A repair process for cobalt-based superalloy nozzle active diffusion brazing
By employing active diffusion brazing technology for cobalt-based high-temperature alloy nozzles, the problem of inaccurate nozzle repair in traditional repair methods has been solved, achieving efficient and precise nozzle repair, improving the strength and durability of turbine components, and reducing maintenance costs.
Patent Information
- Application Number
- CN202411204542.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Traditional argon arc welding and ordinary brazing methods are difficult to efficiently and accurately repair cracks and defects in cobalt-based superalloy nozzles, leading to an expansion of the heat-affected zone, damaging the mechanical properties and corrosion resistance of turbine components, and failing to meet the stability and durability requirements in harsh environments.
The active diffusion brazing process using cobalt-based high-temperature alloy nozzles includes surface pretreatment, filler metal preparation, vacuum heating, and brazing process control. By repairing the nozzle through multiple steps, a clean, rough, and uniform brazing surface is ensured. Specific filler metal and solder resist components are used, and the heating rate and time are controlled to ensure brazing quality.
After repair, the nozzle strength reaches more than 92% of the original material, extending the service life of the equipment, reducing maintenance costs, increasing repair efficiency by 50%, and ensuring the stability and durability of components in high-temperature environments.
Abstract
Description
Technical Field
[0001] This invention relates to a repair process for active diffusion brazing of cobalt-based high-temperature alloy nozzles, belonging to the field of heavy-duty gas turbine maintenance technology. Background Technology
[0002] Cobalt-based superalloys, used as materials for thermal channels in gas turbines, operate in extremely harsh environments, with components subjected to multiple effects including high temperatures, thermal cycling fatigue, impact, and thermal fatigue. Despite their excellent high-temperature performance, long-term operation under such severe conditions inevitably leads to performance degradation, with thermal fatigue-induced cracking and large-area crazing being particularly common.
[0003] Traditional argon arc welding repair methods are only suitable for repairing a small number of cracks and defects. Large-scale welding makes it difficult to precisely control heat input during the welding process, easily leading to an expansion of the heat-affected zone and consequently damaging the mechanical properties and corrosion resistance of turbine components. Furthermore, ordinary brazing methods are only suitable for repairing localized micro-cracks; repairing large-area cracks cannot meet the strength requirements after repair, and therefore cannot ensure the stability and durability of components in harsh operating environments. Summary of the Invention
[0004] To address the problems existing in the prior art, this invention provides a repair process for active diffusion brazing of cobalt-based high-temperature alloy nozzles, which enables more efficient and precise repair of gas turbine thermal passage components.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is: a repair process for active diffusion brazing of a cobalt-based high-temperature alloy nozzle, characterized by comprising the following steps;
[0006] Step S1: Use a cutting blade with a thickness of ≤1mm to cut off the connecting welds between the cooling cover plate, cooling core and other accessories and the outer edge plate of the nozzle, and remove all accessories; align the floating sealing grooves of the inner and outer edge plates, install the inner and outer edge plates into the alignment fixture in a specific posture, and adjust the inner and outer edge plates respectively; clean the entire nozzle with aluminum oxide to remove surface oxides;
[0007] Step S2: Load the nozzle into the reactor of the FIC equipment, fix the nozzle leading edge toward the gas purging direction using a tooling, continuously rinse with hydrogen fluoride, and then anneal in the furnace; then remove the nozzle from the furnace, and use 80-mesh nickel sandblasting to perform nickel sandblasting on the surface to be brazed, with the spray gun at a 60-degree angle to the surface to be sandblasted, to obtain a clean rough surface.
[0008] Step S3: After completing the previous step, within 4 hours, transfer the nozzle to the brazing chamber and use a 0.8mm syringe to inject solder resist into all cooling holes of the nozzle, injecting from inside the hole into the brazing surface, and stopping at a distance of 0.3 to 0.5mm from the surface; the solder resist at the edge of the hole should be full and there should be no gaps.
[0009] Step S4: Prepare the solder and add an appropriate amount of acetone and mix thoroughly;
[0010] Step S5: Spray the prepared brazing agent evenly onto the surface of the nozzle at a distance of 15-20cm. For areas with many cracks, spraying can be repeated after each surface has dried and solidified. Load the sprayed nozzle into the brazing furnace, evacuate the vacuum, and then heat it to a certain temperature to react and allow the S-resin to fully decompose.
[0011] Step S6: Then, heat the temperature to 1100°C at a heating rate of 8–14°C and hold it at 1100°C for 40 minutes. The temperature of the entire nozzle becomes uniform at this temperature. Then, heat the temperature to 1180°C at a heating rate of 8–14°C and hold it at this temperature for 30 minutes. Then, cool the furnace to 1150°C and hold it at this temperature for 4 hours. Then, heat the temperature to 1180°C again at a heating rate of 8–14°C and hold it for 4 hours. Then, heat the temperature to 1200°C again at a heating rate of 8–14°C and hold it for 4 hours.
[0012] Step S7: After the above temperature adjustment reaction, argon gas is introduced to cool to room temperature, and 200-mesh abrasive belt is used to polish from the leading edge to the trailing edge of the nozzle blade to remove excess brazing filler metal and restore the original contour.
[0013] Step S8: EDM opens the cooling holes blocked by brazing, using electrodes with wire diameters of 0.8mm, 1.2mm, and 1.5mm;
[0014] Step S9: Fluorescent penetrant testing and visual inspection of the diffused brazing components. If cracks or surface defects are found during visual inspection, repeat steps S2-S7 to repair the defects.
[0015] Furthermore, in step S1, surface oxides are removed by cleaning the entire nozzle with 220-mesh alumina with a purity greater than 98% at a pressure of 6 Bar.
[0016] Furthermore, in step S2, the furnace is continuously flushed with hydrogen fluoride at 1020°C for at least 60 minutes, followed by furnace annealing.
[0017] Furthermore, in step S4, the solder is prepared by using A powder with the composition Cr: 22.0, Ni: 8.0, W: 7.0, Ta: 3.5, Ti: 0.2, Zr: 0.5 and B powder with the composition Cr: 22.5, Ni: 10.0, W: 7.0, Ta: 3.5, Ti: 0.2, Zr: 0.5, B: 4.0, plus S adhesive in a weight ratio of 6:5:1.
[0018] Furthermore, in step S5, the coated nozzle is loaded into the brazing furnace, and a vacuum is drawn to ensure that the furnace vacuum degree is better than 5x10⁻⁶. -4 Heat to 450°C at a rate of 8–14°C, and hold at 450°C for 40 minutes to allow the S-resin to fully decompose. Before heating to the next temperature stage, ensure that the vacuum level in the oven returns to 5 x 10. -3 torr.
[0019] The beneficial effects of this invention are:
[0020] (1) This invention describes a process for active diffusion repair of a cobalt-based high-temperature alloy nozzle. After repair, the strength of the component reaches more than 92% of the strength of the raw material. The strength of the raw material at 870℃ is 295MPa, and after repair, it reaches 275MPa. After repair, it continues for one cycle of 48,000 hours. This effectively extends the service life of the equipment and reduces maintenance costs.
[0021] (2) Compared with traditional welding, the present invention allows for batch operation of brazing, which improves repair efficiency by 50%. Detailed Implementation
[0022] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below through embodiments. However, it should be understood that the specific embodiments described herein are merely illustrative of the invention and are not intended to limit the scope of the invention.
[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of this invention is for the purpose of describing particular embodiments only and is not intended to limit the invention.
[0024] In this embodiment, a cutting blade with a thickness of ≤1mm is used to remove the cooling cover plate, the cooling core, and other accessories from the weld seam connecting them to the outer edge plate of the nozzle, and all accessories are removed. The floating sealing grooves of the inner and outer edge plates are calibrated by installing them into a calibration fixture in a specific orientation, adjusting the inner and outer edge plates to R710mm and R844mm respectively. The entire nozzle is cleaned using 220-mesh alumina with a purity greater than 98% at a pressure of 6 Bar to remove surface oxides. The nozzle is loaded into the reactor of the FIC equipment, and the nozzle leading edge is fixed towards the gas purging direction using a fixture. It is continuously flushed with hydrogen fluoride at 1020°C for at least 60 minutes, followed by furnace annealing. The nozzle is removed from the furnace, and the surface to be brazed is nickel-blasted using 80-mesh nickel abrasive, with the blasting gun at a 60-degree angle to the surface to be blasted, to obtain a clean, rough surface.
[0025] After completing the previous step, within 4 hours, transfer the nozzle to the brazing chamber and use a 0.8mm syringe to inject solder resist into all cooling holes of the nozzle, injecting from inside the holes into the brazing surface, stopping at a distance of 0.3–0.5mm from the surface. The solder resist should be fully applied to the edges of the holes, leaving no gaps.
[0026] The solder was prepared by mixing A powder with composition Cr22.0Ni8.0W7.0Ta3.5Ti0.2Zr0.5 and B powder with composition Cr22.5Ni10.0W7.0Ta3.5Ti0.2Zr0.5B4.0 with S adhesive in a weight ratio of 6:5:1, and then adding an appropriate amount of acetone and mixing thoroughly.
[0027] Spray the prepared brazing agent evenly onto the surface to be brazed from a distance of 15-20cm from the nozzle surface. For areas with many cracks, the spraying can be repeated after each surface has dried and solidified.
[0028] Load the coated nozzles into the brazing furnace, evacuate the furnace, and ensure the furnace vacuum level is better than 5 x 10⁻⁶. -4 The temperature is increased to 450°C at a heating rate of 8–14°C, and held at 450°C for 40 minutes to allow the S-resin to fully decompose. Before increasing the temperature to the next stage, ensure that the vacuum level in the oven returns to 5 x 10⁻⁶. -3 The temperature is increased to 1100°C at a heating rate of 8–14°C and held at 1100°C for 40 minutes, until the entire nozzle reaches uniform temperature. The temperature is then increased to 1180°C at a heating rate of 8–14°C and held at this temperature for 30 minutes. The furnace is then cooled to 1150°C and held at this temperature for 4 hours. The temperature is then increased to 1180°C again at a heating rate of 8–14°C and held for 4 hours. Finally, the temperature is increased to 1200°C at a heating rate of 8–14°C and held for 4 hours. Argon gas is introduced to cool the furnace to room temperature.
[0029] Use 200-grit abrasive belt to polish from the leading edge to the trailing edge of the nozzle blade to remove excess brazing filler metal and restore the original profile. Use EDM to clear cooling holes blocked by brazing, using electrodes with wire diameters of 0.8mm, 1.2mm, and 1.5mm. Perform fluorescent penetrant testing and visual inspection on the diffused brazed components. If cracks or surface defects are found during visual inspection, repeat steps 5-17 to repair the defects.
[0030] The invention provides an advanced maintenance technology. This technology can repair hot passage components of gas turbines more efficiently and accurately, overcoming the shortcomings of existing technologies, such as the expansion of the heat-affected zone, damage to mechanical properties and corrosion resistance, residual stress, and deformation problems.
[0031] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions or improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A repair process for active diffusion brazing of a cobalt-based superalloy nozzle, characterized in that, Includes the following steps; Step S1: Use a cutting blade with a thickness of ≤1mm to cut off the weld seam connecting the cooling cover plate, cooling core and other accessories to the outer edge plate of the nozzle, and remove all accessories; The inner and outer edge plates are calibrated by installing them into the calibration fixture in a specific posture and adjusting them separately. Clean the entire nozzle with aluminum oxide to remove surface oxides; Step S2: Load the nozzle into the reactor of the FIC equipment, fix the nozzle leading edge toward the gas purging direction using a tooling, continuously rinse with hydrogen fluoride, and then anneal in the furnace; then remove the nozzle from the furnace, and use 80-mesh nickel sandblasting to perform nickel sandblasting on the surface to be brazed, with the spray gun at a 60-degree angle to the surface to be sandblasted, to obtain a clean rough surface. Step S3: After completing the previous step, within 4 hours, transfer the nozzle to the brazing chamber and use a 0.8mm syringe to inject solder resist into all cooling holes of the nozzle, injecting from inside the hole into the brazing surface, and stopping at a distance of 0.3 to 0.5mm from the surface; the solder resist at the edge of the hole should be full and there should be no gaps. Step S4: Prepare the solder and add an appropriate amount of acetone and mix thoroughly; Step S5: Spray the prepared brazing agent evenly onto the surface of the nozzle at a distance of 15-20cm. For areas with many cracks, spraying can be repeated after each surface has dried and solidified. Load the sprayed nozzle into the brazing furnace, evacuate the vacuum, and then heat it to a certain temperature to react and allow the S-resin to fully decompose. Step S6: Then, heat the temperature to 1100°C at a heating rate of 8–14°C and hold it at 1100°C for 40 minutes. The temperature of the entire nozzle becomes uniform at this temperature. Then, heat the temperature to 1180°C at a heating rate of 8–14°C and hold it at this temperature for 30 minutes. Then, cool the furnace to 1150°C and hold it at this temperature for 4 hours. Then, heat the temperature to 1180°C again at a heating rate of 8–14°C and hold it for 4 hours. Then, heat the temperature to 1200°C again at a heating rate of 8–14°C and hold it for 4 hours. Step S7: After the above temperature adjustment reaction, argon gas is introduced to cool to room temperature, and 200-mesh abrasive belt is used to polish from the leading edge to the trailing edge of the nozzle blade to remove excess brazing filler metal and restore the original contour. Step S8: EDM opens the cooling holes blocked by brazing, using electrodes with wire diameters of 0.8mm, 1.2mm, and 1.5mm; Step S9: Fluorescent penetrant testing and visual inspection of the diffused brazing components. If cracks or surface defects are found during visual inspection, repeat steps S2-S7 to repair the defects.
2. The repair process for active diffusion brazing of a cobalt-based high-temperature alloy nozzle according to claim 1, characterized in that, In step S1, surface oxides are removed by cleaning the entire nozzle with 220-mesh alumina with a purity greater than 98% at a pressure of 6 Bar.
3. The repair process for active diffusion brazing of a cobalt-based high-temperature alloy nozzle according to claim 1, characterized in that, In step S2, the furnace is continuously flushed with hydrogen fluoride at 1020°C for at least 60 minutes, followed by furnace annealing.
4. The repair process for active diffusion brazing of a cobalt-based high-temperature alloy nozzle according to claim 1, characterized in that, In step S4, the brazing filler metal is prepared by using A powder with the composition Cr: 22.0, Ni: 8.0, W: 7.0, Ta: 3.5, Ti: 0.2, Zr: 0.5 and B powder with the composition Cr: 22.5, Ni: 10.0, W: 7.0, Ta: 3.5, Ti: 0.2, Zr: 0.5, B: 4.0, plus S glue in a weight ratio of 6:5:
1.
5. The repair process for active diffusion brazing of a cobalt-based high-temperature alloy nozzle according to claim 1, characterized in that, In step S5, the coated nozzle is loaded into the brazing furnace, and a vacuum is drawn to ensure that the furnace vacuum degree is better than 5x10. -4 Heat to 450°C at a rate of 8–14°C, and hold at 450°C for 40 minutes to allow the S-resin to fully decompose. Before heating to the next temperature stage, ensure that the vacuum level in the oven returns to 5 x 10. -3 torr.
Citation Information
Patent Citations
Brazing process of turbine stator blade of gas turbine
CN110919289A
DZ40M alloy part large-gap brazing repair method
CN111218584A