the ammonia solution is 2.2 to 3.3%, preferably 3%.
[0031] S150, cleaning the substrate to remove the residual ammonia solution and impurities.
[0032] Specifically, the substrate sheet is cleaned with a methanol solution or an ethylene glycol solution. In addition, the substrate sheet is cleaned 5 to 8 times to ensure that the residual substances on the surface of the substrate sheet are removed.
[0033] The above substrate processing method is adopted to remove mechanical damage and defects on the surface of the substrate during the grinding process through chemical mechanical polishing, reduce scratches, pits and orange peel on the surface of the substrate, and then chemically corrode the substrate with an ammonia solution to remove the damage layer generated during the chemical mechanical polishing process and the residual stress on the surface, so that the surface is free of scratches, pits and orange peel, improve the problem of many surface defects of the substrate, ensure that the surface roughness of the substrate meets the requirements, and improve the qualified rate of the substrate. At the same time, there is no need to spend a lot of time and extra costs to improve the surface later, which increases the economic benefits of substrate processing.
[0034] In order to facilitate understanding of the technical effects brought about by the technical solution of the present application, several embodiments and comparative examples are provided below for illustration: Example 1 First, a grooved glass disc is used as a grinding disc to grind the surface of the substrate at a grinding pressure of 100 g / cm 2 The grinding speed is 25 rpm, the grinding liquid flow rate is 10 ml / min, the abrasive in the grinding liquid is 3 μm aluminum oxide, and the volume ratio of the abrasive to pure water is 2:9.
[0035] After grinding, the substrate sheet was placed on the platform of the chamfering machine, and then chamfered at 45° with a grinding line speed of 600 m / min, a chamfering time of 6 s, and a chamfering amount of 0.1 mm.
[0036] After chamfering, the upper and lower surfaces of the substrate were chemically mechanically polished using an automatic polishing machine. The chemical mechanical polishing time was 50 min and the polishing pressure was 50 g / cm 2 The polishing speed is 30 rpm. The polishing liquid is sodium hypochlorite polishing liquid, the flow rate of the polishing liquid is 8 ml / min, and the abrasive in the polishing liquid is 0.3 μm cerium oxide.
[0037] After the chemical mechanical polishing, the substrate was chemically etched with an ammonia solution with a mass concentration of 2.2% for 10 seconds. After the etching, the substrate was cleaned 5 times with a methanol solution to obtain a finished substrate. Figure 2 and Figure 3 shown.
[0038] Example 2 First, a grooved glass disc was used as a grinding disc to grind the surface of the substrate at a grinding pressure of 110 g / cm 2 The grinding speed is 28 rpm, the grinding liquid flow rate is 12 ml / min, the abrasive in the grinding liquid is 5 μm aluminum oxide, and the volume ratio of the abrasive to pure water is 3:10.
[0039] After grinding, the substrate sheet was placed on the platform of the chamfering machine, and then chamfered at 45° with a grinding line speed of 700 m / min, a chamfering time of 8 s, and a chamfering amount of 0.15 mm.
[0040] After chamfering, the upper and lower surfaces of the substrate were chemically mechanically polished using an automatic polishing machine. The chemical mechanical polishing time was 30 min and the polishing pressure was 70 g / cm 2 The polishing speed is 40 rpm. The polishing liquid is sodium hypochlorite polishing liquid, the flow rate of the polishing liquid is 10 ml / min, and the abrasive in the polishing liquid is 0.1 μm cerium oxide.
[0041] After the chemical mechanical polishing, the substrate was chemically etched with a 3% ammonia solution for 10 seconds. After the etching, the substrate was cleaned 6 times with ethylene glycol solution to obtain a finished substrate. Figure 4 shown.
[0042] Example 3 First, a grooved glass disc was used as a grinding disc to grind the surface of the substrate at a grinding pressure of 120 g / cm 2 The grinding speed is 30 rpm, the grinding liquid flow rate is 15 ml / min, the abrasive in the grinding liquid is 4 μm aluminum oxide, and the volume ratio of the abrasive to pure water is 4:12.
[0043] After grinding, the substrate sheet was placed on the platform of the chamfering machine, and then chamfered at 45° with a grinding line speed of 800 m / min, a chamfering time of 10 s, and a chamfering amount of 0.2 mm.
[0044] After chamfering, the upper and lower surfaces of the substrate were chemically mechanically polished using an automatic polishing machine. The chemical mechanical polishing time was 40 min and the polishing pressure was 60 g / cm 2 The polishing speed is 35 rpm. The polishing liquid is sodium hypochlorite polishing liquid, the flow rate of the polishing liquid is 12 ml / min, and the abrasive in the polishing liquid is 0.2 μm cerium oxide.
[0045] After the chemical mechanical polishing, the substrate was chemically etched with an ammonia solution with a mass concentration of 3.3% for 10 seconds. After the etching, the substrate was cleaned 6 times with an ethylene glycol solution to obtain a finished substrate. Figure 5 shown.
[0046] Comparative Example 1 This comparative example is basically the same as Example 1, except that 1.4% ammonia solution and 70% hydrogen peroxide solution were used for etching. Figure 6 shown.
[0047] Comparative Example 2 This comparative example is basically the same as Example 2, except that an ammonia solution with a mass concentration of 3.8% is used for etching. Figure 7 shown.
[0048] Comparative Example 3 This comparative example is basically the same as Example 1, except that an ammonia solution with a mass concentration of 25% is used for etching. Figure 8shown.
[0049] The finished substrate sheets in the above embodiments and comparative examples were tested, and the test results are shown in the following table: The finished substrate sheets in Example 1 and Example 2 have no scratches, polishing mist and etch pits on the surface, and there are no pits, orange peel and scratches under bright field 100 / 200 / 500 times observation, and the surface roughness value is also less than 1nm; the finished substrate sheets in Comparative Examples 1 to 3 have scratches, polishing mist and etch pits, and there are pits, orange peel and scratches under bright field 100 / 200 / 500 times observation, and the surface roughness value is also 2nm or 3nm. It can be seen that the substrate sheet processing method provided by the present application can effectively remove the surface defects of the substrate sheet, improve the qualified rate of the substrate sheet and the economic benefits of the substrate sheet processing.
[0050] Although the embodiments of the present application have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A substrate sheet processing method, It is characterized in that Includes steps: S110, grinding the upper and lower surfaces of the substrate sheet; S120, performing chamfering processing on the edge of each of the upper and lower surfaces of the substrate sheet; S130, performing chemical mechanical polishing on the upper and lower surfaces of the substrate; S140, chemically etching the substrate sheet using an ammonia solution; Wherein, the mass concentration of the ammonia solution is 2.2~3.3%.
2. The substrate sheet processing method according to claim 1, It is characterized in that In step S140, the chemical etching time is 10-20 seconds.
3. The substrate processing method according to claim 1, It is characterized in that The substrate sheet processing method further comprises the steps of: S150, cleaning the substrate sheet.
4. The substrate sheet processing method according to claim 3, It is characterized in that In step S150, the substrate is cleaned with a methanol solution or an ethylene glycol solution.
5. The substrate processing method according to claim 3, It is characterized in that In step S150, the substrate sheet is cleaned 5 to 8 times.
6. The substrate sheet processing method according to claim 1, It is characterized in that In step S110, the substrate sheet is ground using a grinding disk and a grinding liquid.
7. The substrate sheet processing method according to claim 6, It is characterized in that The volume ratio of abrasive to pure water in the grinding liquid is 2-5:8-12; the abrasive is at least one of aluminum oxide and diamond; and the particle size of the abrasive is 3-5 μm.
8. The substrate sheet processing method according to claim 1, It is characterized in that In step S130, polishing is performed using a sodium hypochlorite polishing liquid.
9. The substrate sheet processing method according to claim 8, It is characterized in that The abrasive in the sodium hypochlorite polishing liquid is cerium oxide; the particle size of the cerium oxide is 0.1-0.3 μm.
Citation Information
Cited By
Method for finely regulating and controlling macroscopic damage and sub-damage on surface of indium arsenide substrate
CN121083498A