Substrate coating composition
A base coating composition with specific composition and physical property parameters, including acrylic resin, polyester resin and melamine resin, achieves efficient curing at low temperature, improves the mechanical properties of the coating film, solves the problem of insufficient mechanical properties of coating films in the prior art, and is suitable for vehicle body coating.
Patent Information
- Application Number
- CN202380034068.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-21
- Filing Date
- 2023-04-18
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-04-18
AI Technical Summary
When existing base coating compositions are cured at low temperatures, the mechanical properties of the coating film are insufficient, making it difficult to meet the requirements of vehicle body coating.
By using a combination of acrylic resin, polyester resin and melamine resin within a specific range, and by adjusting physical properties such as hydroxyl value and weight-average molecular weight, a crosslinking reaction is achieved at low temperature, thereby improving the mechanical properties of the coating film.
Curing at temperatures below 130℃ significantly improves the gloss, impact resistance, water resistance, and other mechanical properties of the coating, making it suitable for use as a car body coating and reducing coating process costs.
Smart Images

Figure BDA0005083156980000111 
Figure BDA0005083156980000121 
Figure BDA0005083156980000122
Abstract
Description
Technical Field
[0001] This invention relates to a substrate coating composition. Background Technology
[0002] Generally, the exterior body panels should not exhibit coating deterioration or rust, and should possess the durability to maintain the coating's gloss or color. Therefore, in terms of vehicle painting processes, the typical procedure involves electroplating the pre-treated body, followed by an intermediate (primer) coat to improve adhesion and smoothness, and then a base coat on the intermediate-coated body to enhance the body's aesthetics. Subsequently, a clear coat is applied to protect the base coat's color, improve its appearance, and protect it from external influences.
[0003] In the application of base coatings and clear coats, typically, after the base coating composition is applied and dried, the clear coat composition is applied, and both the clear coat and base coating are cured together during the curing of the clear coat. Therefore, existing base coating compositions are designed based on high-temperature curing conditions. However, in order to reduce coating process costs, there is an increasing demand for compositions that can shorten the process and cure at low temperatures. In this regard, Korean Patent No. 10-0158534 (Patent Document 1) discloses a two-component acrylic polyurethane composition, which consists of additives, a main mixture containing alcohol solvents, and a curing agent mixture containing polyisocyanate and ester solvents. The additives consist of acrylic polyols, ester solvents, smoothing agents, slip agents, and waxes. However, as shown in Patent Document 1, although existing base coating compositions that can be used under low-temperature baking conditions, especially under heat curing conditions below 130°C, include coatings for automotive repair and compositions for parts coating, the mechanical properties of the prepared coating film are insufficient, limiting its applicability as a body paint.
[0004] Therefore, there is a need to research and develop a base coating composition that can be cured at low temperatures below 130°C, while the resulting coating film has excellent mechanical properties and is suitable for use as a vehicle body coating.
[0005] [Existing Technical Documents]
[0006] (Patent Document 1) Korean Patent No. 10-0158534 (August 5, 1998) Summary of the Invention
[0007] Technical issues
[0008] The present invention aims to provide a base coating composition that can be cured at a low temperature below 130°C while producing a coating film with excellent mechanical properties.
[0009] Problem Solving Methods
[0010] In one embodiment, the present invention provides a base coating composition comprising an acrylic resin, a polyester resin, and a melamine resin, wherein the acrylic resin has a hydroxyl value of 70 to 85 mg KOH / g and a weight-average molecular weight of 40,000 to 50,000 g / mol, and the polyester resin has an acid value of 10 to 30 mg KOH / g and a hydroxyl value of 250 to 300 mg KOH / g.
[0011] Invention Effects
[0012] According to the present invention, a base coating composition allows for a low-temperature process of less than 130°C, which is lower than the temperature of the prior art, in terms of the thermosetting temperature of the coating process. This saves on the costs required for the coating process and is very economical. Moreover, the coating film prepared by the composition exhibits excellent mechanical properties, especially gloss, impact resistance, water resistance, and cold crack resistance, making it advantageous for use as a vehicle body coating. Detailed Implementation
[0013] The present invention will now be described in detail.
[0014] In this specification, "weight-average molecular weight (Mw)" and "number-average molecular weight (Mn)" are measured by methods commonly known in the art to which this invention pertains, such as gel permeation chromatography (GPC).
[0015] In this specification, the "glass transition temperature (Tg)" is measured by a method commonly known in the art to which this invention pertains, such as differential scanning calorimetry (DSC).
[0016] In this specification, functional group values such as "acid value (Av)" and "hydroxyl value (OHv)" are measured by methods commonly known in the art to which this invention pertains, such as titration.
[0017] According to one embodiment of the present invention, a base coating composition is provided, comprising an acrylic resin, a polyester resin, and a melamine resin, wherein the acrylic resin has a hydroxyl value of 70 to 85 mg KOH / g and a weight-average molecular weight of 40,000 to 50,000 g / mol, and the polyester resin has an acid value of 10 to 30 mg KOH / g and a hydroxyl value of 250 to 300 mg KOH / g.
[0018] As described above, when using acrylic resins with a specific range of hydroxyl values and weight-average molecular weights, by adjusting the curing reaction rate and crosslinking density with fast-reactive melamine resins, not only can the appearance characteristics of the coating be improved, but also the mechanical properties such as impact resistance and water resistance can be improved, and it can be cured at low temperatures below 130°C.
[0019] For example, fast-reactive melamine resin containing imino groups can undergo a cross-linking reaction with acrylic resin based on the hydroxyl value, thereby allowing curing at low temperatures below 130°C. A specific range of weight-average molecular weights can improve the mechanical properties of the prepared coating, such as durability.
[0020] Furthermore, when using polyester resins with specific ranges of acid and hydroxyl values, the surface tension can be adjusted during the curing reaction of fast-reacting melamine resin and acrylic resin, thereby improving the smoothness of the coating film and forming a soft coating film, which has the effect of improving mechanical properties such as crack resistance and scratch resistance.
[0021] <Acrylic resin>
[0022] Acrylic resin, as the main resin (primary resin) of the base coating composition according to the present invention, has the function of improving the appearance properties of the prepared coating film, such as durability and gloss.
[0023] Acrylic resins can be synthesized directly using known methods or are commercially available products. Acrylic resins can be prepared by polymerizing, for example, one or more of a first vinyl monomer and a first (meth)acrylate monomer.
[0024] As the first vinyl monomer, one or more may be selected from, for example, styrene, methylstyrene, dimethylstyrene, fluorostyrene, ethoxystyrene, methoxystyrene, phenyl vinyl ketone, tert-butylbenzoate, vinyl cyclohexanoate, vinyl acetate, vinylpyrrolidone, vinyl chloride, vinyl alcohol, acetoxystyrene, tert-butylstyrene, and vinyltoluene.
[0025] The first (meth)acrylate monomer may comprise one or more selected from the group consisting of (meth)acrylate monomers without hydroxyl groups and (meth)acrylate monomers with hydroxyl groups.
[0026] The (meth)acrylate monomer, which does not contain a hydroxyl group, may contain one or more of the following: for example, (meth)acrylic acid, meth(meth)acrylic acid, (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isooctyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecanyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, isobornyl (meth)acrylate, and lauryl (meth)acrylate.
[0027] The hydroxyl-containing (meth)acrylate monomer can be, for example, a hydroxyalkyl-containing (meth)acrylate, specifically, it can include one or more selected from the group consisting of 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate and 2-hydroxybutyl (meth)acrylate.
[0028] Acrylic resins can be prepared by, for example, free radical polymerization, and their properties can be adjusted according to the initiator and polymerization time. That is, the weight-average molecular weight (Mw), hydroxyl value (OHv), acid value (Av), and other properties can be adjusted.
[0029] The solids content (NV) of the acrylic resin relative to the total weight of the resin can be 40 to 60% by weight or 45 to 55% by weight. When the solids content of the acrylic resin is within the range described, the storage stability of the resin and the substrate coating composition is improved, and the workability is excellent. If the solids content of the acrylic resin is less than the range described, the viscosity becomes too low, resulting in poor workability of the substrate coating composition containing it. If it exceeds the range described, the viscosity of the acrylic resin becomes too high, leading to reduced stability during the reaction, poor dispersion stability, and potentially agglomeration over time.
[0030] The viscosity of acrylic resin at 25°C can be 450 to 650 cps or 470 to 630 cps. When the viscosity of acrylic resin at 25°C is within this range, the appropriate viscosity of the base coating composition improves workability. If the viscosity of acrylic resin at 25°C is below this range, the low viscosity of the composition results in an under-formed coating, leading to poor paint flowability, adhesion, and scratch resistance. When the viscosity exceeds this range, insufficient workability of the composition may result in a reduction in the appearance properties of the prepared coating.
[0031] The acid value (Av) of the acrylic resin can be 10 to 30 mg KOH / g or 15 to 25 mg KOH / g. When the acid value of the acrylic resin is within this range, the reactivity of the composition containing it can be adjusted, thereby improving the appearance properties of the resulting coating. If the acid value of the acrylic resin is below this range, the curing reaction rate is slow, resulting in a deterioration in the appearance of the prepared coating. If it exceeds this range, the viscosity of the composition increases with the increased cohesiveness of the resin, potentially leading to reduced workability and room temperature storage properties.
[0032] The hydroxyl value (OHv) of the acrylic resin can be 70 to 85 mg KOH / g or 75 to 80 mg KOH / g. When the hydroxyl value of the acrylic resin is within this range, it improves the durability and weather resistance of the coating film. If the hydroxyl value of the acrylic resin is below this range, the coating film formed through the crosslinking reaction with the curing agent is insufficient, resulting in a decrease in the mechanical properties of the coating film, such as hardness. If it exceeds this range, over-curing occurs, causing the coating film to become brittle, thus reducing elasticity and potentially leading to insufficient appearance characteristics of the prepared coating film.
[0033] The glass transition temperature (Tg) of acrylic resin can be 20 to 40°C or 25 to 35°C. When the glass transition temperature of acrylic resin is within this range, it improves the hardness and solvent resistance of the coating film. If the glass transition temperature of the acrylic resin is below this range, the drying speed and crosslinking density of the coating film decrease, resulting in insufficient hardness and solvent resistance. When it exceeds this range, the coating film becomes brittle, leading to insufficient appearance and crack resistance.
[0034] The weight-average molecular weight (Mw) of acrylic resins can be 40,000 to 50,000 g / mol or 42,000 to 44,000 g / mol. When the weight-average molecular weight of the acrylic resin is within the specified range, the prepared coating film can exhibit excellent long-term physical properties such as durability and weather resistance. If the weight-average molecular weight of the acrylic resin is less than the specified range, the weather resistance and scratch resistance of the prepared coating film will be insufficient due to the low molecular weight. If it exceeds the specified range, the fluidity will decrease with the increase of molecular weight, resulting in poor workability of the substrate coating composition containing it and poor surface smoothness, which may lead to problems in preparing coating films with excellent appearance.
[0035] Based on the total weight of the base coating composition, the composition may include acrylic resin in an amount of 22 to 33% by weight or 24 to 30% by weight. When the included acrylic resin is within the stated range, it improves the adhesion and durability of the coating film. If the acrylic resin content is less than the stated range, the coating film's adhesion, gloss, and durability are reduced due to poor drying properties. If the content exceeds the stated range, rapid drying may result in insufficient paint workability and flowability, reducing the coating film's appearance and scratch resistance.
[0036] <Polyester Resin>
[0037] Polyester resins have the function of imparting flexibility to the base coating composition, increasing the crosslinking density, and improving the mechanical properties of the prepared coating film, such as cold crack resistance, impact resistance, and scratch resistance.
[0038] Polyester resins can be prepared by reacting carboxylic acid compounds with diol compounds. For example, polyester resins can be prepared by reacting one or more carboxylic acid compounds selected from acetic acid (AA), isophthalic acid (IPA), trimellitic anhydride (TMA), alicyclic acids, phthalic anhydride, isophthalic acid, terephthalic acid, succinic acid, adipic acid, fumaric acid, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride and their derivatives with one or more diol compounds selected from 1,6-hexanediol (1,6-HD), neopentyl glycol (NPG), trimethylolpropane (TMP), ethylene glycol, propylene glycol, diethylene glycol, butanediol, 1,4-hexanediol and 3-methylpentanediol.
[0039] Polyester resins can be prepared by the condensation reaction of acids and alcohols. The physical properties can be adjusted according to the ratio of acid to alcohol, that is, the weight-average molecular weight (Mw), hydroxyl value (OHv), acid value (Av), and other physical properties can be adjusted.
[0040] The solids content (NV) of the polyester resin relative to the total weight of the resin can be 60 to 70% by weight or 63 to 67% by weight. When the solids content of the polyester resin is within the range described, it improves the storage stability of the resin and the substrate coating composition, resulting in excellent workability. If the solids content of the polyester resin is below the range described, the viscosity becomes too low, leading to poor workability of the substrate coating composition containing it. If it exceeds the range described, the viscosity of the polyester resin becomes too high, resulting in reduced stability during the reaction, poor dispersion stability, and potentially agglomeration over time.
[0041] The viscosity of the polyester resin at 25°C can be 800 to 1800 cps or 850 to 1780 cps. When the viscosity of the polyester resin at 25°C is within this range, the appropriate viscosity of the base coating composition improves workability. If the viscosity of the polyester resin at 25°C is below this range, the low viscosity of the composition results in an under-formed coating, leading to poor paint flowability, adhesion, and scratch resistance. When the viscosity exceeds this range, the workability of the composition is insufficient, potentially causing a reduction in the appearance properties of the prepared coating.
[0042] The acid value (Av) of the polyester resin can be 10 to 30 mg KOH / g or 15 to 25 mg KOH / g. When the acid value of the polyester resin is within this range, it improves the weather resistance of the coating film. If the acid value of the polyester resin is below this range, the coating film formed through the crosslinking reaction with the curing agent is insufficient, resulting in a decrease in the mechanical properties of the coating film, such as hardness. If it exceeds this range, over-curing occurs, causing the coating film to become brittle and reducing its elasticity. This may lead to problems with the appearance, water resistance, and scratch resistance of the prepared coating film.
[0043] The hydroxyl value (OHv) of the polyester resin can be 250 to 300 mg KOH / g or 260 to 280 mg KOH / g. When the hydroxyl value of the polyester resin is within this range, its reactivity with melamine resin is enhanced, resulting in increased crosslinking density of the coating film and improved mechanical properties, appearance, and chemical resistance. If the hydroxyl value of the polyester resin is below this range, insufficient reactivity with melamine resin leads to insufficient crosslinking density, resulting in poor durability and chemical resistance of the prepared coating film. If it exceeds this range, over-curing can cause the coating film to become brittle, potentially leading to reduced appearance and scratch resistance.
[0044] The glass transition temperature (Tg) of the polyester resin can be 5 to 20°C or 10 to 14°C. When the glass transition temperature of the polyester resin is within this range, it has the effect of improving the gloss properties and hardness of the coating film. If the glass transition temperature of the polyester resin is below this range, the drying rate of the base coating composition is delayed, resulting in insufficient solvent resistance and shatter resistance of the prepared coating film. If it exceeds this range, the coating film may become brittle, potentially leading to insufficient appearance properties and hardness.
[0045] The weight-average molecular weight (Mw) of the polyester resin can be between 2000 and 4000 g / mol or between 2500 and 3500 g / mol. When the weight-average molecular weight of the polyester resin is within this range, it can improve the smoothness of the base coating composition, forming a soft coating film, and has the effect of improving scratch resistance and hardness. If the weight-average molecular weight of the polyester resin is less than the range, the prepared coating film will have poor mechanical properties due to its low molecular weight. If it exceeds the range, as the molecular weight increases, the flowability decreases, making the coating film brittle, which may lead to reduced smoothness and poor scratch resistance.
[0046] Based on the total weight of the base coating composition, the composition may contain polyester resin at an amount of 3 to 6% by weight or 4 to 5% by weight. When the included polyester resin is within the stated range, it improves the appearance, scratch resistance, and coating smoothness. If the polyester resin content in the composition is less than the stated range, the low crosslinking density leads to reduced appearance and scratch resistance. If the content exceeds the stated range, the high viscosity of the composition reduces workability and drying properties, potentially resulting in reduced appearance and mechanical properties.
[0047] Melamine resin
[0048] Melamine resin, as a curing agent, cures the composition by undergoing a cross-linking reaction with the components of the base coating composition, thereby increasing the hardness of the prepared coating film.
[0049] Melamine resin can be alkylated melamine resin, and can be directly synthesized according to known methods or a commercially available product.
[0050] Melamine resin may contain one or more of the following: methoxymethyl melamine, methyl melamine, butyl melamine, isobutoxy melamine, butoxy melamine, hexahydroxymethyl melamine, hexamethoxymethyl melamine, hexabutoxymethyl melamine, hexamethoxybutoxymethyl melamine, aminomethoxymethyl melamine, and alkylated melamine containing imino groups.
[0051] Commercially available melamine resins include, for example, CYMEL-325, CYMEL-303, CYMEL-1161 and CYMEL-1168 from CYTEC, LUWIPAL 012 and LUWIPAL 072 from BASF, and SETAMINE US-138 from NUPLEX.
[0052] The solids content (NV) of melamine resin relative to the total weight of the resin can be 60 to 80% by weight or 65 to 75% by weight. When the solids content of melamine resin is within the range described, it has the effect of improving the workability of the base coating composition. If the solids content of melamine resin is less than the range described, the viscosity becomes too low, resulting in poor flowability and causing insufficient workability of the base coating composition containing it. If it exceeds the range described, the viscosity becomes too high, leading to reduced stability during the reaction and poor dispersion stability. Therefore, agglomerates may form within the base coating composition over time.
[0053] The viscosity of melamine resin at 25°C can be 1000 to 1800 cps or 1100 to 1700 cps. When the viscosity of melamine resin at 25°C is within this range, it provides excellent gloss and appearance. If the viscosity of melamine resin at 25°C is below this range, the low viscosity results in poor film formation, leading to poor adhesion and scratch resistance. When the viscosity exceeds this range, the workability of the composition deteriorates, potentially resulting in insufficient appearance characteristics of the prepared coating.
[0054] Furthermore, the acid value (Av) of the melamine resin can be 0.1 to 3 mg KOH / g or 0.1 to 2 mg KOH / g. When the acid value of the melamine resin is less than the specified range, the curing reaction rate is low, resulting in poor hardness and appearance properties of the prepared coating film. If it exceeds the specified range, the water resistance may decrease as the hydrophilicity increases.
[0055] Based on the total weight of the base coating composition, the composition may contain melamine resin at a content of 5 to 20% by weight or 8 to 15% by weight. When the content of melamine resin is within the stated range, it can improve the adhesion and hardness of the prepared coating film by increasing the crosslinking density. If the content of melamine resin is less than the stated range, there is a problem of poor hardness and appearance due to low curing properties. If it exceeds the stated range, the coating film becomes brittle due to excessive curing properties, which may lead to reduced adhesion, impact resistance, and scratch resistance.
[0056] <Acrylic anti-sagging agent>
[0057] To adjust the sag properties of the base coating composition, an acrylic anti-sagging agent may be included.
[0058] Acrylic anti-sagging agents can be synthesized directly using known methods or are commercially available products. Acrylic anti-sagging agents can be prepared by polymerization of, for example, one or more of a second vinyl monomer and a second (meth)acrylate monomer.
[0059] As another example, acrylic anti-sagging agents can also be prepared by reacting a second vinyl monomer, a second (meth)acrylate monomer, and benzylamine, and can have a chemical structure with needle-shaped diurea groups.
[0060] As the second vinyl monomer, one or more may be selected from, for example, styrene, methylstyrene, dimethylstyrene, fluorostyrene, ethoxystyrene, methoxystyrene, phenyl vinyl ketone, tert-butylbenzoate, vinyl cyclohexanoate, vinyl acetate, vinylpyrrolidone, vinyl chloride, vinyl alcohol, acetoxystyrene, tert-butylstyrene, and vinyltoluene.
[0061] The second (meth)acrylate monomer may comprise one or more monomers selected from the group consisting of (meth)acrylate monomers without hydroxyl groups and (meth)acrylate monomers with hydroxyl groups.
[0062] The (meth)acrylate monomer, which does not contain a hydroxyl group, may contain one or more of the following: for example, (meth)acrylic acid, meth(meth)acrylic acid, (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, isooctyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isodecanyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, isobornyl (meth)acrylate, and lauryl (meth)acrylate.
[0063] The hydroxyl-containing (meth)acrylate monomer can be, for example, a hydroxyalkyl-containing (meth)acrylate, specifically, it can contain one or more selected from, for example, 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate and 2-hydroxybutyl (meth)acrylate.
[0064] Acrylic anti-sagging agents can be prepared by, for example, free radical polymerization. The physical properties can be adjusted according to the initiator and polymerization time, that is, the weight-average molecular weight (Mw), hydroxyl value (OHv), acid value (Av), etc.
[0065] The solids content (NV) of the acrylic anti-sagging agent relative to the total weight of the resin can be 50 to 70% by weight or 55 to 65% by weight. When the solids content of the acrylic anti-sagging agent is within the range described, it improves the storage stability of the resin and the substrate coating composition, and provides excellent workability. If the solids content of the acrylic anti-sagging agent is below the range described, the viscosity becomes too low, resulting in poor workability of the substrate coating composition containing it. If it exceeds the range described, the viscosity becomes too high, leading to reduced stability during the reaction, poor dispersion stability, and potentially agglomeration over time.
[0066] The viscosity of acrylic anti-sagging agents at 25°C can be between 10,000 and 18,000 cps or between 11,000 and 17,000 cps. When the viscosity of the acrylic anti-sagging agent at 25°C is within this range, the appropriate viscosity of the base coating composition improves workability. If the viscosity of the acrylic anti-sagging agent at 25°C is below this range, the low viscosity of the composition can lead to problems such as incomplete film formation, resulting in poor paint flowability, adhesion, and scratch resistance. When the viscosity exceeds this range, insufficient workability of the composition may lead to a reduction in the appearance properties of the prepared coating.
[0067] Based on the total weight of the base coating composition, the composition may contain an acrylic anti-sagging agent at an amount of 4 to 9 wt% or 5 to 8 wt%. When the contained acrylic anti-sagging agent is within the stated content range, it has the effect of improving the sagging properties of the base coating composition. If the content of the acrylic anti-sagging agent is less than the stated range, the workability of the base coating composition containing it is reduced due to poor drying properties. If it exceeds the stated range, the rapid drying may result in poor paint workability and paint flowability, and increased viscosity of the base coating composition, thereby deteriorating storage stability and appearance.
[0068] <Toner>
[0069] The substrate coating composition according to one embodiment of the present invention may further include a colorant. The colorant has the function of imparting color to the prepared coating film.
[0070] For colorants, there are no particular restrictions as long as they are pigments that can generally be used in coating compositions; for example, inorganic and organic pigments can be used. As another example, the pigments mentioned include metal oxides such as titanium dioxide, carbon black, zinc oxide, ultramarine, and red iron oxide; zinc barium white, lead, cadmium, iron, cobalt, and aluminum sulfides and their hydrochlorides or lactates; azo pigments; and copper phthalocyanine pigments, etc.
[0071] The solids content (NV) of the toner can be 65 to 85% by weight or 70 to 80% by weight relative to the total weight of the toner. When the solids content of the toner is within the range described, it has the effect of improving the workability of the base coating composition.
[0072] The viscosity of the toner at 25°C can be 880 to 2270 cps or 900 to 2000 cps. When the viscosity of the toner at 25°C is within the range described above, the appropriate viscosity of the base coating composition improves workability and appearance.
[0073] Based on the total weight of the base coating composition, the composition may contain a toner at an amount of 33 to 50% by weight or 37 to 45% by weight. When the toner content in the base coating composition is within the range described above, problems such as insufficient hiding power of the prepared coating film, low stability of the composition, and poor dispersibility of the toner can be prevented.
[0074] <Additives>
[0075] The substrate coating composition according to one embodiment of the present invention may further include additives such as ultraviolet absorbers, leveling agents, surface smoothers, and curing catalysts.
[0076] Ultraviolet absorbers improve the weather resistance of coatings by blocking ultraviolet rays from reaching them. The solids content (NV) of ultraviolet absorbers is 80 to 100% by weight, the specific gravity is 1.0 to 1.2 g / cm³, and the ignition point is 45 to 49°C.
[0077] Ultraviolet absorbers can be benzotriazole-based ultraviolet absorbers, such as α-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-hydroxy poly(oxy-1,2-ethanediyl)(α-[3-[3-(2H-Benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-h ydroxypoly(oxy-1,2-ethanediyl)), α-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]poly(oxy-1,2-ethanediyl)(α-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl]-ω-[3-[3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxyphenyl]-1-oxopropyl] Benzotriazole-based ultraviolet absorbers such as [nyl]-1-oxopropoxy]poly(oxy-1,2-ethanediyl) and 3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy-methylester (3-(2H-benzotriazol-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy-methylester).
[0078] Leveling agents impart leveling and wetting properties to the prepared coating. Leveling agents can be cationic, anionic, or nonionic surfactants; for example, they may include nonionic surfactants. The leveling agent has a solids content (NV) of 45 to 55% by weight, a specific gravity of 1.0 to 1.3, and a viscosity of 40 to 60 cps at 25°C.
[0079] Surfactants affect the smoothness of the prepared coating and improve its appearance properties. The surfactant has a solids content (NV) of 50 to 54% by weight, a viscosity of 110 to 120 cSt, and a specific gravity of 0.8 to 1.0.
[0080] The curing catalyst has the function of preventing unstable curing of the substrate coating composition, thereby improving the mechanical properties of the coating film prepared therefrom. Examples of curing catalysts include amine-containing phosphate ester compounds or dodecylbenzene sulfonic acid compounds. The solids content (NV) of the curing catalyst can be 72 to 76% by weight, the specific gravity at 25°C can be 0.9 to 1.0, and the acid value (Av) can be 120 to 140 mg KOH / g.
[0081] There are no particular restrictions on the amount of additives, as long as it is within the range that is generally acceptable in a base coating composition. For example, the composition may contain additives at a content of 1 to 8% by weight or 2 to 7% by weight, based on the total weight of the base coating composition.
[0082] Solvent
[0083] The substrate coating composition according to one embodiment of the present invention may further include a solvent. The solvent may have the function of adjusting the viscosity of the composition, improving drying properties, and improving the appearance and spreadability of the prepared coating film.
[0084] The solvent is not particularly limited as long as it is a solvent commonly used in the base coating composition, and may include one or more solvents selected from, for example, aromatic solvents, acetate solvents, alcohol solvents, and propionate solvents. Specifically, the solvent may include aromatic solvents such as toluene, xylene, etc.; acetate solvents such as 1-methoxy-2-propyl acetate, methyl acetate, ethyl acetate, n-propyl acetate, n-butyl acetate, methyl glutarate, methyl succinate, methyl adipate, dimethyl glutarate, dimethyl succinate, dimethyl adipate, propylene glycol methyl ether acetate (PMA), butyl carbitol acetate, butyl cellosolve acetate, etc.; alcohol solvents such as n-butanol, propanol, 1-methoxy-2-propanol, 2-butoxyethanol, etc.; ketone solvents such as acetone, methyl ethyl ketone, methyl butyl ketone, and methyl isobutyl ketone; and propionate solvents such as ethyl ethoxypropionate, etc. Furthermore, commercially available aromatic solvents include Kocosol #100 and Kocosol #150.
[0085] Based on the total weight of the base coating composition, the composition may contain solvent at a content of 1 to 50% by weight or 5 to 25% by weight. When the solvent content is within the range described above, it can appropriately adjust the viscosity of the composition, thus improving workability and drying properties. If the solvent content in the base coating composition is less than the range described above, the composition will have poor workability due to its high solids content. If it exceeds the range described above, the solids content of the base coating composition used to prepare will be low, resulting in increased fluidity and potentially causing problems with the appearance and adhesion of the prepared coating film.
[0086] According to one embodiment of the present invention, the substrate coating composition can be a liquid comprising a main component and a curing agent component.
[0087] Based on the total weight of the composition, the solids content of the base coating composition of the present invention can be 50 to 60% by weight or 52 to 58% by weight. When the solids content of the base coating composition of the present invention is within the range described above, it has the advantage of providing appropriate coating workability. If the solids content of the base coating composition of the present invention is less than the range described above, there is a problem of reduced curing reactivity due to the decreased solids content; if it exceeds the range described above, the workability of the base coating composition may be reduced due to the high solids content.
[0088] The base coating composition of the present invention, based on Ford Cup No. 4 at 25°C, can have a viscosity of 30 to 50 seconds, 32 to 48 seconds, or 35 to 45 seconds. If the viscosity of the base coating composition of the present invention is less than the range described above, problems such as vertical surface dripping may occur. If it exceeds the range, the viscosity of the composition is high, which may reduce the appearance characteristics of the coating film prepared thereby or may put a load on the coating machine, causing coating machine malfunction.
[0089] As mentioned above, the thermosetting temperature of the coating process of the base coating composition according to the present invention can be performed at a low temperature of less than 130°C, which is lower than the temperature of the prior art, thus saving the cost required for the coating process and making it very economical. Moreover, the coating film prepared by the base coating composition according to the present invention has excellent mechanical properties, especially gloss, impact resistance, water resistance, cold crack resistance, etc., which is advantageous for use as a vehicle body coating.
[0090] The present invention will now be described in more detail through embodiments. However, these embodiments are only for the purpose of helping to understand the present invention, and the scope of the present invention is not limited to these embodiments in any way.
[0091] [Example]
[0092] Preparation of substrate coating compositions in examples and comparative examples
[0093] The components were mixed according to the amounts shown in Tables 1 to 4 to prepare a base coating composition with a viscosity of 40 seconds based on Ford Cup No. 4.
[0094] Table 1
[0095]
[0096]
[0097] Table 2
[0098]
[0099]
[0100] Table 3
[0101] Table 4
[0102]
[0103]
[0104]
[0105] The physical properties, manufacturers, and / or product names of the components used in the examples and comparative examples are shown in Table 5 below.
[0106] Table 5
[0107]
[0108]
[0109] Experimental Example: Evaluation of the Properties of the Prepared Coating Film
[0110] The substrate coating compositions prepared in the examples and comparative examples were applied to the electroplated samples by bell spraying to a thickness of 35 μm and then cured in an oven at 130°C for 20 minutes to prepare the final coating film.
[0111] The appearance and physical properties of the final coating were measured using the method described below, and the results are shown in Tables 6 to 9.
[0112] (1) Painting operation
[0113] For coating workability, the evaluation was conducted by observing the spray pattern when the paint is dispensed and its wettability on the base material.
[0114] Based on the observed condition, the evaluation is as follows: Excellent (◎), Good (○), Average (△), Poor (×).
[0115] (2) Coating appearance
[0116] Using the final coating as the object, gloss (LU), sharpness (SH), and orange peel (OP) were measured using Wave Scan DOI (BYKGardner), an automotive appearance tester. Based on the measured physical properties, the overall appearance evaluation value (CF) was calculated using the following mathematical formula 1.
[0117] [Mathematical Expression 1]
[0118] CF=LU×0.15+SH×0.35+OP×0.5
[0119] CF is measured and calculated horizontally and vertically. As the horizontal / vertical value of CF, when CF is greater than or equal to 65, it is rated as excellent (◎); when CF is greater than or equal to 60 but less than 65, it is rated as good (○); when CF is greater than or equal to 55 but less than 60, it is rated as average (△); when CF is less than 55, it is rated as poor (×).
[0120] (3) Gloss
[0121] To measure the gloss (GLOSS, %) reflected from the coating, a gloss meter (BYK Gardner) was used to measure the gloss at 20° of the final coating.
[0122] According to the measurement results, when the gloss is greater than or equal to 90%, it is rated as excellent (◎); when the gloss is greater than or equal to 89% but less than 90%, it is rated as good (○); when the gloss is greater than or equal to 87% but less than 89%, it is rated as average (△); and when the gloss is less than 87%, it is rated as poor (×).
[0123] (4) Adhesion
[0124] After curing the substrate coating compositions of the examples and comparative examples, the adhesion was evaluated using the checkerboard method.
[0125] Specifically, using the checkerboard method, 100 squares, each 2mm wide and 2mm long, are drawn on the recoating film with a blade. Adhesive tape is then used to separate the squares to measure adhesion. When all 100 squares are 100% completely bonded, the adhesion is rated as excellent (◎); when 70% or more but less than 100% of the remaining squares are bonded, the adhesion is rated as good (○); when 50% or more but less than 70% of the remaining squares are bonded, the adhesion is rated as fair (△); and when less than 50% of the remaining squares are bonded, the adhesion is rated as poor (×).
[0126] (5) Impact resistance
[0127] The final coating was used as the test subject, and its impact resistance was evaluated according to ASTM D2794. Using a DuPont impact testing machine, a 500g weight was dropped onto the sample from a height varying from 30cm to 50cm, and the appearance of the coating was observed.
[0128] The observation results show that when the falling height of the heavy object is greater than or equal to 50 cm, if the coating does not crack or peel, it is rated as excellent (◎). When the falling height of the heavy object is greater than or equal to 30 cm but less than 50 cm, if the coating cracks or peels, it is rated as good (○). When the falling height of the heavy object is greater than or equal to 20 cm but less than 30 cm, if the coating cracks or peels, it is rated as average (△). When the falling height of the heavy object is less than 20 cm, if the coating cracks or peels, it is rated as poor (×).
[0129] (6) Water resistance
[0130] The final coating was deposited in a constant temperature water bath at 40°C for 240 hours. After being left at room temperature for 1 hour, the adhesion was evaluated using the checkerboard method, and the color change was confirmed visually.
[0131] Specifically, adhesion was measured using the same method as the checkerboard method described in item (4). The same evaluation criteria were also applied to evaluate the water resistance of the coating.
[0132] (7) Paint flowability
[0133] A sample with a primer coating was vertically suspended on a steel plate with a hole of 5 mm in diameter after electroplating. The substrate coating compositions of the examples and comparative examples were coated by the same method as described above. After drying and curing, the surface of the prepared coating was observed to evaluate the paint flowability of the composition.
[0134] Specifically, paint condensation was observed at the lower end of the orifice, and the thickness (μm) of the paint film at the point where flow was observed to begin was recorded as the critical flow film thickness. At this point, the lower the measured critical flow film thickness, the worse the paint flowability. In this case, a critical flow film thickness greater than or equal to 40 μm is rated as excellent (◎), a critical flow film thickness greater than or equal to 35 μm but less than 40 μm is rated as good (○), a critical flow film thickness greater than or equal to 30 μm but less than 35 μm is rated as average (△), and a critical flow film thickness less than 30 μm is rated as poor (×).
[0135] (8) Cold fracture resistance
[0136] After the final coating was placed at -20°C for 3 hours, it was then impacted with 50g of gravel (4mm in diameter) at a 45° angle under a pressure of 4 bar. Afterwards, foreign matter such as coating residue that had formed or peeled off was removed from the final coating.
[0137] For the damaged areas of the final coating, if there are 10 or fewer damaged areas of 1 mm or less, the rating is excellent (◎); if there are 10 or fewer damaged areas of more than 1 mm but less than or equal to 2 mm, the rating is good (○); if there are 10 or fewer damaged areas of more than 2 mm but less than or equal to 3 mm, the rating is fair (△); and if there are more than 10 damaged areas of more than 2 mm but less than or equal to 3 mm, the rating is poor (×).
[0138] (9) Recoating adhesion
[0139] After preparing recoating films by recoating and curing the substrate coating compositions of the examples and comparative examples using the same method as described above, the adhesion was evaluated using the checkerboard method.
[0140] Specifically, using the checkerboard method, 100 squares, each 2mm wide and 2mm long, are drawn on the recoating film with a blade. Adhesive tape is then used to separate the squares to measure adhesion. When all 100 squares are 100% completely bonded, the adhesion is rated as excellent (◎); when 70% or more but less than 100% of the remaining squares are bonded, the adhesion is rated as good (○); when 50% or more but less than 70% of the remaining squares are bonded, the adhesion is rated as fair (△); and when less than 50% of the remaining squares are bonded, the adhesion is rated as poor (×).
[0141] Table 6
[0142]
[0143]
[0144] Table 7
[0145]
[0146] Table 8
[0147]
[0148] Table 9
[0149]
[0150] As shown in Tables 6 to 9, it can be seen that the base coating composition of the embodiments has excellent paint workability and paint flowability, and the coating film prepared therefrom also has excellent mechanical properties such as appearance characteristics, gloss, recoating adhesion, impact resistance, water resistance and cold cracking resistance.
[0151] The various embodiments of the present invention will now be described.
[0152] (1) A base coating composition comprising an acrylic resin, a polyester resin and a melamine resin, wherein the acrylic resin has a hydroxyl value of 70 to 85 mg KOH / g and a weight-average molecular weight of 40,000 to 50,000 g / mol, and the polyester resin has an acid value of 10 to 30 mg KOH / g and a hydroxyl value of 250 to 300 mg KOH / g.
[0153] (2) A base coating composition wherein the acrylic resin has an acid value of 10 to 30 mg KOH / g and a glass transition temperature of 20 to 40 °C.
[0154] (3) A base coating composition wherein the polyester resin has a glass transition temperature of 5 to 20°C and a weight-average molecular weight of 2000 to 4000 g / mol.
[0155] (4) A base coating composition wherein the melamine resin has a viscosity of 1000 to 1800 cps at 25°C and an acid value of 0.1 to 3 mg KOH / g.
[0156] (5) A base coating composition, wherein, based on the total weight of the base coating composition, it comprises 22 to 33% by weight of acrylic resin, 3 to 6% by weight of polyester resin and 5 to 20% by weight of melamine resin.
Claims
1. A base coating composition, wherein, Including acrylic resin, polyester resin and melamine resin, The hydroxyl value of acrylic resin is 75 to 80 mg KOH / g, and the weight-average molecular weight is 40,000 to 50,000 g / mol. The polyester resin has an acid value of 10 to 30 mg KOH / g, a hydroxyl value of 250 to 300 mg KOH / g, a glass transition temperature of 5 to 20°C, and a weight-average molecular weight of 2500 to 3500 g / mol. The acid value of melamine resin is 0.1 to 3 mg KOH / g.
2. The substrate coating composition according to claim 1, wherein, The acid value of acrylic resin is 10 to 30 mg KOH / g, and the glass transition temperature is 20 to 40℃.
3. The substrate coating composition according to claim 1, wherein, The viscosity of melamine resin at 25°C is 1000 to 1800 cps.
4. The substrate coating composition according to claim 1, wherein, Based on the total weight of the base coating composition, it comprises 22 to 33% by weight of acrylic resin, 3 to 6% by weight of polyester resin and 5 to 20% by weight of melamine resin.
Citation Information
Patent Citations
Acryl urethane composition for polyethylene tube coating and coating method using the same
KR100158534B1
Coating composition
CN105518091A