CMP (chemical mechanical polishing) method

CN119017247APending Publication Date: 2024-11-26BEIJING SEMICORE MICROELECTRONICS EQUIPMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411346137.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-26

Smart Images

  • Figure CN119017247A_ABST
    Figure CN119017247A_ABST
Patent Text Reader

Abstract

The invention relates to a CMP (chemical mechanical polishing) method. The CMP method comprises the following steps: placing a wafer to be polished on a polishing pad; a silicon nitride film layer, an oxide film layer and a polycrystalline silicon film layer are sequentially arranged on the surface of the wafer; a first grinding step: introducing a first grinding liquid with a first film layer selection ratio to grind the wafer, and removing the polycrystalline silicon film layer; a second grinding step: introducing a second grinding liquid with a second film layer selection ratio to grind the wafer, and removing the oxide film layer; the friction coefficient of the wafer to the grinding pad is obtained in real time, and a friction coefficient curve is obtained; when the change rate of the friction coefficient is smaller than a first preset change rate, the first grinding step is stopped; when the change rate of the friction coefficient is smaller than a second preset change rate, the second grinding step is stopped; and cleaning the wafer. According to the CMP grinding method provided by the invention, the CMP process efficiency, quality, stability and productivity for different film layers on the wafer surface can be improved, the product yield is improved, and the process cost is saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor technology, and in particular to a CMP grinding method. Background Art

[0002] Highly integrated integrated circuit manufacturing often uses chemical mechanical polishing (CMP) to flatten the wafer. With the continuous upgrading of chip manufacturing technology, higher requirements are placed on the CMP process. The existing CMP process usually removes different material layers on the surface of the wafer in a step-by-step fixed time method. After the CMP process is completed, a film thickness measurement device is generally used to monitor the film layer on the surface of the wafer to obtain data on the wafer film removal rate. The polishing time is calculated based on the removal rate to remove unnecessary material layers on the wafer surface.

[0003] The grinding rate of the existing CMP process is greatly affected by consumables. It is difficult to obtain precise thickness control by the fixed-time grinding method, which may cause over-grinding or under-grinding of the wafer, resulting in low efficiency of the CMP process for different material layers on the wafer surface, poor process quality and stability, and thus low product yield and high process cost. In particular, over-grinding will cause serious dishing of the device's open area, resulting in isolation failure and affecting the reliability of the device. For example, when CMP is insufficiently ground, the residual silicon oxide film on the silicon nitride film will prevent the next process from removing the silicon nitride film, resulting in residual silicon nitride on the active area, causing the device to fail to work.

[0004] Therefore, a CMP grinding method is needed to better control the thickness of the film layer on the wafer surface after the CMP process, thereby improving the CMP process efficiency for different film layers on the wafer surface, while improving the quality, stability and productivity of the CMP process, avoiding excessive or insufficient wafer grinding, improving product yield and saving process costs. Summary of the invention

[0005] Therefore, the present invention provides a CMP polishing method to solve the problem that the polishing rate of the existing CMP process is greatly affected by consumables, and the fixed time polishing method is difficult to obtain precise thickness control, which may cause over-polishing or under-polishing of the wafer, resulting in low CMP process efficiency for different film layers on the wafer surface, poor process quality and stability, and further leading to low product yield and high process cost.

[0006] The present invention provides a CMP grinding method, comprising:

[0007] Placing a wafer to be polished on a polishing pad; a silicon nitride film layer, an oxide film layer to be removed, and a polysilicon film layer to be removed are sequentially present on a surface of the wafer facing the polishing pad;

[0008] A first grinding step, introducing a first grinding liquid to grind the wafer to remove the polysilicon film layer; the first grinding liquid has a first film layer selectivity;

[0009] a second grinding step, introducing a second grinding liquid to grind the wafer to remove the oxide film layer; the second grinding liquid has a second film layer selectivity;

[0010] At least in the first grinding step and the second grinding step, the friction coefficient of the wafer to the grinding pad is acquired in real time to obtain a friction coefficient curve;

[0011] When the rate of change of the friction coefficient is less than a first preset rate of change, the first grinding step is stopped; or: when the grinding time reaches a first termination time, the first grinding step is stopped;

[0012] When the rate of change of the friction coefficient is less than a second preset rate of change, the second grinding step is stopped; or: when the grinding time reaches a second end time, the second grinding step is stopped;

[0013] The wafer is cleaned.

[0014] Optionally, when the rate of change of the friction coefficient is less than a first preset rate of change, the step of stopping the first grinding step includes:

[0015] Monitoring the friction coefficient curve in real time within a first monitoring time period;

[0016] Setting a first stop window, when the change rate of the friction coefficient within the time interval of the first stop window is less than a first preset change rate, entering a first supplementary grinding stage;

[0017] After maintaining the first supplementary grinding time, the first grinding step is stopped.

[0018] Optionally, the first termination duration is 160s to 300s;

[0019] The first monitoring duration is 100s to 290s;

[0020] The first supplementary grinding time is 10s to 60s;

[0021] The first preset change rate is 0.01 / s to 0.1 / s.

[0022] Optionally, when the rate of change of the friction coefficient is less than a second preset rate of change, the step of stopping the second grinding step includes:

[0023] monitoring the friction coefficient curve in real time during a second monitoring period;

[0024] Setting a second stop window, when the change rate of the friction coefficient within the time interval of the second stop window is less than a second preset change rate, entering the second supplementary grinding stage;

[0025] After the second supplementary grinding time period is maintained, the second grinding step is stopped.

[0026] Optionally, the second termination duration is 160s to 300s;

[0027] The second monitoring duration is 100s to 290s;

[0028] The second supplementary grinding time is 10s to 60s;

[0029] The second preset change rate is 0.01 / s to 0.1 / s.

[0030] Optionally, the first film layer selection ratio is polysilicon film layer to oxide film layer=800:1-850:1;

[0031] The second film layer selection ratio is oxide film layer to silicon nitride film layer=200:1-220:1.

[0032] Optionally, the first grinding liquid has a particle size of 40 μm to 120 μm, a solid content of 3 wt% to 30 wt%, and a pH of 7 to 10;

[0033] The particle size of the second grinding liquid is 70 μm to 300 μm, the solid content is 1 wt% to 10 wt%, and the pH value is 8 to 12.

[0034] Optionally, in the step of cleaning the wafer,

[0035] Deionized water is used to remove the second polishing liquid remaining on the surface of the wafer.

[0036] Optionally, before the first grinding step, the process further comprises:

[0037] The film thickness on the wafer surface is acquired in real time to obtain thickness curves of different film layers.

[0038] Optionally, the step of acquiring the film thickness on the surface of the wafer in real time and obtaining thickness curves of different film layers includes:

[0039] By scanning the film layer on the wafer surface and performing spectral fitting, a thickness curve graph of different film layers on the wafer surface can be obtained for real-time monitoring.

[0040] The technical solution of the present invention has the following advantages:

[0041] The CMP grinding method provided by the present invention selects corresponding grinding liquid selection ratios for different film layers on the surface of the wafer, and can accurately judge whether the film layer is completely removed by real-time monitoring of the change rate of the friction coefficient of the wafer to the grinding pad, thereby avoiding excessive or insufficient grinding of the wafer, and can also better control the wafer surface after the CMP process to have a stable film layer thickness, thereby improving the CMP process efficiency for different film layers on the surface of the wafer, while improving the quality, stability and productivity of the CMP process, avoiding excessive or insufficient grinding of the wafer, improving product yield, reducing process time, and saving process costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0043] Figure 1 A schematic diagram of a CMP polishing method according to an embodiment of the present invention;

[0044] Figure 2 A schematic diagram of the structure of a wafer to be ground according to an embodiment of the present invention;

[0045] Figure 3 A schematic diagram of film removal in a CMP polishing method according to an embodiment of the present invention;

[0046] Figure 4 A schematic diagram of a specific process of a CMP polishing method according to an embodiment of the present invention;

[0047] Figure 5 A schematic diagram of a friction coefficient curve of a CMP polishing method according to an embodiment of the present invention;

[0048] Figure 6 FIG. 1 is a schematic diagram of a thickness curve of a polysilicon film layer in a CMP polishing method according to an embodiment of the present invention.

[0049] Description of reference numerals:

[0050] 1-wafer; 10-silicon; 11-silicon nitride film layer; 12-oxide film layer; 13-polysilicon film layer; 2-polishing pad; E1-stop window; E2-start window. DETAILED DESCRIPTION

[0051] In order to solve the problem that the grinding rate of the existing CMP process is greatly affected by consumables, the fixed time grinding method is difficult to obtain accurate thickness control, which may cause over-grinding or under-grinding of the wafer, resulting in low CMP process efficiency for different film layers on the wafer surface, poor process quality and stability, and thus low product yield and high process cost, the present invention provides a CMP grinding method, comprising: placing a wafer to be ground on a grinding pad; a silicon nitride film layer, an oxide film layer to be removed and a polysilicon film layer to be removed are sequentially present on a side surface of the wafer facing the grinding pad; a first grinding step, introducing a first grinding liquid to grind the wafer to remove the polysilicon film layer; the first grinding liquid has a first film layer selection ratio; a second grinding step, introducing a second grinding liquid to grind the wafer to remove the oxide film layer; the second grinding liquid has a second film layer selection ratio; at least in the first grinding step and the second grinding step, the friction coefficient of the wafer to the grinding pad is obtained in real time to obtain a friction coefficient curve; when the rate of change of the friction coefficient is less than a first preset rate of change, the first grinding step is stopped; or: when the grinding time reaches a first termination time, the first grinding step is stopped; when the rate of change of the friction coefficient is less than a second preset rate of change, the second grinding step is stopped; or: when the grinding time reaches a second termination time, the second grinding step is stopped; and the wafer is cleaned.

[0052] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. In the description of the present invention, it should be noted that the terms "first", "second" and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0053] Example 1

[0054] like Figure 1 As shown, this embodiment provides a CMP polishing method, comprising:

[0055] S101, placing a wafer to be ground on a grinding pad; a silicon nitride film layer, an oxide film layer to be removed, and a polysilicon film layer to be removed are sequentially disposed on a surface of the wafer facing the grinding pad, such as Figure 2 As shown;

[0056] S102, a first grinding step, introducing a first grinding liquid to grind the wafer to remove the polysilicon film layer; the first grinding liquid has a first film layer selectivity;

[0057] In a specific implementation, a wafer and a grinding pad are placed in a first polishing plate, and a first grinding liquid having a suitable first film layer selection ratio is selected according to the polysilicon film layer to be removed in the first grinding step, so that the polysilicon film layer can be completely removed. Figure 3 shown.

[0058] S102-1, obtaining the friction coefficient of the wafer to the grinding pad in real time to obtain a friction coefficient curve; when the change rate of the friction coefficient is less than a first preset change rate, stopping the first grinding step; or: when the grinding time reaches a first end time, stopping the first grinding step;

[0059] In this embodiment, GEGV Horizon series software can be selected for process control, and the Motortorque function of the software is used to obtain the friction coefficient of the wafer to the polishing pad in real time, and obtain a friction coefficient curve.

[0060] In a specific implementation, since different wafer film layers have different polishing friction coefficients on the grinding pad, the removal of the polysilicon film layer can be monitored in real time by monitoring the rate of change of the friction coefficient in real time. When the rate of change of the friction coefficient is less than the first preset rate of change, it means that the polysilicon film layer has been basically removed. In another embodiment, when the grinding time reaches the first termination time, the first grinding step is stopped.

[0061] In this embodiment, the Motor torque function can be used to adjust various parameters on the Endpoint function and set multiple windows on the friction coefficient curve; the windows are used to capture characteristic curves of different film layers on the wafer surface to achieve a grabbing and stopping function.

[0062] S103, a second grinding step, introducing a second grinding liquid to grind the wafer to remove the oxide film layer; the second grinding liquid has a second film layer selectivity;

[0063] In the specific implementation, the wafer and the grinding pad are moved into the second polishing plate, and according to the oxide film layer to be removed in the second grinding step, a second grinding liquid with a suitable second film layer selection ratio is selected so that the oxide film layer can be completely removed, such as Figure 3 shown.

[0064] S103-1, acquiring the friction coefficient of the wafer to the grinding pad in real time to obtain a friction coefficient curve; when the change rate of the friction coefficient is less than a second preset change rate, stopping the second grinding step; or: when the grinding time reaches a second end time, stopping the second grinding step;

[0065] In a specific implementation, since different wafer film layers have different polishing friction coefficients on the grinding pad, the removal of the oxide film layer can be monitored in real time by monitoring the rate of change of the friction coefficient in real time. When the rate of change of the friction coefficient is less than the first preset rate of change, it means that the oxide film layer has been basically removed at this time. In another embodiment, when the grinding time reaches the second end time, the second grinding step is stopped.

[0066] S104, cleaning the wafer.

[0067] In the specific implementation, the wafer and the grinding pad are moved into the third polishing plate to remove the residual grinding liquid on the surface of the wafer. Figure 3 shown.

[0068] The CMP polishing method provided in this embodiment selects the corresponding polishing liquid selection ratio for different film layers on the wafer surface, and can accurately determine whether the film layer is completely removed by real-time monitoring the rate of change of the friction coefficient of the wafer to the polishing pad, thereby avoiding over- or under-polishing of the wafer. It can also better control the wafer surface to have a stable film thickness after the CMP process, thereby improving the CMP process efficiency for different film layers on the wafer surface, while improving the quality, stability and productivity of the CMP process, avoiding over- or under-polishing of the wafer, improving product yield, reducing process time, and saving process costs.

[0069] Further, in some embodiments, when the rate of change of the friction coefficient is less than a first preset rate of change, the step of stopping the first grinding step includes:

[0070] Monitoring the friction coefficient curve in real time within a first monitoring time period;

[0071] Setting a first stop window, when the change rate of the friction coefficient within the time interval of the first stop window is less than a first preset change rate, entering a first supplementary grinding stage;

[0072] After maintaining the first supplementary grinding time, the first grinding step is stopped.

[0073] In specific implementation, if the polishing liquid has a high removal rate for the polysilicon film layer, the curve will form an upward or downward trend. If the trend is almost flat, it means that the polishing liquid has a very low removal rate for the polysilicon film layer, indicating that the polysilicon film layer is completely removed. Therefore, by setting the first stop window, when the rate of change of the friction coefficient within the time interval of the first stop window is less than the first preset rate of change, the polysilicon film layer has been basically removed. In order to ensure the complete removal of the polysilicon film layer, the first supplementary polishing stage is entered; after maintaining the first supplementary polishing time, the first polishing step is stopped.

[0074] The time interval of the first stop window can be set according to actual conditions, such as 3s, 5s, etc., which is not limited in this embodiment. For example, when the change rate of the friction coefficient within the time interval of 3s of the first stop window is less than the first preset change rate, the first supplementary grinding stage is entered.

[0075] Further, in some embodiments, the sum of the first monitoring duration and the first supplementary grinding duration is less than or equal to the first termination duration.

[0076] In some embodiments, a start window is also provided. When the first grinding step begins, a start window appears on the curve. When the window appears, the surface wafer has begun to be ground. When the curve slowly extends and enters from the left side of the window, it means that the grinding has begun. The condition of the curve stop window can be set in the parameters. The curve can be selected to stop the grinding process when it is above, to the right or below the window.

[0077] In some embodiments, multiple stop windows can be set according to actual conditions, and the stop windows can be set to left-in-right-out, left-in-bottom-out, or left-in-top-out.

[0078] Further, in some embodiments, the first termination duration is 160s to 300s;

[0079] The first monitoring duration is 100s to 290s;

[0080] The first supplementary grinding time is 10s to 60s;

[0081] The first preset change rate is 0.01 / s to 0.1 / s.

[0082] In one embodiment, the Endpoint time parameter may be set as:

[0083] 1)Notch Filter~Period to Average(2~30) / filter order(2~25);

[0084] 2)Lowpass Filter~Time Constant(3~15);

[0085] 3) Median Filter~Time Constant(2~12);

[0086] 4)Torque Calibration~Cali Valuc Min(5~25) / Max(20~80);

[0087] 5) Set the time to By time: 160s, Endpoint time: 120s, OP time: 30s.

[0088] The parameters are set as follows: the first termination time is 160 seconds, the first monitoring time is 120 seconds, the first supplementary grinding time is 30 seconds, and the first preset change rate is set as 0.01 / s.

[0089] In a specific implementation, in one example, the friction coefficient curve is monitored within the first monitoring time of 120 seconds. When the change rate of the friction coefficient is less than the first preset change rate, it indicates that the gripping is successful, and the first supplementary grinding stage is entered. The first supplementary grinding time is continued for 30 seconds, and then the first grinding step is stopped. At this time, the total duration of the first grinding step is less than 150 seconds. For example, if the gripping is successful at the 100th second, the total duration of the first grinding step is less than 130 seconds.

[0090] In another example, the friction coefficient curve is monitored within the first monitoring time of 120s. When the change rate of the friction coefficient is continuously greater than or equal to the first preset change rate, it indicates that the gripping and stopping fails. At this time, grinding is performed according to the first termination time. When the grinding time reaches the first termination time, the first grinding step is stopped. At this time, the total duration of the first grinding step is 160s.

[0091] This embodiment combines the Motor torque function with the Endpoint time function to control the first end time, the first monitoring time, and the first supplementary grinding time of the first grinding step, so as to accurately and safely remove the unnecessary polysilicon film layer on the wafer surface and avoid the problem of over-grinding or under-grinding.

[0092] Further, in some embodiments, when the rate of change of the friction coefficient is less than a second preset rate of change, the step of stopping the second grinding step includes:

[0093] monitoring the friction coefficient curve in real time during a second monitoring period;

[0094] Setting a second stop window, when the change rate of the friction coefficient within the time interval of the second stop window is less than a second preset change rate, entering the second supplementary grinding stage;

[0095] After the second supplementary grinding time period is maintained, the second grinding step is stopped.

[0096] In specific implementation, if the polishing liquid has a high removal rate for the oxide film, the curve will form an upward or downward trend. If the trend is almost flat, it means that the polishing liquid has a very low removal rate for the oxide film, indicating that the oxide film is completely removed. Therefore, by setting a second stop window and monitoring the change rate of the friction coefficient within the time interval of the second stop window is less than the second preset change rate, the oxide film has been basically removed at this time. In order to ensure the complete removal of the oxide film, the second supplementary grinding stage is entered; after maintaining the second supplementary grinding time, the second grinding step is stopped.

[0097] The time interval of the second stop window can be set according to actual conditions, such as 3s, 5s, etc., which is not limited in this embodiment. For example, when the change rate of the friction coefficient within the time interval of 3s of the second stop window is less than the second preset change rate, the second supplementary grinding stage is entered.

[0098] Further, in some embodiments, the sum of the second monitoring duration and the second supplementary grinding duration is less than or equal to the second termination duration.

[0099] Further, in some embodiments, the second termination time is 160s to 300s;

[0100] The second monitoring duration is 100s to 290s;

[0101] The second supplementary grinding time is 10s to 60s;

[0102] The second preset change rate is 0.01 / s to 0.1 / s.

[0103] In one embodiment, the Endpoint time parameter may be set as:

[0104] 1)Notch Filter~Period to Average(2~30) / filter order(2~25);

[0105] 2)Lowpass Filter~Time Constant(3~15);

[0106] 3) Median Filter~Time Constant(2~12);

[0107] 4)Torque Calibration~Cali Valuc Min(5~25) / Max(20~80);

[0108] 5) Set the time to By time: 160s, Endpoint time: 120s, OP time: 30s.

[0109] The parameters are set as follows: the second termination time of the second grinding step is 160 seconds, the second monitoring time is 120 seconds, the first supplementary grinding time is 30 seconds, and the second preset change rate is set as 0.01 / s.

[0110] In a specific implementation, in one example, the friction coefficient curve is monitored within the second monitoring time of 120 seconds. When the change rate of the friction coefficient is less than the second preset change rate, it indicates that the gripping is successful, and the second supplementary grinding stage is entered. The second supplementary grinding time is continued for 30 seconds, and then the second grinding step is stopped. At this time, the total duration of the second grinding step is less than 150 seconds. For example, if the gripping is successful at the 100th second, the total duration of the second grinding step is less than 130 seconds.

[0111] In another example, the friction coefficient curve is monitored within the second monitoring time of 120s. When the change rate of the friction coefficient is continuously greater than or equal to the second preset change rate, it indicates that the gripping and stopping fails. At this time, grinding is performed according to the second termination time. When the grinding time reaches the second termination time, the second grinding step is stopped. At this time, the total duration of the second grinding step is 160s.

[0112] This embodiment combines the Motor torque function with the Endpoint time function to control the first end time, the second monitoring time, and the second supplementary grinding time of the second grinding step, thereby accurately and safely removing unnecessary oxide film layers on the wafer surface and avoiding the problem of over-grinding or under-grinding.

[0113] Furthermore, in some embodiments, the first film layer selection ratio is polysilicon film layer to oxide film layer=800:1-850:1;

[0114] The second film layer selection ratio is oxide film layer to silicon nitride film layer=200:1-220:1.

[0115] When the first film layer selection ratio is polysilicon film layer to oxide film layer = 800:1-850:1, the polysilicon film layer can be better polished and removed while ensuring that the surface of the remaining oxide film layer will not be uneven.

[0116] When the selection ratio of the second film layer is oxide film layer to silicon nitride film layer = 200:1 to 220:1, the oxide film layer can be better polished and removed while ensuring that the surface of the remaining silicon nitride film layer will not be uneven.

[0117] In one embodiment, the oxide film layer is a silicon oxide film layer. Under the same polishing parameters and consistent with the consumables, the polishing rate of the polysilicon polishing liquid on the polysilicon film layer wafer is about 8000A / min, and the polishing rate of the polysilicon polishing liquid on the silicon oxide film layer wafer is about 10A / min, so the first film layer selection ratio of the first polishing liquid is polysilicon film layer to oxide film layer = 800:1; and the polishing rate of the silicon oxide polishing liquid on the silicon oxide film layer wafer is about 2000A / min, and the polishing rate of the silicon oxide polishing liquid on the silicon nitride film layer wafer is about 10A / min, so the first film layer selection ratio of the first polishing liquid is oxide film layer to silicon nitride film layer = 200:1.

[0118] Further, in some embodiments, the particle size of the first grinding liquid is 40 μm to 120 μm, the solid content is 3 wt % to 30 wt %, and the pH is 7 to 10;

[0119] The particle size of the second grinding liquid is 70 μm to 300 μm, the solid content is 1 wt% to 10 wt%, and the pH value is 8 to 12.

[0120] Furthermore, in some embodiments, in the step of cleaning the wafer,

[0121] Deionized water is used to remove the second polishing liquid remaining on the surface of the wafer.

[0122] In a specific implementation, deionized water is used to remove the residual grinding liquid on the surface of the wafer, thereby reducing the cleaning pressure and improving the roughness of the wafer surface.

[0123] Furthermore, in some embodiments, before the first grinding step, the process further includes:

[0124] The film thickness on the wafer surface is acquired in real time to obtain thickness curves of different film layers.

[0125] Furthermore, in some embodiments, the step of acquiring the film thickness on the surface of the wafer in real time and obtaining thickness curves of different film layers includes:

[0126] By scanning the film layer on the wafer surface and performing spectral fitting, a thickness curve graph of different film layers on the wafer surface can be obtained for real-time monitoring.

[0127] In this embodiment, the white light function can be used to transmit the signal to the endpoint detection (EPD), and the EPD is used to scan the film layer on the surface of the wafer and perform spectral fitting on it to obtain a thickness curve graph for real-time monitoring of different film layers on the surface of the wafer.

[0128] In a specific implementation, the different film layers on the surface of the wafer include non-metallic film layers, such as polysilicon film layers, oxide film layers, etc. In the grinding step of removing non-metallic film layers such as polysilicon film layers and oxide film layers, the white light function is used to transmit the signal to the EPD, and the EPD is used to scan the non-metallic film layer on the surface of the wafer and perform spectral fitting to obtain a thickness curve for real-time monitoring of the non-metallic film layer on the surface of the wafer. As the grinding progresses, at the same time, the thickness of the non-metallic film layer at different positions on the top layer of the wafer is monitored, and the points of thickness at different positions are obtained and connected into a curve. Select different times (t1~t n ), different curves are obtained. As the grinding progresses, the thickness of the non-metallic film layer gradually decreases until it drops to 0A. According to the thickness curve, the process of the non-metallic film layer changing from thick to thin to no thickness over time can be monitored.

[0129] Example 2

[0130] refer to Figure 4 This embodiment provides a specific process of a CMP polishing method, including steps S201-S204:

[0131] S201, placing a wafer to be ground on a grinding pad; a silicon nitride film layer, an oxide film layer to be removed, and a polysilicon film layer to be removed are sequentially present on a surface of the wafer facing the grinding pad.

[0132] S202, placing the wafer and the grinding pad in the first polishing plate, performing the first grinding step, introducing the first grinding liquid to grind the wafer to remove the polysilicon film layer; the first grinding liquid has a first film layer selectivity. The particle size of the first grinding liquid is 40 to 120, the solid content is 3 wt% to 30 wt%, and the pH is 7 to 10; the first film layer selectivity is polysilicon film layer to oxide film layer = 800:1.

[0133] S202-1, acquiring the friction coefficient of the wafer to the grinding pad in real time to obtain a friction coefficient curve; monitoring the friction coefficient curve in real time within a first monitoring period; setting a first stop window, and entering a first supplementary grinding stage when the rate of change of the friction coefficient within the time interval of the first stop window is less than a first preset rate of change; after maintaining the first supplementary grinding time, stopping the first grinding step; or: when the grinding time reaches a first termination time, stopping the first grinding step.

[0134] Select GEGV Horizon series software for process control, use the Motor torque function of the software to obtain the friction coefficient of the wafer to the polishing pad in real time, and obtain the friction coefficient curve, such as Figure 5 As shown, E1 is the stop window and E2 is the start window.

[0135] Set the Endpoint time parameters for the first grinding step to:

[0136] 1)Notch Filter~Period to Average(2~30) / filter order(2~25);

[0137] 2)Lowpass Filter~Time Constant(3~15);

[0138] 3) Median Filter~Time Constant(2~12);

[0139] 4)Torque Calibration~Cali Valuc Min(5~25) / Max(20~80);

[0140] 5) Set the time to By time: 160s, Endpoint time: 120s, OP time: 30s.

[0141] S202-2, by scanning the film layer on the surface of the wafer and performing spectrum fitting on it, a thickness curve graph of the polysilicon film layer on the surface of the wafer is obtained for real-time monitoring. The signal is transmitted to the EPD using the white light function, and the film layer on the surface of the wafer is scanned by the EPD and performed spectrum fitting on it, so as to obtain a thickness curve graph of the polysilicon film layer on the surface of the wafer for real-time monitoring, such as Figure 6 As shown in the figure, as the grinding progresses, at the same time, the thickness of the polysilicon film layer at different positions is monitored, and the points of thickness at different positions are obtained, which are connected into a curve to obtain a curve in the figure. Different curves are obtained by selecting different moments (t1~t9). As the grinding progresses, the thickness of the polysilicon film layer gradually decreases from 3200A at t1 to 1400A-1500A at t9, and finally to 0A. Figure 6 The process of the polysilicon film layer changing from thick to thin to no thickness over time can be monitored.

[0142] S203, moving the wafer and the grinding pad into the second polishing plate, performing a second grinding step, introducing a second grinding liquid to grind the wafer to remove the oxide film layer; the second grinding liquid has a second film layer selectivity. The particle size of the second grinding liquid is 70 to 300, the solid content is 1 wt% to 10 wt%, and the pH is 8 to 12; the second film layer selectivity is oxide film layer to silicon nitride film layer = 200:1.

[0143] S203-1, acquiring the friction coefficient of the wafer to the grinding pad in real time to obtain a friction coefficient curve; monitoring the friction coefficient curve in real time within a second monitoring period; setting a second stop window, and entering a second supplementary grinding stage when the rate of change of the friction coefficient within the time interval of the second stop window is less than a second preset rate of change; after maintaining the second supplementary grinding time, stopping the second grinding step; or: stopping the second grinding step when the grinding time reaches the second termination time.

[0144] Select GEGV Horizon series software for process control, use the Motor torque function of the software to obtain the friction coefficient of the wafer to the polishing pad in real time, and obtain the friction coefficient curve, such as Figure 5 As shown, E1 is the stop window and E2 is the start window.

[0145] Set the Endpoint time parameters for the second grinding step to:

[0146] 1)Notch Filter~Period to Average(2~30) / filter order(2~25);

[0147] 2)Lowpass Filter~Time Constant(3~15);

[0148] 3) Median Filter~Time Constant(2~12);

[0149] 4)Torque Calibration~Cali Valuc Min(5~25) / Max(20~80);

[0150] 5) Set the time to By time: 160s, Endpoint time: 120s, OP time: 30s.

[0151] S203-2, by scanning the film layer on the surface of the wafer and performing spectrum fitting, a thickness curve graph of the oxide film layer on the surface of the wafer is obtained for real-time monitoring. The signal is transmitted to the EPD using the white light function, and the film layer on the surface of the wafer is scanned by the EPD and performed spectrum fitting, to obtain a thickness curve graph of the oxide film layer on the surface of the wafer for real-time monitoring.

[0152] S204, moving the wafer and the grinding pad into a third polishing plate, and using deionized water to remove the second grinding liquid remaining on the surface of the wafer.

[0153] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A CMP polishing method, characterized in that: include: placing the wafer to be ground on the grinding pad; A silicon nitride film layer, an oxide film layer to be removed, and a polysilicon film layer to be removed are sequentially present on a surface of the wafer facing the polishing pad; A first grinding step, introducing a first grinding liquid to grind the wafer to remove the polysilicon film layer; the first grinding liquid has a first film layer selectivity; a second grinding step, introducing a second grinding liquid to grind the wafer to remove the oxide film layer; the second grinding liquid has a second film layer selectivity; At least in the first grinding step and the second grinding step, the friction coefficient of the wafer to the grinding pad is acquired in real time to obtain a friction coefficient curve; When the rate of change of the friction coefficient is less than a first preset rate of change, stopping the first grinding step; Or: when the grinding time reaches a first end time, stopping the first grinding step; When the rate of change of the friction coefficient is less than a second preset rate of change, stopping the second grinding step; Or: when the grinding time reaches the second end time, stopping the second grinding step; The wafer is cleaned.

2. The CMP polishing method according to claim 1, characterized in that: The step of stopping the first grinding step when the rate of change of the friction coefficient is less than a first preset rate of change includes: Monitoring the friction coefficient curve in real time within a first monitoring time period; Setting a first stop window, when the change rate of the friction coefficient within the time interval of the first stop window is less than a first preset change rate, entering a first supplementary grinding stage; After maintaining the first supplementary grinding time, the first grinding step is stopped.

3. The CMP polishing method according to claim 2, characterized in that: The first termination time is 160s to 300s; The first monitoring duration is 100s to 290s; The first supplementary grinding time is 10s to 60s; The first preset change rate is 0.01 / s to 0.1 / s.

4. The CMP polishing method according to claim 1, characterized in that: The step of stopping the second grinding step when the rate of change of the friction coefficient is less than a second preset rate of change includes: monitoring the friction coefficient curve in real time during a second monitoring period; Setting a second stop window, when the change rate of the friction coefficient within the time interval of the second stop window is less than a second preset change rate, entering the second supplementary grinding stage; After the second supplementary grinding time period is maintained, the second grinding step is stopped.

5. The CMP polishing method according to claim 4, characterized in that: The second termination time is 160s to 300s; The second monitoring duration is 100s to 290s; The second supplementary grinding time is 10s to 60s; The second preset change rate is 0.01-0.1 / s.

6. The CMP polishing method according to claim 1, characterized in that: The first film layer selection ratio is polysilicon film layer to oxide film layer=800:1-850:1; The second film layer selection ratio is oxide film layer to silicon nitride film layer=200:1-220:

1.

7. The CMP polishing method according to claim 6, characterized in that: The first grinding liquid has a particle size of 40 μm to 120 μm, a solid content of 3 wt% to 30 wt%, and a pH of 7 to 10; The particle size of the second grinding liquid is 70 μm to 300 μm, the solid content is 1 wt% to 10 wt%, and the pH value is 8 to 12.

8. The CMP polishing method according to claim 1, characterized in that: In the step of cleaning the wafer, Deionized water is used to remove the second polishing liquid remaining on the surface of the wafer.

9. The CMP polishing method according to claim 1, characterized in that: Before the first grinding step, the method further comprises: The film thickness on the wafer surface is acquired in real time to obtain thickness curves of different film layers.

10. The CMP polishing method according to claim 9, characterized in that: The step of acquiring the film thickness on the wafer surface in real time and obtaining thickness curves of different film layers includes: By scanning the film layer on the wafer surface and performing spectral fitting, a thickness curve graph of different film layers on the wafer surface can be obtained for real-time monitoring.