Method for welding structural parts of excavator
Through batch welding and arc-extinguishing plate processing, the problem of insufficient distinction between butt welds and corner welds in the welding of excavator structural parts is solved, high-quality welding and structural strength improvement are achieved, and production costs and failure risks are reduced.
Patent Information
- Application Number
- CN202411202655.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-26
Smart Images

Figure CN119017020A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of welding, and in particular to a welding method for excavator structural parts. Background Art
[0002] The main load-bearing and force-bearing structures of excavators are all welded structures, such as booms, dipper arms, platforms, chassis, buckets and other structural parts. Poor control of process flow, assembly gap, welding parameters, welding sequence and other aspects during welding can easily lead to welding defects, large residual stress after welding, welding deformation and other problems. During use, external forces or fatigue loads will cause cracking of welded structural parts and other quality problems, reducing the strength and service life of the structural parts.
[0003] Due to the complex welding process of excavator structural parts, butt welds and fillet welds are the main types, involving a large number of butt and fillet joints. In the past welding process, the two types of welds were often not distinguished, but were welded uniformly by welding robots at the same welding station. Take the boom as an example. Figure 1 As shown, there are the following problems:
[0004] (1) In the T-shaped structure, the defects at both ends of the butt weld need to be dealt with before the fillet weld can be welded. At the same time, the butt weld joint cannot be handled by welding. The fillet weld needs to be disconnected here, and the joint cannot be welded at one time.
[0005] (2) Due to the discontinuity of the weld at the T-shaped structure, manual repair welding is required for the unwelded area, which adds two fillet weld joints and increases the risk of failure.
[0006] (3) Manual repair welding reduces the welding automation rate. At the same time, the extra joints need to be polished, which reduces production efficiency and increases production costs. Summary of the invention
[0007] In view of the deficiencies in the above-mentioned prior art, the present invention provides a method for welding excavator structural parts, which welds butt welds and fillet welds in batches, effectively improving the welding quality and structural strength of the structural parts, while improving the welding efficiency.
[0008] To achieve the above object, the present invention adopts the following technical solution:
[0009] Provided is a method for welding an excavator structural part, comprising:
[0010] Step 1, assemble the components in sequence and perform positioning welding to fix the positions of the components;
[0011] Step 2, welding the butt weld using a welding robot;
[0012] Step 3, processing the butt weld joint;
[0013] Step 4, welding the fillet weld;
[0014] Step 5: annealing heat treatment.
[0015] Furthermore, in step 1, the gap of the butt weld is adjusted to 4-7 mm, and the gap of the fillet weld is not greater than 2 mm, so as to avoid welding defects such as lack of fusion and undercut caused by too large or too small gaps, and ensure welding quality.
[0016] Furthermore, in step 1, the positioning welding assembly is performed by spot welding, and then the internal welds are welded by intermittent welding to ensure structural rigidity and prevent welding deformation.
[0017] Furthermore, in step 1, the length of the positioning weld is 30-50 mm, and the weld foot is 5 mm, which can not only ensure the welding quality, but also avoid the cost waste caused by the weld foot being too long.
[0018] Furthermore, in step 2, before welding the butt weld, an arc-starting and arc-ending plate is installed to guide the arc starting and arc ending positions of the butt weld to the arc-starting and arc-ending plates outside the weld area, thereby avoiding welding defects at the weld end and effectively improving the weld quality.
[0019] Furthermore, in step 2, after the butt weld is completed, the arc-initiating and extinguishing plates are planed off, and the weld ends are polished and cleaned to ensure that there are no defects at the butt weld ends, which is beneficial to the subsequent fillet weld welding process and the overall quality improvement of the structural parts.
[0020] Furthermore, in step 2 or step 3, priming, filling, and covering are performed alternately to avoid excessive heat input at the welding position, so as to facilitate the control of the interlayer temperature and thus ensure the welding quality of the weld; for welds filled with more than 2 layers, fill every 2 layers and then weld the remaining welds, and cover the surface after the filling is completed.
[0021] Further, in step 4, the heat treatment process includes:
[0022] Placing the welded structural component in a heat treatment furnace, and heating the structural component to a first temperature at a first heating rate;
[0023] heating the structural member to a second temperature at a second heating rate, the second heating rate being less than the first heating rate, the second temperature being higher than the first temperature;
[0024] Insulation;
[0025] Cooling the heat treatment furnace to a third temperature at a third rate;
[0026] The structural parts are taken out of the heat treatment furnace and cooled to room temperature.
[0027] Furthermore, the first heating rate is 200°C / hour and the first temperature is 300°C.
[0028] Furthermore, the second heating rate is 160°C / hour, and the second temperature is 620±20°C. Stress is released through local plastic deformation inside the structure, thereby reducing residual stress of the structural parts and improving fatigue strength.
[0029] Furthermore, the heat preservation process is to keep the structural component at the second temperature in the heat treatment furnace for 3 hours.
[0030] Furthermore, the third rate is 100° C. / hour, and the third temperature is 200° C., and new residual stress is avoided by slow cooling.
[0031] By adopting the above technical solution, the beneficial effects of the present invention are as follows:
[0032] 1. The present invention divides the welding process of excavator structural parts such as the boom into two parts according to the welds. The butt welds between the plates are firstly welded, and after the weld ends are processed, the fillet welds between the remaining parts are welded. The two weld joints do not need to be disconnected and can be directly welded, so that the fillet welds at the T-shaped structure can be continuously welded without disconnection and redundant joints, which effectively reduces the risk of failure. At the same time, the degree of welding automation is greatly improved, the manual workload is reduced, and the production efficiency is improved.
[0033] 2. Before welding the butt weld, the present invention installs an arc-starting and extinguishing plate first, and removes the arc-starting and extinguishing plate after the butt weld is completed and before welding the fillet weld, and grinds the end to eliminate the end weld defects and ensure direct welding of the weld in the subsequent process.
[0034] 3. The present invention performs annealing heat treatment on the welded structural parts, which can effectively reduce the residual stress of the structure, improve the fatigue strength of the welded structural parts, and help to extend the service life of the structural parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0036] Figure 1 This is the welding structure diagram of the boom;
[0037] Figure 2 A welding process flow chart of an embodiment of the present invention;
[0038] Figure 3 This is a welding structure diagram of the bucket arm in an embodiment of the present invention;
[0039] Figure 4 4 is a heat treatment process curve diagram of an embodiment of the present invention.
[0040] In the figure: 1, butt weld of first side plate; 2, butt weld of second side plate; 3, butt weld of third side plate; 4, butt weld of fourth side plate; 5, butt weld of first cover plate; 6, butt weld of second cover plate DETAILED DESCRIPTION
[0041] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by ordinary technicians in the technical field to which the present invention belongs. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0042] Embodiment 1
[0043] In a typical embodiment of the present application, a method for welding a structural part of an excavator is provided, such as Figure 2-4 As shown, including:
[0044] Step 1: Assemble the components one by one and fix the positions of the components by positioning welding.
[0045] Specifically, the lifting operations of the components are carried out in sequence from top to bottom and from front to back on the special tooling according to the assembly sequence, and the positioning mechanism and the clamping mechanism are operated to clamp and fix the components.
[0046] Adjust the butt weld gap between adjacent components. In this embodiment, the butt weld gap is 4-7mm, and the fillet weld gap is less than or equal to 2mm to ensure the optimal welding size, avoid welding defects such as unfusion due to too large a gap or undercut due to too small a gap, and improve welding quality.
[0047] After that, positioning welding is performed to fix the relative positions of the components. In this embodiment, positioning is performed by spot welding. If the positioning welding is too long, it will cause cost waste. If it is too short, the arc starting and ending currents will be unstable and welding defects will easily occur. Therefore, the positioning welding length is 30-50mm, and the weld foot is 5mm. This can not only ensure the welding quality, but also avoid the weld foot being too large to affect the welding of the upper weld. It is also economical and environmentally friendly.
[0048] After the positioning welding is completed, the internal welds are manually welded by intermittent welding. The length of each welding section is about 100mm, and the interval is 150-300mm to ensure the overall rigidity of the boom and avoid deformation during the hoisting and welding process, and then complete the assembly of the boom assembly. The welding of positioning welding and internal welds can ensure the overall rigidity of the structural parts, facilitate hoisting and clamping, and at the same time reduce some welding deformation, improve the welding quality of the structural parts, and effectively improve the strength and service life of the structural parts.
[0049] Step 2: Use a welding robot to weld the butt weld.
[0050] In the welding of excavator structural parts, the butt weld plays the role of connecting the parent material and participates in the overall strength of the structural parts. The welding quality of the butt weld is related to the overall quality and strength of the welded structural parts.
[0051] Specifically, taking the boom as an example, it includes the cover plate butt weld and the side plate butt weld, such as Figure 3 As shown, first, the arc-starting and arc-ending plates are assembled and fixed at the ends of the first cover plate butt weld 5 and the second cover plate butt weld 6. Since the current and voltage at the arc starting and arc ending positions of the weld are unstable, welding defects are easily caused. The arc-starting and arc ending plates at the ends of the cover plate butt welds can lead the arc starting and arc ending positions of the welds out of the weld area, avoiding defects at the ends of the formal welds and improving the quality of the welds. Specifically, the steel plate is combined with the ceramic block and fixed to the bottom of the butt weld end by spot welding.
[0052] Then, a welding robot is used to weld all the butt welds of the boom, including the first side plate butt weld 1, the second side plate butt weld 2, the third side plate butt weld 3, the fourth side plate butt weld 4, the first cover plate butt weld 5 and the second cover plate butt weld 6, where the arc starting and arc ending positions of the two cover plate butt welds are located on the arc starting and extinguishing plates. After the butt welds are welded, the end position can be processed in advance to eliminate welding defects, which is conducive to the subsequent fillet weld welding and the overall efficiency improvement of the structural parts.
[0053] During the butt weld process, priming, filling and capping are performed alternately to avoid excessive heat input affecting the quality of the weld. Specifically, filling is performed after all welds are primed. For welds that need to be filled with more than 2 layers, every 2 layers are filled once and then the remaining welds are welded. After all the filling is completed, capping is performed to avoid excessive welding heat input, effectively control the interlayer temperature, and thus improve the welding quality. The working current of the welding robot is 380-460A, the working voltage is 28-26V, and the welding speed is controlled at 14-45cm / min. In this embodiment, the optimal effects of filling amount, heat input value, penetration depth, etc. can be achieved by controlling the welding parameters, thereby maximizing efficiency, quality, and cost.
[0054] Step 3: Process the weld end.
[0055] like Figure 2 As shown, after the butt weld is completed, the arc initiation and extinguishing plate is planed off, and all butt weld ends are polished and cleaned to an ideal state to ensure that there are no defects in the butt weld ends, which is beneficial to the subsequent welding process and improves the overall quality and efficiency of the structural parts.
[0056] In this embodiment, the welding of the butt weld and the fillet weld are performed separately, and the welding of the butt weld is completed using an arc-initiating and extinguishing plate. After the butt weld is completed, the weld end can be processed to an ideal state in advance to facilitate the subsequent welding of the fillet weld.
[0057] Step 4: Weld the fillet weld.
[0058] After the weld end is processed, the boom is welded by robot. After all welds are primed, they are filled. For welds that need to be filled with more than 2 layers, they are filled once every 2 layers and then the remaining welds are welded. After the filling is completed, the surface is covered to avoid excessive heat input affecting the quality of the weld. Since the butt weld joints have been processed in advance, the two weld joints do not need to be disconnected and can be welded directly, so that the fillet welds at the T-shaped structure can be welded continuously without disconnection and redundant joints, effectively reducing the risk of failure.
[0059] During this process, the welding robot's operating current is 380-460A, the operating voltage is 28-26V, and the dry extension is 20-30mm.
[0060] In order to further avoid welding defects and improve the overall strength of the boom, manual welding and grinding are performed after the robot welding is completed.
[0061] Specifically, the robot will manually repair the unwelded position, and the positioner will be used to adjust various welding postures to ensure welding quality. After the repair welding is completed, all butt joints will be polished. After flaw detection, the defective position will be repaired.
[0062] Step 5: annealing heat treatment is performed on the welded structural parts.
[0063] During the welding process, due to the overall rigidity of the structural parts and the limitations of the tooling fixtures, the welding stress cannot be released after the boom welding is completed and remains in the structural parts. Since the boom needs to withstand very high dynamic loads when working, stress concentration will occur, resulting in a decrease in fatigue strength and affecting the service life of the boom. In this embodiment, stress relief annealing can be used to reduce the welding residual stress in the boom structural parts and improve the quality and fatigue resistance of the structural parts.
[0064] Specifically, the heat treatment process is:
[0065] (1) Stage 1: placing the welded boom in a heat treatment furnace and heating the boom to a first temperature at a first heating rate;
[0066] (2) Stage 2: heating the boom to a second temperature at a second heating rate, wherein the second heating rate is less than the first heating rate, and the second temperature is higher than the first temperature;
[0067] (3) Stage 3: Insulation;
[0068] (4) Stage 4: Cooling to a third temperature at a third rate in the heat treatment furnace;
[0069] (5) Stage 5: Remove the boom from the heat treatment furnace and cool to room temperature.
[0070] like Figure 4 As shown, in stage 1, the first heating rate is 200°C / hour, the first temperature is 300°C, and the bucket arm is heated from room temperature to 300°C at 200°C / hour in the heat treatment furnace.
[0071] In stage 2, the temperature is increased based on the first temperature. The second heating rate is 160℃ / hour and the second temperature is 620±20℃. The boom is heated from 300℃ to 620±20℃ at 160℃ / hour, which can reduce the yield strength of the boom and release stress through plastic deformation inside the structure, thereby reducing the residual stress of the structural parts, effectively improving the fatigue resistance of the boom and extending its service life.
[0072] In stage 3, the boom is kept warm at the second temperature in the heat treatment furnace. The holding time is determined based on the steel material and simulation calculations. In this embodiment, the boom is kept warm at 620±20°C for 3 hours to complete the local plastic deformation and stress release process of the structure.
[0073] In stage 4, the third rate is 100°C / hour, the third temperature is 200°C, and the cold cutting is slow to avoid generating new residual stress.
[0074] In stage 5, the 200°C stick is removed from the heat treatment furnace and air-cooled to room temperature.
[0075] Step 6: perform machining.
[0076] After the heat treatment annealing is completed, the deformation of the structural parts tends to be stable, the residual stress is reduced, and finally mechanical processing is carried out to ensure the accuracy of the processing size.
[0077] In this embodiment, by applying and controlling the welding process throughout the entire production process of the boom, the welding residual stress of the material is reduced, the strength and service life of the structural parts are effectively improved, the process quality risk and usage quality risk of the welded parts are reduced, and the method can also be applied to the welding processing of other structural parts of the excavator.
[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for welding an excavator structural part, characterized in that: include: Step 1, assemble the components in sequence and perform positioning welding to fix the positions of the components; Step 2, welding the butt weld using a welding robot; Step 3, processing the butt weld joint; Step 4, welding the fillet weld; Step 5: annealing heat treatment.
2. The method for welding an excavator structure according to claim 1, characterized in that: In step 1, adjust the butt weld gap to 4-7mm and the fillet weld gap to no more than 2mm.
3. The method for welding an excavator structure according to claim 1, characterized in that: In step 1, positioning welding is performed by spot welding, and then the internal weld is welded by intermittent welding; the positioning welding length is 30-50mm, and the weld foot is 5mm.
4. The method for welding an excavator structure according to claim 1, characterized in that: In step 2, before welding the butt weld, an arc starting and arc ending plate is installed to lead the arc starting and arc ending positions of the butt weld to the arc starting and arc ending plate outside the weld area.
5. The method for welding an excavator structure according to claim 4, characterized in that: In step 2, after the butt weld is completed, the arc-starting and extinguishing plates are planed off, and the weld ends are polished and cleaned.
6. The method for welding an excavator structure according to claim 1, characterized in that: In step 2 or step 3, base coating, filling and covering are performed alternately to avoid excessive heat input at the welding position, facilitate control of interlayer temperature and thus ensure the quality of the weld.
7. The method for welding an excavator structure according to claim 6, characterized in that: For welds that are filled with more than 2 layers, fill every 2 layers and then weld the remaining welds. After filling is completed, cover the surface.
8. The method for welding an excavator structure according to claim 1, characterized in that: In step 4, the heat treatment process includes: Placing the welded structural component in a heat treatment furnace, and heating the structural component to a first temperature at a first heating rate; heating the structural member to a second temperature at a second heating rate, the second heating rate being less than the first heating rate, the second temperature being higher than the first temperature; Keeping the structural member warm at the second temperature in a heat treatment furnace; Cooling the heat treatment furnace to a third temperature at a third rate; The structural parts are taken out of the heat treatment furnace and cooled to room temperature.
9. The method for welding an excavator structure according to claim 8, characterized in that: The first heating rate is 200°C / hour and the first temperature is 300°C.
10. The method for welding an excavator structure according to claim 8, characterized in that: The second heating rate is 160°C / hour, and the second temperature is 620±20°C.