Regeneration treatment method for cavity wall plate
Through the smooth treatment of the corners of the chamber wall panel and the DC treatment in a specific anodized solution, the problem of ablation of the wall panels below 0.8mm during the oxidation process is solved, which improves the regeneration and repair efficiency and reduces the scrap rate.
Patent Information
- Application Number
- CN202411163227.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
In the semiconductor industry, anode chamber wall panels below 0.8mm are prone to overheating and ablation due to edge and corner effects during the oxidation process, resulting in product scrapping, and the existing technology is difficult to effectively solve this problem.
By grinding the corners of the chamber wall, and performing DC processing in a treatment cell containing a specific anodized solution, the voltage is less than or equal to 15V, and the current is 1000A to 1500A, avoiding ablation caused by concentration of current.
It improves the regeneration and repair efficiency of the chamber wall panel, significantly reduces the product scrap rate, and can directly perform anodization without removing the original oxide film.
Smart Images

Figure CN119020839A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material recycling, and in particular to a chamber wall plate recycling method. Background Art
[0002] In the semiconductor industry, the manufacturing and maintenance of solar equipment, as well as the manufacturing and maintenance of display equipment, involve the refurbishment of electronic products. Since there is no need to produce electronic products from scratch, only surface treatment and material regeneration are required. The production efficiency will be much higher and the production cost will be lower.
[0003] However, when it comes to anode Chamber WALL sheets below 0.8 mm, some technical problems arise. Such sheets are difficult to oxidize again because the edge effect during oxidation can easily lead to overheating and ablation of the product, or even cause the product to be scrapped. Summary of the invention
[0004] Based on this, it is necessary to provide a chamber wall panel regeneration method to address at least one of the above-mentioned problems.
[0005] The chamber wall plate regeneration treatment method provided by the present invention comprises the following steps:
[0006] Grind the corners of the chamber wall panels to make them smooth and clean them;
[0007] placing the cleaned chamber wall panel into a treatment tank containing an anodic oxidation solution;
[0008] A direct current is connected to the chamber wall plate, wherein the voltage of the direct current is less than or equal to 15V and the current is 1000A to 1500A, and a regenerated chamber wall plate is obtained after treatment.
[0009] In one embodiment, the step of rounding the corners of the chamber wall includes rounding the right angles of the chamber wall.
[0010] In one of the embodiments, after the step of rounding the edges and corners of the chamber wall panel, the step further includes providing a smooth warping portion of 5 to 15 degrees at the edges and corners of the chamber wall panel.
[0011] In one embodiment, the cleaning process includes: degreasing, washing and drying the chamber wall panels respectively.
[0012] In one embodiment, the degreasing uses a mixed solution containing the following components, measured by mass fraction: 12-18% NaOH, 10-20% NaPO3 and 5-12% NaSiO3.
[0013] In one embodiment, the anodizing solution includes 8-15% tartaric acid, 6-10% oxalic acid, 3-6% sulfosalicylic acid, 3-4% glacial acetic acid, and the balance is water.
[0014] In one embodiment, the anodizing solution includes 10% tartaric acid, 8% oxalic acid, 5% sulfosalicylic acid and 3% glacial acetic acid.
[0015] In one embodiment, the temperature of the anodizing solution is 30-40°C.
[0016] The technical solution provided in the embodiments of the present invention brings the following beneficial technical effects:
[0017] The chamber wall panel regeneration processing method provided by the present invention grinds the edges and corners of the chamber wall panel smoothly, thereby avoiding the concentration of current at the edges and corners during the anodizing process, which causes the thin plates less than 0.8 mm to be burned or even scrapped. There is no need to remove the original oxide film of the chamber wall panel, and anodizing can be directly performed, which not only improves the regeneration and repair efficiency of the chamber wall panel, but also can greatly reduce the scrap rate of the product.
[0018] Additional aspects and advantages of the present application will be given in subsequent parts and will be understood in detail from the subsequent description or learned through specific implementations of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic flow chart of a chamber wall panel regeneration method according to an embodiment of the present invention. DETAILED DESCRIPTION
[0020] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Possible embodiments of the present invention are shown in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein by the drawings. The embodiments described with reference to the drawings are exemplary and are used to make the understanding of the disclosure of the present invention more thorough and comprehensive, and cannot be interpreted as limiting the present invention. In addition, if the detailed description of the known technology is non-essential technology for the features of the present invention shown, these technical details may be omitted.
[0021] It will be understood by those skilled in the relevant art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those skilled in the art in the art to which the present invention belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with those in the prior art, and will not be interpreted with idealized or overly formal meanings unless specifically defined as herein.
[0022] It will be understood by those skilled in the art that, unless otherwise stated, the singular forms "a", "an", "said" and "the" used herein may also include plural forms. It should be further understood that the term "comprising" used in the specification of the present application refers to the presence of the features, integers, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof. It should be understood that the term "and / or" used herein includes all or any unit and all combinations of one or more associated listed items.
[0023] The technical solution of the present invention and how the technical solution solves the above-mentioned technical problems are described in detail below with specific embodiments.
[0024] The chamber wall panel regeneration treatment method provided by the present invention is as follows: Figure 1 As shown, the regeneration method comprises the following steps:
[0025] S100: Grind the corners of the chamber wall to make them smooth and clean them. The chamber wall is thin. For thin plates, the corners are usually right angles or have concentrated tips. When entering the anodizing tank for anodizing, the current is easily concentrated at these positions. Compared with other positions, the current parameters will be significantly different, so it is easy to cause ablation of the material, which may cause serious scrapping. Therefore, the corners are ground in advance to make them smooth or round, and no longer have tips where electrons can be concentrated, thus avoiding ablation of the material.
[0026] S200: placing the cleaned chamber wall panel into a treatment tank containing anodizing solution.
[0027] S300: connecting direct current to the chamber wall plate, wherein the voltage of the direct current is less than or equal to 15V and the current is 1000A-1500A, and obtaining a regenerated chamber wall plate after treatment.
[0028] The chamber wall panel regeneration processing method provided by the present invention grinds the edges and corners of the chamber wall panel smoothly, thereby avoiding the concentration of current at the edges and corners during the anodizing process, which causes the thin plates less than 0.8 mm to be burned or even scrapped. There is no need to remove the original oxide film of the chamber wall panel, and anodizing can be directly performed, which not only improves the regeneration and repair efficiency of the chamber wall panel, but also can greatly reduce the scrap rate of the product.
[0029] Optionally, in the first embodiment of the present application, the step of rounding the corners of the chamber wall includes rounding the right angles of the chamber wall. The specific rounded corner size is determined according to the size of the chamber wall.
[0030] Optionally, in the second embodiment of the present application, after the step of rounding the edges and corners of the chamber wall panel, a smooth warp portion of 5 to 15° is provided at the edges and corners of the chamber wall panel. The corners of the chamber wall panel are provided with a warp degree so that the chamber wall panel is no longer in the common flat shape, and can contact a larger range of solutions than a flat surface when immersed in the anodizing solution. Experiments have shown that compared with flat chamber wall panels, under the same anodizing parameters, the chamber wall panels with smooth warps have a higher anodizing efficiency, which can be increased by 10 to 15%.
[0031] Optionally, in a third embodiment of the present application, the cleaning treatment includes: degreasing, washing and drying the chamber wall panels. Specifically, in one implementation, the degreasing uses a mixed solution containing the following components by mass fraction: 12-18% NaOH, 10-20% NaPO3 and 5-12% NaSiO3. The chamber wall panels are cleaned by the above process to prepare for subsequent anodizing.
[0032] Specifically, in the fourth embodiment of the present application, the anodizing solution includes 8-15% tartaric acid, 6-10% oxalic acid, 3-6% sulfosalicylic acid, 3-4% glacial acetic acid, and the balance is water. According to experiments, the use of such anodizing solution and the corresponding process-treated products can extend the service life by 30-50%. Preferably, in one of the specific implementations, the anodizing solution includes 10% tartaric acid, 8% oxalic acid, 5% sulfosalicylic acid and 3% glacial acetic acid. The use of such anodizing solution and the corresponding process-treated products can extend the service life by 50%.
[0033] In addition, the present application also conducted tests on the temperature of the anodizing solution. Combined with the technical solutions in the aforementioned implementations, the efficiency of anodizing is better at 30 to 40°C.
[0034] The following are specific embodiments:
[0035] Embodiment 1:
[0036] The chamber wall panels with a thickness of 0.4 mm are polished at the edges and corners, and then degreased after the edges and corners are polished and rounded. The degreasing solution uses an aqueous solution containing 16% NaOH, 15% NaPO3 and 7% NaSiO3. Then it is washed in clean water and dried after completion. Then it is placed in the anodizing tank and the chamber wall panels are energized. The anodizing solution includes 10% tartaric acid, 8% oxalic acid, 5% sulfosalicylic acid and 3% glacial acetic acid. The DC voltage is 15V and the current is 1500A. After treatment, the regenerated chamber wall panels are obtained.
[0037] It will be appreciated by those skilled in the art that the various operations, methods, steps, measures, and schemes in the processes discussed in this application may be alternated, altered, combined, or deleted. Furthermore, other steps, measures, and schemes in the various operations, methods, and processes discussed in this application may also be alternated, altered, rearranged, decomposed, combined, or deleted. Furthermore, the steps, measures, and schemes in the prior art that are similar to those disclosed in this application may also be alternated, altered, rearranged, decomposed, combined, or deleted.
[0038] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, "plurality" means two or more.
[0039] In the description of this specification, specific features, structures, materials or characteristics may be combined in an appropriate manner in any one or more embodiments or examples.
[0040] It should be understood that, although the steps in the flowchart of the accompanying drawings are displayed in sequence as indicated by the arrows, these steps are not necessarily executed in sequence in the order indicated by the arrows. Unless otherwise specified herein, there is no strict order restriction on the execution of these steps, and they can be executed in other orders. Moreover, at least a part of the steps in the flowchart of the accompanying drawings may include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but can be executed at different times, and their execution order is not necessarily sequential, but can be executed in turn or alternately with other steps or at least a part of the sub-steps or stages of other steps.
[0041] The above description is only a partial implementation method of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.
Claims
1. A chamber wall panel regeneration method, characterized in that: The steps include: Grind the edges and corners of the chamber wall panels to make them smooth and clean them; placing the cleaned chamber wall panel into a treatment tank containing an anodic oxidation solution; A direct current is connected to the chamber wall plate, wherein the voltage of the direct current is less than or equal to 15V and the current is 1000A-1500A, and a regenerated chamber wall plate is obtained after treatment.
2. The chamber wall panel regeneration method according to claim 1, characterized in that: The step of rounding the corners of the chamber wall includes rounding the right angles of the chamber wall.
3. The chamber wall panel regeneration method according to claim 1, characterized in that: After the step of rounding the edges and corners of the chamber wall panel, the method further includes providing a smooth warping portion of 5 to 15 degrees at the edges and corners of the chamber wall panel.
4. The chamber wall panel regeneration method according to claim 1, characterized in that: The cleaning process comprises: degreasing, washing and drying the chamber wall panels respectively.
5. The chamber wall panel regeneration method according to claim 4, characterized in that: The degreasing uses a mixed solution containing the following components by mass fraction: 12-18% NaOH, 10-20% NaPO3 and 5-12% NaSiO3.
6. The chamber wall panel regeneration method according to claim 1, characterized in that: The anodizing solution comprises 8-15% tartaric acid, 6-10% oxalic acid, 3-6% sulfosalicylic acid, 3-4% glacial acetic acid, and the balance is water.
7. The chamber wall panel regeneration method according to claim 6, characterized in that: The anodizing solution includes 10% tartaric acid, 8% oxalic acid, 5% sulfosalicylic acid and 3% glacial acetic acid.
8. The chamber wall panel regeneration method according to claim 1, characterized in that: The temperature of the anodizing solution is 30-40°C.