Method for value-added recycling of thermoplastic polyurethane through multiple cycles

By removing oxime in vacuum and promoting cross-linking reaction, the thermoplastic polyurethane is converted into high-performance thermoset polyurethane, and can be converted into thermoplastic polyurethane again through reverse reaction, solving the problem of limited recycling times of thermoplastic materials in the prior art, and achieving multiple times Recycling value-added recycling and performance improvement.

CN119019643AActive Publication Date: 2024-11-26HANGZHOU NORMAL UNIVERSITY

Patent Information

Application Number
CN202411201777.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-26
Estimated Expiration
2044-08-29

Smart Images

  • Figure CN119019643A_ABST
    Figure CN119019643A_ABST
Patent Text Reader

Abstract

The invention discloses a method for recycling thermoplastic polyurethane in a multi-cycle and value-added manner, which comprises the following steps: placing the thermoplastic polyurethane containing oxime in vacuum, and heating at 80-200 DEG C to react for 1-20 hours to remove oxime to obtain thermosetting polyurethane; and dissolving the removed oxime in a solvent when necessary to obtain an oxime solution, placing the thermosetting polyurethane in the oxime solution, carrying out a reverse reaction at 50-150 DEG C for 10 min to 10 h, and removing the solvent after the reaction is completed to obtain the thermoplastic polyurethane. According to the method, the properties of the polyurethane material are changed by removing and returning the oxime, the residual components can be subjected to cross-linking reaction by removing the oxime component in molecules, so that the thermoplastic material is converted into thermosetting polyurethane which does not contain oxime and has better mechanical properties, and the oxime is returned to the thermosetting polyurethane, so that the thermosetting polyurethane can be returned to the thermoplastic material again; the value-added recovery of the thermoplastic material can be realized, the thermosetting polyurethane with better mechanical property is obtained, and the economic value is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermoplastic material recycling, and more specifically relates to a method for recycling thermoplastic polyurethane capable of multiple cycles and value-added recycling. Background Art

[0002] Plastics are closely related to our lives. It is reported that in 2022, the annual global plastic production has reached 400 million tons (Plastics Europe. Plastics — The Facts 2023. Available online: https: / / plasticseurope.org / knowledge-hub / plastics-the-facts-2023 / .). Among them, thermoplastic materials are the main form, accounting for more than 80% of the total plastic production. Such a large amount of plastics has also brought a heavy burden to the environment, accompanied by the problem of waste disposal.

[0003] The current method of recycling thermoplastic materials is mainly through melt reprocessing. This method achieves the goal of reuse by heating the waste to a molten state and reshaping it with the aid of mechanical force. However, during the reprocessing process, the material will be affected by factors such as high temperature, shear force, oxygen and moisture, resulting in inevitable and difficult to quantify side reactions, including molecular chain breakage, hydrolysis and oxidation, thereby reducing the performance and economic value of the material and causing the product to be downgraded. In addition, degradation has a cumulative effect. After 2-3 times of downgrading and recycling, the performance of the product is severely degraded and difficult to reuse, resulting in a limited number of recycling times.

[0004] People are currently trying to achieve the transformation of thermoplastic materials into thermosetting materials. However, they can often only achieve a short-term property transformation to obtain a temporary material, which cannot permanently maintain the transformed form; or they usually need to graft other cross-linking agents to obtain a stable thermosetting material. Summary of the invention

[0005] The object of the present invention is to provide a method for recycling thermoplastic polyurethane for multiple cycles and value-added use, wherein the thermoplastic polyurethane can be recycled for value-added use into thermosetting polyurethane with higher mechanical properties, and the value-added recycling can be carried out for multiple cycles without obvious performance degradation after multiple cycles.

[0006] The present invention provides the following technical solutions: A method for recycling thermoplastic polyurethane for multiple cycles and value-added use, the method comprising the following steps: Step (1), value-added recovery: mixing a dibasic oxime, a diol and a dibasic isocyanate to generate a thermoplastic polyurethane containing an oxime, and then heating the thermoplastic polyurethane containing an oxime in a vacuum environment to react, and obtaining a thermosetting polyurethane after removing the oxime; You can also perform the following steps as needed: Step (2), reverse conversion: dissolving oxime in a solvent to obtain an oxime solution, placing the thermosetting polyurethane in the oxime solution for reverse reaction, and removing the solvent after the reaction is completed to obtain the thermoplastic polyurethane.

[0007] The recycling object of the present invention is thermoplastic materials, especially thermoplastic polyurethane materials, and the target product of recycling is thermosetting polyurethane with higher performance.

[0008] Preferably, the oxime-containing thermoplastic polyurethane contains a large amount of dioxime-urethane groups and common urethane groups; wherein the dioxime is one or more of dimethylglyoxime, ethylenedioxime, and 1,4-benzoquinonedioxime, the diol is one or more of polytetramethylene glycol, polypropylene glycol, polyethylene glycol, and polycaprolactone diol, and the diisocyanate is one or more of diphenylmethane diisocyanate, toluene-2,4-diisocyanate, and 1,6-hexamethylene diisocyanate. The molar ratio of dioxime to diol is 0.1:1 to 10:1, and the molar amount of diisocyanate is the sum of the molar amounts of dioxime and diol. The reaction temperature is 50-120°C, and the reaction time is 1-10h.

[0009] Preferably, in step (1), the vacuum degree is 10-1000 Pa, the heating temperature is 80-200° C., and the heating time is 1-20 h.

[0010] In the value-added recovery reaction of step (1), after the oxime component in the thermoplastic polyurethane is removed, the remaining components undergo a cross-linking reaction and are converted into a thermosetting polyurethane without oxime; specifically, the principle of the value-added recovery reaction is: under heating and vacuum conditions, the dynamics of the dioxime-urethane group in the thermoplastic polyurethane are activated, and cleavage produces dioxime and isocyanate-terminated polyurethane prepolymer. The generated dioxime is separated from the main material due to its vacuum sublimation, so that the reaction continues to proceed in the direction of cleavage, producing more isocyanate-terminated polyurethane prepolymer. The terminal isocyanate group of the isocyanate-terminated polyurethane prepolymer reacts with the ordinary urethane group in the molecule to generate a trifurcated cross-linking site-alophanate group, thereby completing the conversion to thermosetting polyurethane.

[0011] The removed oxime can be recovered by condensation and used as a raw material for synthesizing new thermoplastic polyurethane after recovery; it can also be used as a reaction reagent to return the thermosetting polyurethane obtained by value-added recovery to thermoplastic polyurethane.

[0012] Preferably, the solvent in step (2) is one of ethyl acetate, butyl acetate, tetrahydrofuran, N,N-dimethylformamide, N-methylpyrrolidone, 1,4-dioxane, and dimethyl sulfoxide, and its mass is 1-5 times that of oxime.

[0013] Preferably, the reaction temperature of the reverse reaction in step (2) is 50-150° C., the reaction time is 10 min-10 h, and the reaction is carried out in a sealed container at normal pressure.

[0014] Preferably, in step (2), the solvent is removed by rotary evaporation at a temperature of 25-150° C. for a time of 30 min-2 h.

[0015] In the reverse conversion reaction of step (2), after the thermosetting polyurethane obtains oxime, it can return to the state of thermoplastic material; specifically, the principle of the reverse conversion reaction is: the thermal reversibility of the allophanate group in the thermosetting polyurethane is activated, and reversible cleavage is performed to produce an isocyanate-terminated polyurethane prepolymer. The isocyanate-terminated polyurethane prepolymer reacts with the dioxime and returns to the thermoplastic polyurethane.

[0016] Compared with the current recycling method, the method provided by the present invention has the following advantages: (1) The method of the present invention regulates the material components of thermoplastic polyurethane and changes the properties of the polyurethane material by removing and returning oxime. Removing the oxime component in the molecule can cause the remaining components to undergo a cross-linking reaction, so that the thermoplastic material is converted into a thermosetting polyurethane that does not contain oxime and has better mechanical properties. Returning the oxime to the thermosetting polyurethane can make it return to the thermoplastic material. The obtained thermoplastic material is a linear, non-cross-linked molecule in the traditional sense and can be kept for use at room temperature. The method of the present invention can realize the value-added recovery of thermoplastic materials, obtain thermosetting polyurethane with better mechanical properties, and improve economic value.

[0017] (2) The method of the present invention can be repeated multiple times for value-added recovery, and the performance of the product obtained after each value-added recovery does not significantly decay. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Schematic diagram of the synthesis reaction of oxime-containing thermoplastic polyurethane; Figure 2 A schematic diagram of a reaction for recycling oxime-containing thermoplastic polyurethane into thermosetting polyurethane for value-added recovery; Figure 3 The schematic diagram of the reaction for reverse conversion of thermosetting polyurethane into oxime-containing thermoplastic polyurethane; Figure 4 A schematic diagram of the comprehensive reaction for multiple cycles of value-added recycling; Figure 5Schematic diagram of value-added recovery of oxime-containing thermoplastic polyurethane into thermosetting polyurethane in the embodiment, wherein (a) is thermoplastic polyurethane, (b) is thermosetting polyurethane; Figure 6 Schematic diagram of the dissolution experiment of the initial oxime-containing thermoplastic polyurethane and the thermosetting polyurethane after value-added recovery in the examples, wherein (a) thermoplastic polyurethane, (b) thermosetting polyurethane; Figure 7 The NMR spectra of dimethylglyoxime separated from the main material and deposited on the top of the bottle during value-added recovery in the embodiment and the pure dimethylglyoxime raw material; Figure 8 Schematic diagram of reverse conversion of thermosetting polyurethane into oxime-containing thermoplastic polyurethane in the embodiment, wherein (a) is thermosetting polyurethane, and (b) is thermoplastic polyurethane; Fig. 9 The stress-strain curve of the thermosetting polyurethane subjected to three cycles of value-added recovery in the example. DETAILED DESCRIPTION

[0019] As mentioned above, the present invention provides a method for recycling thermoplastic polyurethane for multiple cycles and value-added use, the method comprising the following steps: Step (1), placing the thermoplastic polyurethane containing oxime in an environment with a vacuum degree of 10-1000 Pa and heating it to 80-200° C. for reaction for 1-20 hours, and obtaining a thermosetting polyurethane after removing the oxime; Step (2), dissolving oxime in a solvent to obtain an oxime solution, placing the thermosetting polyurethane in the oxime solution for reverse reaction at 50-150° C. for 10 min-10 h, and removing the solvent after the reaction is completed to obtain a thermoplastic polyurethane; the solvent is one of ethyl acetate, butyl acetate, tetrahydrofuran, N,N-dimethylformamide, N-methylpyrrolidone, 1,4-dioxane, and dimethyl sulfoxide; The thermoplastic polyurethane containing oxime is prepared by the following method: The dibasic oxime, diol and dibasic isocyanate are mixed and reacted to generate thermoplastic polyurethane containing oxime, wherein the dibasic oxime is one or more of dimethylglyoxime, ethylenedioxime and 1,4-benzoquinonedioxime, the diol is one or more of polytetramethylene glycol, polypropylene glycol, polyethylene glycol and polycaprolactone diol, and the dibasic isocyanate is one or more of diphenylmethane diisocyanate, toluene-2,4-diisocyanate and 1,6-hexamethylene diisocyanate.

[0020] The technical principle of the method for recycling thermoplastic polyurethane for multiple cycles and value-added use provided by the present invention is as follows: Figure 1-Figure 4As shown, there are respectively a schematic diagram of the synthesis reaction of oxime-containing thermoplastic polyurethane, a schematic diagram of the value-added recycling reaction, a schematic diagram of the reverse conversion reaction, and a schematic diagram of the comprehensive reaction of multiple cycles of value-added recycling; the method provided by the present invention has low raw material prices, simple material preparation and recycling processes, can achieve value-added recycling, obtain thermosetting polyurethane with better mechanical properties, and improve economic value; in addition, value-added recycling can be carried out for multiple cycles without obvious performance degradation.

[0021] The present invention is further described below in conjunction with specific examples. It should be noted that the following examples are only used to deepen the understanding of the present invention, and are not used to limit the scope of the present invention.

[0022] Example 1 In this embodiment, dimethylglyoxime is selected as the dibasic oxime, polytetramethylene glycol is selected as the diol, and diphenylhexane diisocyanate is selected as the dibasic isocyanate to prepare the thermoplastic polyurethane containing oxime.

[0023] Raw materials: dimethylglyoxime, polytetramethylene glycol (M n = 1000 g / mol), purchased from Aladdin Reagent Platform; diphenylhexane diisocyanate, purchased from Wanhua Chemical Group Co., Ltd.; N,N-dimethylformamide, purchased from Sinopharm Chemical Reagent Co., Ltd.

[0024] Synthesis of oxime-containing thermoplastic polyurethane: Dissolve polytetramethylene glycol (40 g, 0.04 mol) and dimethylglyoxime (4.64 g, 0.04 mol) in N,N-dimethylformamide (180 mL). Then add diphenylmethane diisocyanate (20 g, 0.08 mol) and react at 70 °C for 6 h. After the reaction is completed, remove N,N-dimethylformamide by rotary evaporation to obtain oxime-containing thermoplastic polyurethane.

[0025] Value-added recovery of oxime-containing thermoplastic polyurethane to thermosetting polyurethane: Place the oxime-containing thermoplastic polyurethane on a polytetrafluoroethylene plate and place it at the bottom of a vacuum reactor (such as Figure 5 As shown). Under vacuum conditions (150Pa), the bottom of the reactor is heated (140℃) for 5h to obtain thermosetting polyurethane. Figure 5 The red frame in (b) shows the deposited diacetyl oxime.

[0026] The thermoplastic / thermosetting conversion was confirmed by dissolution experiments. The material was placed in N,N-dimethylformamide solvent. Figure 6 As shown, Figure 6 (a) Thermoplastic polyurethane is soluble, Figure 6The thermosetting polyurethane obtained after value-added recovery in (b) was insoluble, proving the formation of a cross-linked structure. In addition, the dimethylglyoxime deposited on the top of the reactor was collected and its recovery rate was calculated to be 98% by weighing method; the nuclear magnetic resonance spectrum confirmed the chemical structure of the recovered dimethylglyoxime and its high purity (such as Figure 7 as shown).

[0027] Reverse conversion of thermosetting polyurethane into oxime-containing thermoplastic polyurethane: dissolve the above collected oxime in N,N-dimethylformamide and add the above obtained thermosetting polyurethane. Figure 8 As shown in (a), the thermosetting polyurethane at this time only swells but cannot dissolve. After reacting at 130°C for 15 minutes, the thermosetting polyurethane is completely dissolved. Figure 8 As shown in (b); after removing N,N-dimethylformamide by rotary evaporation, a new thermoplastic polyurethane is obtained.

[0028] Test Example 1: Multiple cycles of value-added recycling The newly obtained thermoplastic polyurethane in Example 1 is subjected to value-added recovery-reverse conversion-value-added recovery (the method is the same as that in Example 1) again, and thus the thermosetting polyurethane with value-added recovery after three cycles can be obtained. Fig. 9 As shown in the figure, mechanical property tests indicate that: (1) compared with the initial material, the mechanical properties of the material are significantly enhanced after value-added recycling; (2) after multiple cycles of recycling, its mechanical properties do not significantly decay.

[0029] The above embodiments are only for illustration, and are not intended to limit the embodiments. For those skilled in the art, other different forms of changes or modifications may be made based on the above description. Any modifications and changes made to the present invention are still within the scope of protection of the present invention.

Claims

1. A method for recycling thermoplastic polyurethane for multiple cycles and value-added use, characterized in that: The method comprises the following steps: Value-added recovery: dioxime, diol and diisocyanate are mixed and reacted to generate thermoplastic polyurethane containing oxime, and then the thermoplastic polyurethane containing oxime is placed in a vacuum, heated at 80-200℃ for 1-20h to remove the oxime to obtain thermosetting polyurethane. The removed oxime is recovered by condensation.

2. The method according to claim 1, characterized in that The vacuum degree in step (1) is 10-1000 Pa.

3. The method according to claim 1, characterized in that The dioxime is one or more of dimethylglyoxime, glyoxime, and 1,4-benzoquinone dioxime; the diol is one or more of polytetramethylene glycol, polypropylene glycol, polyethylene glycol, and polycaprolactone glycol; and the diisocyanate is one or more of diphenylmethane diisocyanate, toluene-2,4-diisocyanate, and 1,6-hexamethylene diisocyanate.

4. The method according to claim 3, characterized in that The molar ratio of dibasic oxime to diol is 0.1-10:1, and the molar weight of diisocyanate is the sum of the molar weights of dibasic oxime and diol.

5. The method according to claim 1, characterized in that The following steps are also included: Reverse conversion: dissolve the removed oxime in a solvent to obtain an oxime solution, place the thermosetting polyurethane in the oxime solution, and carry out a reverse reaction at a temperature of 50-150°C for 10 minutes to 10 hours. After the reaction is completed, remove the solvent to obtain a thermoplastic polyurethane.

6. The method according to claim 5, characterized in that The solvent is one of ethyl acetate, butyl acetate, tetrahydrofuran, N,N-dimethylformamide, N-methylpyrrolidone, 1,4-dioxane, and dimethyl sulfoxide.

7. The method according to claim 5, characterized in that The mass ratio of the solvent to the oxime is 1-5:

1.

8. The method according to claim 5, characterized in that The reverse reaction is carried out under closed and normal pressure conditions.

9. The method according to claim 5, characterized in that The solvent is removed by rotary evaporation at a temperature of 25-150° C. for 30 min-2 h.

10. The method according to claim 5, characterized in that In the value-added recovery step, the thermoreversibility of the dioxime-urethane groups in the thermoplastic polyurethane is activated under heating and vacuum conditions, and reversible cleavage is performed to produce dioxime and isocyanate-terminated polyurethane prepolymers. The terminal isocyanate groups of the isocyanate-terminated polyurethane prepolymer react with the ordinary urethane groups in the molecule to form trifurcated crosslinking sites - allophanate groups, thereby completing the conversion to thermosetting polyurethane. In the reverse conversion step, the thermal reversibility of the allophanate groups in the thermosetting polyurethane is activated and reversibly cleaved to produce an isocyanate-terminated polyurethane prepolymer, which reacts with the dioxime to return to the thermoplastic polyurethane.

Citation Information

Patent Citations

  • Dynamically-repairable polyurethane based on oxime and preparation method thereof

    CN108314763A

  • Polyurethane hot-melt adhesive containing dynamic oxime-urethane bond and preparation method thereof

    CN109852326A

  • Preparation method of self-repairing thermosetting film based on multi-component Ugi polymerization reaction and dynamic oxime urethane bond exchange

    CN113121781A

  • Recycling method of polyurethane

    CN114672066A

  • Method for recycling polyurethane foam based on acetoxime

    CN117624723A

Cited By

  • Thermosetting resin capable of being degraded and recycled by heating as well as preparation method and application of thermosetting resin

    CN121226706A

  • A heat-degradable thermosetting resin, and a preparation method and application thereof

    CN121226706B