Compound, curable resin composition and cured product thereof, and method for producing compound
Patent Information
- Application Number
- CN202380031324.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-10
Smart Images

Figure CN119032113A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a compound, a curable resin composition, a cured product thereof and a method for producing the compound, which are suitable for use in semiconductor sealing materials, printed wiring boards, electrical and electronic components such as build-up laminates, lightweight and high-strength materials such as carbon fiber reinforced plastics and glass fiber reinforced plastics, and 3D printing applications. Background Art
[0002] In recent years, as the application fields of laminated boards for mounting electrical and electronic components have expanded, the required characteristics have become more extensive and advanced. In the past, semiconductor chips were mainly mounted on metal lead frames, but semiconductor chips with high processing power such as central processing units (hereinafter referred to as CPUs) are increasingly mounted on laminated boards made of polymer materials.
[0003] In particular, semiconductor packages (hereinafter referred to as PKG) used in smart phones, etc., require the thickness of the PKG substrate to be thinner in order to meet the requirements of miniaturization, thinness, and high density. However, the thinner the PKG substrate, the lower the rigidity. Therefore, when the PKG solder is mounted on the motherboard (printed circuit board: PCB), it will cause large warping due to heat. In order to reduce this situation, a PKG substrate material with a high Tg above the solder mounting temperature is required.
[0004] In addition, in the fifth generation communication system "5G" which is now accelerating its development, it is expected that large capacity and high-speed communication will be further enhanced. There is an increasing demand for low dielectric loss tangent materials, and various studies are underway. Patent document 1 records a thermosetting resin composition having (A) an imine compound having a maleic imide group and (B) a phenol aralkyl resin having an aliphatic unsaturated bond in one molecule as essential components. Patent document 2 records an allyl ether modified biphenyl aralkyl phenolic varnish resin. Patent document 3 records a compound having a styrene structure.
[0005] [Prior art literature]
[0006] [Patent Document]
[0007] [Patent Document 1] Japanese Patent Application Laid-Open No. 04-359911
[0008] [Patent Document 2] International Publication No. 2016 / 002704
[0009] [Patent document 3] Japanese Patent No. 6951829. Summary of the invention
[0010] [Problems to be solved by the invention]
[0011] When the applicant of the present application retested patent document 3, it was found that when the method described in patent document 3 was used for synthesis, when the synthesized compound was dissolved in a solvent such as toluene and stored, there was a problem of crystallization. In order to solve this problem of crystallization, the use of a compound precursor with a high molecular weight 2-bromoethylbenzene structure was also explored, but in this case, the problem that the styrene reaction on the polymer side could not be fully carried out was generated. In addition, making the reaction conditions more stringent to promote the reaction was also explored, but although the reaction rate (conversion rate) increased, the increase in the amount of impurities reduced the electrical properties and the progress of the unexpected free radical polymerization reaction, resulting in other problems such as high molecular weight and gelation. In other words, it is extremely difficult to achieve solvent stability and suppression of impurity generation (low dielectric properties) at the same time.
[0012] In view of the above circumstances, an object of the present invention is to provide a compound having excellent solvent stability and low dielectric properties, a curable resin composition and a cured product thereof, and a method for producing the compound.
[0013] [Methods for solving the problem]
[0014] That is, the present invention relates to the following [1] to
[13] . [1]
[0016] A compound represented by the following formula (1), wherein the compound wherein n in the formula (1) is 1 accounts for less than 50% of the total amount of the aforementioned compounds in terms of GPC area percentage.
[0017]
[0018] In formula (1), the multiple Rs each independently represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms. p and r are integers from 0 to 4, q is an integer from 0 to 3, n is a repetition number, and the average value of n is n ave Conform to 1≤n ave ≤20. ) [2]
[0020] The compound as described in the above item [1], wherein the value (α / β) obtained by dividing the sum of the HP-LC peak areas (α) of the compounds represented by the following formulae (2) to (4) by the HP-LC peak area (β) of the compound wherein n is 1 in the above formula (1) is 0.10 or less.
[0021]
[0022] (In formula (2), a plurality of Rs each independently represent a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group. A plurality of s each independently represent an integer of 0 to 4.)
[0023]
[0024] (In formula (3), the multiple Rs each independently represent a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group. The multiple As each independently represent any one of the following formulae (3-a) to (3-c). The multiple s each independently represent an integer from 0 to 4, and t is an integer from 0 to 3.)
[0025]
[0026] (In formulae (3-a) to (3-c), * represents a position bonded to the aromatic ring of the compound of formula (3).)
[0027]
[0028] (In formula (4), a plurality of Rs each independently represent a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group. A plurality of Bs each independently represent the following formula (4-d) or (4-e). D is the following formula (4-f). A plurality of s each independently represent an integer from 0 to 4, and t is an integer from 0 to 3. One of the five ms in formula (4) is 1, and the remaining four are 0.)
[0029]
[0030] (In formulae (4-d) to (4-f), * represents a position bonded to the aromatic ring of the compound of formula (4).) [3]
[0032] The compound as described in the above item [1] or [2], wherein in the above formula (1), p=0, q=0, and r=0. [4]
[0034] The compound as described in any one of the above items [1] to [3], wherein the compound represented by the above formula (1) is derived from a compound represented by the following formula (5).
[0035]
[0036] (In formula (5), a plurality of Rs exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms. p and r are integers from 0 to 4, q is an integer from 0 to 3, n is a repetition number, and the average value of n is n ave Conform to 1≤n ave ≤20. X represents a halogen atom. ) [5]
[0038] The mixture as described in any one of the above items [1] to [4], further comprising a polymerization inhibitor. [6]
[0040] A curable resin composition comprising the compound described in any one of the above items [1] to [4], or the mixture described in the above item [5]. [7]
[0042] The curable resin composition as described in the above item [6] contains at least one of a polyphenylene ether compound, polybutadiene and a modified product thereof, and polystyrene and a modified product thereof. [8]
[0044] The curable resin composition as described in the above item [6] or [7] contains a radical polymerization initiator. [9]
[0046] A cured product obtained by curing the compound described in any one of the above items [1] to [4], the mixture described in the above item [5], or the curable resin composition described in any one of the above items [6] to [8].
[10]
[0048] A method for producing a compound represented by the following formula (1), comprising subjecting a compound represented by the following formula (5) to a dehydrohalogenation reaction in the presence of a basic catalyst in a solvent in an amount of 4 to 7 times the weight of the compound represented by the following formula (5).
[0049]
[0050] (In formula (1), a plurality of Rs exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms. p and r are integers from 0 to 4, q is an integer from 0 to 3, n is a repetition number, and the average value of n is n ave Conform to 1≤n ave ≤20. )
[0051]
[0052] (In formula (5), a plurality of Rs exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms. p and r are integers from 0 to 4, q is an integer from 0 to 3, n is a repetition number, and the average value of n is n ave Conform to 1≤n ave ≤20. X represents a halogen atom. )
[11]
[0054] The method for producing a compound according to the above item
[10] , wherein the solvent is a mixed solvent of an aprotic polar solvent and a water-insoluble solvent.
[12]
[0056] The method for producing a compound according to the above item
[11] , wherein the amount of the aprotic polar solvent used is 1 to 10 times the weight of the water-insoluble solvent.
[13]
[0058] The method for producing a compound according to the above item
[11] or
[12] , wherein dimethyl sulfoxide is used as the aprotic polar solvent and toluene is used as the water-insoluble solvent.
[0059] [Effects of the invention]
[0060] The compound of the present invention has excellent solvent solubility, and its cured product has excellent low dielectric properties. Therefore, it is a useful material for sealing of electric and electronic components, circuit substrates, carbon fiber composites, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 The GPC chart of Synthesis Example 1 is shown.
[0062] Figure 2 The GPC chart of Example 1 is shown.
[0063] Figure 3 Example 1 1 H-NMR chart.
[0064] Figure 4 The LC-MS chart of Example 1 is shown.
[0065] Figure 5 The HP-LC chart of Example 1 is shown.
[0066] Figure 6 The GPC chart of Example 2 is shown.
[0067] Figure 7 The HP-LC chart of Example 2 is shown.
[0068] Figure 8 The GPC chart of Example 3 is shown.
[0069] Fig. 9 The HP-LC chart of Example 3 is shown.
[0070] Fig.10 The GPC chart of Example 4 is shown.
[0071] Fig.11 The HP-LC chart of Example 4 is shown.
[0072] Fig.12 The GPC chart of Comparative Synthesis Example 1 is shown.
[0073] Fig.13 The GPC chart of Comparative Synthesis Example 2 is shown.
[0074] Fig.14The HP-LC chart of Comparative Synthesis Example 2 is shown. DETAILED DESCRIPTION
[0075] The compound of the present embodiment is a compound represented by the following formula (1), wherein the ratio (area percentage) of the area (time-integrated value of the signal value) of the compound in which n in the formula (1) is 1 to the total area (time-integrated value of the signal value) of the compound having the structure represented by the formula (1) in the chromatogram obtained by gel permeation chromatography (hereinafter, also referred to as GPC) is less than 50%. When the area percentage of the compound having the structure in which n in the formula (1) is 1 is 50% or more, there is a concern that crystals may precipitate (that is, solvent solubility decreases) when a resin solution containing the compound represented by the above formula (1) is stored.
[0076]
[0077] In formula (1), the multiple Rs each independently represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms. p and r are integers from 0 to 4, and q is an integer from 0 to 3. n is the number of repetitions, and the average value of n is n ave Conform to 1≤n ave ≤20. )
[0078] In the above formula (1), p and r are usually 0 to 4, preferably 0 to 2, and more preferably 0. q is usually 0 to 3, preferably 0 to 2, and more preferably 0. n ave Usually 1≤n≤20, preferably 1.1≤n ave ≤20, more preferably 1.1≤n ave ≤10, particularly preferably 1.1≤n ave ≤5. Average value of n ave It can be calculated from the value of the number average molecular weight (Mn) determined by GPC measurement of the compound represented by formula (1). The number average molecular weight is preferably 200 or more and less than 5000, more preferably 300 or more and less than 3000, and particularly preferably 400 or more and less than 2000. When the number average molecular weight is less than 5000, purification by water washing becomes easy, and when it is 200 or more, the possibility of the target compound volatilizing in the solvent distillation step is small.
[0079] In the above formula (1), R is a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group, preferably a hydrocarbon group having 1 to 10 carbon atoms, more preferably a hydrocarbon group having 1 to 5 carbon atoms, and particularly preferably a hydrocarbon group having 1 to 3 carbon atoms. When R has a small carbon number, it is difficult to generate molecular vibration when exposed to high frequencies, so in the case of the hydrocarbon group having 1 to 3 carbon atoms described above, the electrical properties are particularly excellent.
[0080] In addition, the GPC measurement in the present embodiment is performed under the following conditions.
[0081] <GPC>
[0082] GPC: Online degasser (DGU-20A3R), binary liquid transfer device (LC-20AD), autosampler (SIL-20AHT), differential refractive index detector (RID-20A), column oven (CTO-20A), system controller (CBM-20A) (all made by Shimadzu Corporation)
[0083] Column: Shodex KF-603×1, KF-602.5×1, KF-602×1, KF-601×1 (all made by Showa Denko Co., Ltd.)
[0084] Protection column: Shodex KF-G 4A (manufactured by Showa Denko Co., Ltd.)
[0085] Combined eluent: tetrahydrofuran
[0086] Flow rate: 1.5ml / min.
[0087] Column temperature: 40℃
[0088] Detection: RI (differential refractive index detector)
[0089] The compound represented by the above formula (1) sometimes contains compounds represented by the following formulas (2) to (4) as by-products. The value (α / β) obtained by dividing the sum of the peak areas (α) of the compounds represented by the following formulas (2) to (4) in the chromatogram obtained by high performance liquid chromatography (HP-LC) by the peak area (β) of the HP-LC compound of the above formula (1) where n is 1 is preferably 0.10 or less, more preferably 0.07 or less. Here, "peak area" means the area enclosed by the straight line connecting the two tails of the peak and the peak. In practice, it is obtained by an approximate value of the half-value width method or by the number of counts obtained by integrating the peak time value output (JIS K0214: 2013). Since the compounds represented by the following formulas (2) to (4) have polar groups in their structures, increasing the content of these groups deteriorates the dielectric properties. The lower limit of the value of (α / β) may be 0, but is preferably 0.01. This is because when the molecular weight is 0.01 or more, the adhesiveness, solvent solubility, and compatibility with a compound having a polar group are improved.
[0090]
[0091] (In formula (2), a plurality of Rs exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms. s is an integer from 0 to 4.)
[0092]
[0093] (In formula (3), the multiple Rs each independently represent a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group. The multiple As each independently represent any one of the following formulae (3-a) to (3-c). s is an integer from 0 to 4, and t is an integer from 0 to 3.)
[0094]
[0095] (In formulae (3-a) to (3-c), * represents a position bonded to the aromatic ring of the compound of formula (3).)
[0096]
[0097] (In formula (4), a plurality of Rs each independently represent a hydrocarbon group having 1 to 10 carbon atoms or a halogenated alkyl group. A plurality of Bs each independently represent the following formula (4-d) or (4-e). D is the following formula (4-f). A plurality of s each independently represent an integer from 0 to 4, and t is an integer from 0 to 3. One of the five ms in formula (4) is 1, and the remaining four are 0.)
[0098]
[0099] (In formulae (4-d) to (4-f), * represents a position bonded to the aromatic ring of the compound of formula (4).)
[0100] It is generally believed that the by-products of the compounds shown in the above formulas (2) to (4) can be removed by purification, but in the case of the compounds shown in the above formula (1), it is difficult to remove the compounds shown in the above formulas (2) to (4) by purification methods such as distillation, recrystallization, and water washing. Specifically, the compound shown in the above formula (1) has a styrene structure as a functional group, so it is highly reactive and undesirable polymerization is carried out in purification methods such as distillation that require overheating. In addition, it is known that the compound shown in the above formula (1) is a liquid compound after the solvent is distilled off, and it is difficult to form a crystalline structure, so it is difficult to recrystallize it with a high yield. Moreover, water washing has also been performed in Patent Document 3, but the effect is small.
[0101] Accordingly, in this embodiment, the reaction temperature, the amount of solvent, and the mixing ratio of the solvent in the synthesis step of the compound represented by the above formula (1) are adjusted to control the production amount of the compounds represented by the above formulas (2) to (4). The details of the synthesis method of the compound represented by the above formula (1) are described below.
[0102] In this embodiment, the structure analysis is performed by liquid chromatography-mass spectrometry (hereinafter also referred to as LC-MS), and the content of the compounds represented by the above formulae (2) to (4) is analyzed by high performance liquid chromatography (hereinafter also referred to as HP-LC).
[0103] <LC-MS>
[0104] Apparatus: Ultra-high performance liquid chromatography (UHPLC) system (Ultimate 3000), mass spectrometer (Q-Exactive (registered trademark)) (both manufactured by Thermo Fisher Scientific Inc.)
[0105] Column: ODS-2 (manufactured by GL Sciences)
[0106] Combined eluent: tetrahydrofuran: water = 3:1 (no gradient)
[0107] Flow rate: 0.5ml / min.
[0108] Ionization mode: ESI
[0109] Mass range: m / z = 150-2000
[0110] <HP-LC>
[0111] Devices: Binary liquid transfer device (LC-20AB), online degasser (DGU-20A3R), autosampler (SIL-20A), column oven (CTO-20A), system controller (CBM-20A), photodiode array detector (SPD-M20A) (all manufactured by Shimadzu Corporation)
[0112] Column: ODS-2 (manufactured by GL Sciences)
[0113] Combined eluent: tetrahydrofuran: water = 3:1 (no gradient)
[0114] Flow rate: 0.5ml / min.
[0115] Column temperature: 40℃
[0116] Detection: PDA (Photodiode Array Detector)
[0117] Detector: 274nm
[0118] The hydroxyl equivalent of the compound represented by the formula (1) is preferably 100,000 g / eq. or less. When the hydroxyl equivalent is 100,000 g / eq. or less, electrical properties and low heat resistance are not impaired, and adhesion, solvent solubility, and compatibility with compounds having a polar group are improved.
[0119] The compound represented by the above formula (1) is derived from the compound represented by the following formula (5).
[0120]
[0121] (In formula (5), a plurality of Rs exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms. p and r are integers from 0 to 4, q is an integer from 0 to 3, n is a repetition number, and the average value of n is n ave Conform to 1≤n ave ≤20. X represents a halogen atom. )
[0122] The definition of R, p, r, q, and the average value of n in the above formula (5) are ave The preferred range of is the same as that of the above formula (1). From the viewpoint of reactivity and raw material stability, R represents a halogen atom in R when an alkyl group is halogenated, and X is preferably a bromine atom or a chlorine atom, and particularly preferably a bromine atom.
[0123] The compound represented by the above formula (1) can be obtained, for example, by subjecting the compound represented by the above formula (5) to a dehydrohalogenation reaction in a solvent in the presence of a basic catalyst. The amount of solvent used is preferably 4 to 7 times the weight of the compound represented by the formula (5).
[0124] The solvent used is preferably an aprotic polar solvent, and examples thereof include dimethyl sulfone, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, 1,3-dimethyl-2-imidazolidinone, and N-methylpyrrolidone. Two or more of these solvents may be used in combination.
[0125] In addition, it is also preferred to use an aprotic polar solvent and a non-water-soluble solvent to form a mixed solvent. At this time, as aprotic polar solvent, dimethyl sulfoxide, dimethylformamide, 1,3-dimethyl-2-imidazolidinone, N-methylpyrrolidone are preferred. As a non-water-soluble solvent, benzene, toluene, xylene, trimethylbenzene, hexane, cyclohexane, methylcyclohexane are preferred. Among these, the most preferred combination is a combination of dimethyl sulfoxide and toluene.
[0126] In the aforementioned mixed solvent, the aforementioned aprotic polar solvent is preferably used in an amount of 1 to 10 times by weight of the aforementioned water-insoluble solvent, more preferably 1 to 8 times, and particularly preferably 2 to 6 times. When it is less than 1 time, there is a concern that the reaction is difficult to proceed and the raw material remains. When it exceeds 10 times, the reaction promoting effect is high, but the production amount of the compound represented by the aforementioned formula (2) to (4) is easy to increase. In the second half of the reaction, the reaction is carried out in a state where the aprotic polar solvent layer and the water-insoluble solvent layer are separated in two layers. Therefore, from the viewpoint of controlling the reactivity of the interface, the above range is preferably used.
[0127] The total amount of the solvent used is preferably 1 to 9 times by weight, more preferably 2 to 8 times by weight, and particularly preferably 3 to 7 times by weight relative to the compound represented by the above formula (5). If the amount is less than 1 time by weight, there is a concern that stirring becomes difficult due to salt precipitation, and if the amount is more than 9 times by weight, there is a concern that the kettle efficiency (the amount of resin that can be synthesized in one batch) is significantly reduced.
[0128] The reaction temperature is preferably 0 to 80° C., more preferably 10 to 60° C., and even more preferably 26 to 70° C. If the temperature is lower than 0° C., the reaction may not proceed sufficiently, while if the temperature is higher than 80° C., the polymerization reaction of the styrene structure may occur, resulting in gelation.
[0129] The catalyst is not particularly limited, but alkaline catalysts such as sodium hydroxide, potassium hydroxide, potassium carbonate, etc. can be listed. Since the dehydrohalogenation reaction is difficult to proceed completely, a large excess of aprotic polar solvent relative to the substrate can be used, and the dehydrohalogenation reaction can be carried out 2 or 3 times or more. For example, the solution obtained by subjecting the compound represented by the above formula (2) to a dehydrohalogenation reaction in the presence of an alkaline catalyst in an organic solvent can be washed with water, returned to the reaction vessel again, and an alkaline catalyst is added to react it again. The degree of progress of the dehydrohalogenation reaction can be improved accordingly. That is, the mass concentration of residual halogen contained in the target compound can be reduced. As the mass concentration of residual halogen, it is preferably 1 to 10000 ppm in the target, more preferably 1 to 1000 ppm, and even more preferably 1 to 750 ppm. If the mass concentration of residual halogen contained in the compound represented by the above formula (1) is high, it will cause molecular vibration when exposed to high-frequency waves, and there is a concern that the electrical properties such as the dielectric loss tangent will be adversely affected. Furthermore, when the mass concentration of the residual halogen is high, there is a concern that the risk of causing problems such as metal corrosion and ion migration in environmental tests such as the HAST test (High Accelerated Stress Test) increases, so the above-mentioned halogen content is preferably used.
[0130] The method for preparing the compound represented by the above formula (5) is not particularly limited, but for example, a compound having a (2-bromoethyl)benzene structure can be reacted with a dihalogenated methyl aryl compound (or a bishydroxymethyl aryl compound, etc.) under an acid catalyst such as hydrochloric acid, sulfonic acid, activated clay, etc., or a compound having a (2-bromoethyl)benzene structure can be reacted with a bishydroxymethyl aryl compound under an acid catalyst such as hydrochloric acid, sulfonic acid, activated clay, etc. In the case of using sulfonic acid or the like as a catalyst, the extraction step can be performed after neutralization with an alkali metal such as sodium hydroxide or potassium hydroxide. For the extraction step, an aromatic hydrocarbon solvent such as toluene or xylene can be used alone, or a non-aromatic hydrocarbon such as cyclohexane or toluene can be used in combination. After extraction, the organic layer is washed with water until the waste water becomes neutral, and the solvent and excess compounds having a (2-bromoethyl)benzene structure are distilled off using an evaporator or the like, thereby obtaining a compound having at least two or more 2-bromoethylethylbenzene structures in the target molecule.
[0131] The charge ratio of the compound having a (2-bromoethyl)benzene structure is preferably 1.0 to 4.0 times, more preferably 1.0 to 3.0, and even more preferably 1.0 to 2.0, relative to 1 mol of the dihalogenated methyl aryl compound (or bishydroxymethyl aryl compound, etc.). When the charge ratio is 4.0 times or less, significant precipitation of crystals can be avoided when the resin solution containing the compound represented by the above formula (1) is refrigerated or frozen. In addition, when the charge ratio is 1.0 times or more, significant generation of high molecular weight products can be avoided, and purification by water washing can be achieved.
[0132] Among the compounds represented by the above formula (5), slice data of the chromatogram is obtained using an RI (differential refractive index) detector of GPC analysis, and the content of the compound represented by formula (5) where n is 1 can be determined by the ratio (area percentage) of the area of the slice data corresponding to the compound represented by formula (5) where n is 1 to the total area (time-integrated value of the signal value) of the slice data corresponding to the compound represented by formula (5). The content (area percentage) of the compound represented by formula (5) where n is 1 is preferably 25 to 75%, more preferably 30 to 60%, and even more preferably 35 to 50%. If the content is more than 75%, there is a concern that crystals will precipitate significantly when the resin solution containing the compound represented by formula (1) is refrigerated or frozen. If the content is less than 25%, there is a concern that the reactivity of the high molecular weight product will decrease. This is because when the compound represented by formula (1) derived from the compound represented by formula (5) is synthesized under the above preferred conditions, the higher the high molecular weight product, the more difficult the reaction is to proceed.
[0133] As compounds having a (2-bromoethyl)benzene structure, for example: (2-bromoethyl)benzene, 1-(2-bromoethyl)-2-methylbenzene, 1-(2-bromoethyl)-3-methylbenzene, 1-(2-bromoethyl)-4-methylbenzene, 1-(2-bromoethyl)-2,3-dimethylbenzene, 1-(2-bromoethyl)-2,4-dimethylbenzene, 1-(2-bromoethyl)-2,5-dimethylbenzene, 1-(2-bromoethyl)-2,6-dimethylbenzene, etc., but are not limited to these. These can be used alone or in combination of two or more. The more carbons there are, the better the solvent solubility is, but since the heat resistance is reduced, it is preferably unsubstituted or substituted by an alkyl group having 1 to 3 carbons, more preferably unsubstituted or substituted by an alkyl group having 1 to 2 carbons, and most preferably unsubstituted or substituted by a methyl group.
[0134] As the dihalogenated methyl aryl compound, for example, difluoro-o-xylene, difluoro-m-xylene, difluoro-p-xylene, dichloro-o-xylene, dichloro-m-xylene, dichloro-p-xylene, dibromo-o-xylene, dibromo-m-xylene, dibromo-p-xylene, diiodo-o-xylene, diiodo-m-xylene, diiodo-p-xylene, etc. can be cited, but it is not limited to these. These can be used alone, or two or more can be used in combination. From the viewpoint of the reactivity of the raw materials during synthesis, preferably chlorine compounds, bromine compounds, iodine compounds, more preferably chlorine compounds, bromine compounds.
[0135] Examples of the bishydroxymethyl aryl compound include, but are not limited to, o-phthalic acid alcohol, isophthalic acid alcohol, and p-phthalic acid alcohol. These may be used alone or in combination of two or more. The amount of these used is preferably 0.05 to 0.8 parts by mass, more preferably 0.1 to 0.6 parts by mass, relative to 1 part by mass of the compound having a (2-bromoethyl)benzene structure.
[0136] When the compound having a (2-bromoethyl) benzene structure reacts with a halogenated methyl aryl compound, in addition to hydrochloric acid, phosphoric acid, sulfuric acid, formic acid, p-toluenesulfonic acid, and methanesulfonic acid as catalysts, Lewis acids such as aluminum chloride and zinc chloride, activated clay, acid clay, white carbon, zeolite, solid acids such as aluminum silicate, and acidic ion exchange resins can be used as needed. These can be used alone or in combination of two or more. The amount of the catalyst used is 0.05 to 0.8 moles, preferably 0.1 to 0.7 moles, relative to 1 mole of the compound having a (2-bromoethyl) benzene structure used. If the amount of the catalyst used is too much, the viscosity of the reaction solution is too high and there is a worry that stirring is difficult, and if it is too little, there is a worry that the reaction will slow down. Organic solvents such as hexane, cyclohexane, octane, toluene, and xylene can be selected for reaction as needed, or the reaction can be carried out without a solvent. For example, after adding an acidic catalyst to a mixed solution of a compound having a (2-bromoethyl)benzene structure, a methyl halogenated aromatic compound, and a solvent, if the catalyst contains water, water is removed from the system by azeotropy. Thereafter, the reaction is carried out at 40 to 180°C, preferably 50 to 170°C for 0.5 to 40 hours. After the reaction is completed, the acidic catalyst can be neutralized with an alkaline aqueous solution, but the water washing step can also be carried out directly without neutralization. For the water washing step, a water-insoluble organic solvent is added to the oil layer, and the water washing is repeated until the wastewater becomes neutral.
[0137] The softening point of the compound represented by the above formula (5) is preferably 80°C or less, more preferably 70°C or less. When the softening point is 80°C or less, the viscosity of the compound represented by the above formula (5) when it is derived into the compound represented by the above formula (1) becomes low. Accordingly, it is easy to ensure fluidity, the impregnation property of fibrous materials such as glass cloth and carbon fiber is not impaired, and it is easy to make the curable resin composition into a semi-cured state (B stage) such as prepreg. When the dilution solvent is increased to reduce the viscosity, the curable resin composition in the impregnation step may not be sufficiently attached to the fibrous material.
[0138] [Polymerization inhibitor]
[0139] The compound and curable resin composition of this embodiment may contain a polymerization inhibitor. By containing a polymerization inhibitor, the storage stability can be improved and the reaction start temperature can be controlled. By controlling the reaction start temperature, it is easy to ensure fluidity, not to damage the impregnation of glass cloth, etc., and it is easy to become a B-stage such as prepreg. If the polymerization reaction is excessive during prepreg, it is easy to cause problems such as lamination becoming difficult in the lamination step.
[0140] The polymerization inhibitor may be added during or after the synthesis of the compound represented by the formula (1). The amount of the polymerization inhibitor used is 0.008 to 1 part by weight, preferably 0.01 to 0.5 part by weight, based on 100 parts by weight of the compound represented by the formula (1).
[0141] Examples of the polymerization inhibitor include phenolic, sulfuric, phosphorus, hindered amine, nitroso, and nitroxyl free radicals. In addition, one type of polymerization inhibitor may be used, or multiple types may be used in combination. Among these, in the present embodiment, phenolic, hindered amine, nitroso, and nitroxyl free radicals are preferred.
[0142] Examples of the phenolic polymerization inhibitor include monophenols such as 2,6-di-tert-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-tert-butyl-p-ethylphenol, stearyl-β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, isooctyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 2,4-bis-(n-octylthio)-6-(4-hydroxy-3,5-di-tert-butylaniline)-1,3,5-triazine, 2,4-bis[(octylthio)methyl]-o-cresol, and 2,2′-methylenebis(4-methyl-6- tert-butylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-butylenebis(3-methyl-6-tert-butylphenol), triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamic acid), 2,2-thio-bis(diethylenebis(3-tert-butyl-4-hydroxy-hydrocinnamic acid), Bisphenols such as [3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], 3,5-di-tert-butyl-4-hydroxybenzylphosphonic acid-diethyl ester, 3,9-bis[1,1-dimethyl-2-{β-(3-tert-butyl-4-hydroxy-5-methylphenyl) propionyloxy}ethyl]2,4,8,10-tetraoxaspiro[5,5]undecane, bis(3,5-di-tert-butyl-4-hydroxybenzylsulfonic acid ethyl) calcium, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6 -Tris-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tetrakis-[methylene-3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane, bis[3,3'-bis-(4'-hydroxy-3'-tert-butylphenyl)butyric acid]ethylene glycol ester, tris-(3,5-di-tert-butyl-4-hydroxybenzyl)-isocyanurate, 1,3,5-tris-(3',5'-di-tert-butyl-4'-hydroxybenzyl)-S-triazine-2,4,6-(1H,3H,5H)trione, high molecular weight phenols such as tocopherol, etc., but are not limited to these.
[0143] Examples of the sulfur-based polymerization inhibitor include, but are not limited to, dilauryl-3,3′-thiodipropionate, dimyristyl-3,3′-thiodipropionate, and distearyl-3,3′-thiodipropionate.
[0144] Examples of the phosphorus-based polymerization inhibitor include triphenyl phosphite, diphenyl isodecyl phosphite, phenyl diisodecyl phosphite, tris(nonylphenyl) phosphite, diisodecyl pentaerythritol phosphite, tris(2,4-di-tert-butylphenyl) phosphite, cyclic neopentanetetraoylbis(octadecyl)phosphite, cyclic neopentanetetraoylbis(2,4-di-tert-butylphenyl)phosphite, cyclic neopentanetetraoylbis(2,4-di-tert-butyl-4-methylphenyl)phosphite, bis[2-tert-butylphenyl]
[0063] Phosphites such as [-6-methyl-4-{2-(octadecyloxycarbonyl)ethyl}phenyl] hydrogen phosphite, oxyphosphaphenanthrene oxides such as 9,10-dihydro-9-oxy-10-phosphaphenanthrene-10-oxide, 10-(3,5-di-tert-butyl-4-hydroxybenzyl)-9,10-dihydro-9-oxy-10-phosphaphenanthrene-10-oxide, and 10-decyloxy-9,10-dihydro-9-oxy-10-phosphaphenanthrene-10-oxide, but are not limited to these.
[0145] Examples of the hindered amine polymerization inhibitor include Adekastab LA-40MP, Adekastab LA-40Si, Adekastab LA-402AF, Adekastab LA-87, Adekastab LA-82, Adekastab LA-81, Adekastab LA-77Y, Adekastab LA-77G, Adekastab LA-72, Adekastab LA-68, Adekastab LA-63P, Adekastab LA-57, Adekastab LA-52, Chimassorb 2020FDL, Chimassorb 944FDL, Chimassorb 944LD, Tinuvin 622SF, Tinuvin PA 144, Tinuvin 765, Tinuvin 770DF, Tinuvin XT55FB, Tinuvin 111FDL, Tinuvin 783FDL, Tinuvin 791FB, etc. manufactured by BASF Japan Co., Ltd., but not limited to these.
[0146] Examples of the nitroso-based polymerization inhibitor include, but are not limited to, p-nitrosophenol, N-nitrosodiphenylamine, ammonium salts of N-nitrosophenylhydroxylamine, and cupferroalan. Among these, ammonium salts of N-nitrosophenylhydroxylamine (cupferroalan) are preferred.
[0147] Examples of the nitroxyl radical polymerization inhibitor include, but are not limited to, di-tert-butyl nitroxide, 2,2,6,6-tetramethylpiperidine-1-oxide, 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxide, 4-oxo-2,2,6,6-tetramethylpiperidine-1-oxide, 4-amino-2,2,6,6-tetramethylpiperidine-1-oxide, 4-methoxy-2,2,6,6-tetramethylpiperidine-1-oxide, 4-acetoxy-2,2,6,6-tetramethylpiperidine-1-oxide, and 4-benzoyloxy-2,2,6,6-tetramethylpiperidine-1-oxide.
[0148] [Polyphenylene ether compound]
[0149] The curable resin composition of the present embodiment may contain a polyphenylene ether compound.
[0150] As the polyphenylene ether compound, from the viewpoint of heat resistance and electrical properties, it is preferably a polyphenylene ether compound having an ethylenic unsaturated bond, and more preferably a polyphenylene ether compound having an acryloyl group, a methacryloyl group, or a styrene structure. As commercially available products, SA-9000 (manufactured by SABIC, a polyphenylene ether compound having a methacryloyl group) and OPE-2St1200 (manufactured by Mitsubishi Gas Chemical Co., Ltd., a polyphenylene ether compound having a styrene structure) etc. can be cited.
[0151] The number average molecular weight (Mn) of the polyphenylene ether compound is preferably 500 to 5000, more preferably 2000 to 5000, and even more preferably 2000 to 4000. If the molecular weight is less than 500, the heat resistance of the cured product tends to be insufficient. In addition, if the molecular weight is greater than 5000, the melt viscosity becomes high, and sufficient fluidity cannot be obtained, which tends to be prone to poor molding. In addition, the reactivity is also reduced, and a long time is required for the curing reaction, the unreacted products that are not included in the curing system increase, the glass transition temperature of the cured product decreases, and the heat resistance of the cured product tends to decrease.
[0152] When the number average molecular weight of the polyphenylene ether compound is 500 to 5000, it can maintain excellent dielectric properties while exhibiting excellent heat resistance and moldability, etc. Specifically, the number average molecular weight can be measured using gel permeation chromatography or the like.
[0153] The polyphenylene ether compound can be obtained by polymerization reaction, or by redistribution reaction of a high molecular weight polyphenylene ether compound with a number average molecular weight of about 10000 to 30000. In addition, free radical polymerizability can be imparted by reacting these as raw materials with compounds having ethylenic unsaturated bonds such as methacryloyl chloride, acryloyl chloride, chloromethyl styrene, etc. The polyphenylene ether compound obtained by redistribution reaction, for example, is obtained by heating a high molecular weight polyphenylene ether compound in a solvent such as toluene in the presence of a phenol compound and a free radical initiator and performing a redistribution reaction. The polyphenylene ether compound obtained by such a redistribution reaction has a hydroxyl group derived from a phenolic compound imparting hardening at both ends of the molecular chain, so that in addition to further maintaining high heat resistance, even after modification with a compound having ethylenic unsaturated bonds, a functional group can be introduced at both ends of the molecular chain, thereby preferably. In addition, the polyphenylene ether compound obtained by polymerization reaction shows excellent fluidity, thereby preferably.
[0154] The molecular weight of the polyphenylene ether compound can be adjusted by adjusting the polymerization conditions, etc. in the case of a polyphenylene ether compound obtained by a polymerization reaction. In addition, in the case of a polyphenylene ether compound obtained by a redistribution reaction, the molecular weight of the obtained polyphenylene ether compound can be adjusted by adjusting the conditions of the redistribution reaction, etc. More specifically, it can be considered to adjust the amount of the phenolic compound used in the redistribution reaction. That is, the more the amount of the phenolic compound is, the lower the molecular weight of the obtained polyphenylene ether compound. At this time, as a high molecular weight polyphenylene ether compound that undergoes the redistribution reaction, poly(2,6-dimethyl-1,4-phenylene ether) can be used. In addition, as a phenolic compound used in the aforementioned redistribution reaction, there is no particular limitation, but it is preferred to use, for example: a multifunctional phenolic compound having two or more phenolic hydroxyl groups in the molecule, such as bisphenol A, phenol novolac, cresol novolac, etc. These can be used alone or in combination of two or more.
[0155] The content of the polyphenylene ether compound is not particularly limited, but is preferably 5 to 1000 parts by mass, more preferably 10 to 750 parts by mass, relative to 100 parts by mass of the compound represented by the above formula (1). When the content of the polyphenylene ether compound is within the above range, not only excellent heat resistance, etc. but also a cured product that fully exhibits the excellent dielectric properties of the polyphenylene ether compound can be obtained, which is preferred.
[0156] [Polybutadiene and its modified products]
[0157] The curable resin composition of the present embodiment may contain polybutadiene and a modified product thereof.
[0158] Polybutadiene and its modified products refer to compounds having polybutadiene or a structure derived from polybutadiene in the molecule. The structure derived from polybutadiene may have some or all unsaturated bonds converted to single bonds by hydrogen addition.
[0159] As polybutadiene and its modified product, for example: polybutadiene, hydroxyl-terminated polybutadiene, terminal (meth) acrylated polybutadiene, carboxylic acid-terminated polybutadiene, amine-terminated polybutadiene, styrene butadiene rubber, etc. can be cited, but it is not limited to these. In addition, one kind can be used, and multiple kinds can also be used in combination. Among these, from the perspective of dielectric properties, polybutadiene or styrene butadiene rubber is preferred. As styrene butadiene rubber (SBR), for example: RICON-100, RICON-181, RICON-184 (all made by CRAY VALLEY), 1,2-SBS (made by Nippon Soda Co., Ltd.), etc., as polybutadiene, B-1000, B-2000, B-3000 (all made by Nippon Soda Co., Ltd.), etc. can be cited. As the molecular weight of polybutadiene and styrene butadiene rubber, the weight average molecular weight is preferably 500 to 10000, more preferably 750 to 7500, and even more preferably 1000 to 5000. Below the lower limit of the above range, the amount of volatility is large, and it is difficult to adjust the solid content when making the prepreg. Above the upper limit of the above range, the compatibility with other curable resins is deteriorated. In general, in the case of compounds containing heteroatoms such as oxygen or nitrogen such as bismaleimide or polymaleimide, it is difficult to ensure compatibility with low-polarity compounds such as compounds mainly composed of hydrocarbons or compounds composed only of hydrocarbons due to their polarity. On the other hand, the compound represented by the above formula (1) is due to the skeleton design that does not actively introduce heteroatoms such as oxygen or nitrogen, so it is also excellent in compatibility with materials having low polarity and low dielectric properties, or compounds composed only of hydrocarbons.
[0160] The content of polybutadiene and its modified product is not particularly limited, but is preferably 5 to 1000 parts by mass, more preferably 10 to 750 parts by mass, relative to 100 parts by mass of the compound represented by the above formula (1). When the polybutadiene and its modified product fall within the above range, not only excellent heat resistance, etc., but also a cured product that fully exhibits the excellent dielectric properties of polybutadiene and its modified product can be obtained, which is preferred.
[0161] [Polystyrene and its modified products]
[0162] The curable resin composition of the present embodiment may contain polystyrene and a modified product thereof.
[0163] Polystyrene and modified products thereof refer to compounds having a structure of polystyrene or a structure derived from polystyrene in the molecule.
[0164] Examples of polystyrene and modified products thereof include polystyrene, styrene and 2-isopropenyl-2-oxazoline copolymers (Epocros RPS-1005 and RP-61, both manufactured by NIPPON SHOKUBAI), SEP (styrene-ethylene and propylene copolymer: SEPTON 1020, manufactured by KURARAY), SEPS (styrene-ethylene and propylene-styrene copolymers: SEPTON 2002, SEPTON 2004F, SEPTON 2005, SEPTON 2006, SEPTON 2063, and SEPTON 2104, all manufactured by KURARAY), SEEPS (styrene-ethylene / ethylene and propylene-styrene block copolymers: SEPTON 4003, SEPTON 4044, SEPTON 4055, SEPTON 4077, and SEPTON 4099, all manufactured by KURARAY), and SEBS (styrene-ethylene and butylene-styrene block copolymer: SEPTON 8004, SEPTON 8006, SEPTON 8007L are all manufactured by KURARAY Co., Ltd.), SEEPS-OH (a compound having a hydroxyl group at the terminal of a styrene-ethylene / ethylene and propylene-styrene block copolymer: SEPTON HG252 manufactured by KURARAY Co., Ltd.), SIS (styrene-isoprene-styrene block copolymer: SEPTON 5125, SEPTON 5127 are all manufactured by KURARAY Co., Ltd.), hydrogenated SIS (hydrogenated styrene-isoprene-styrene block copolymer: HYABRAR 7125F, HYABRAR 7311F are all manufactured by KURARAY Co., Ltd.), SIBS (styrene-isobutylene-styrene block copolymer: SIBSTAR073T, SIBSTAR102T, SIBSTAR103T (all manufactured by Kaneka Co., Ltd.), SEPTON V9827 (manufactured by KURARAY Co., Ltd.) etc., but are not limited to these. In addition, one kind may be used or a plurality of kinds may be used in combination. Polystyrene and its modified products preferably do not have unsaturated bonds, so they have high heat resistance and are difficult to oxidatively degrade. In addition, the weight average molecular weight of polystyrene and its modified products is not particularly limited as long as it is 10,000 or more, but if it is too large, then, in addition to the polyphenylene ether compound, the compatibility with the low molecular weight components of about 50 to 1000 and the oligomer components of about 1000 to 5000 is deteriorated, and it is difficult to ensure mixing and solvent stability, so it is preferably about 10,000 to 300,000.
[0165] The content of polystyrene and its modified products is not particularly limited, but is preferably 5 to 1000 parts by mass, more preferably 10 to 750 parts by mass, relative to 100 parts by mass of the compound represented by the above formula (1). Styrene and its modified products falling within the above range not only have excellent heat resistance, etc., but also can obtain a cured product that fully utilizes the excellent dielectric properties of polystyrene and its modified products, which is preferred.
[0166] [Inorganic filler]
[0167] The curable resin composition of the present embodiment may also contain an inorganic filler. Examples of the inorganic filler include fused silica, crystalline silica, porous silica, alumina, zircon, calcium silicate, calcium carbonate, quartz powder, silicon carbide, silicon nitride, boron nitride, zirconium oxide, aluminum nitride, graphite, forsterite, steatite, spinel, mullite, titanium dioxide, talc, clay, iron oxide asbestos, glass powder and other powders, or inorganic fillers made into spherical shapes or crushed from these, but are not limited to these. In addition, one type may be used, or multiple types may be used in combination.
[0168] In the case of obtaining a curable resin composition for semiconductor sealing, the amount of the inorganic filler used is preferably 80 to 92 parts by mass, more preferably 83 to 90 parts by mass, based on 100 parts by mass of the curable resin composition. In addition, in the case of obtaining a curable resin composition for a substrate material such as an interlayer insulating layer forming material, a copper laminate, a prepreg, or RCC, the amount of the inorganic filler used is preferably 5 to 80 parts by mass, more preferably 10 to 60 parts by mass, based on 100 parts by mass of the curable resin composition.
[0169] [Hardening accelerator]
[0170] The curable resin composition of this embodiment can improve the curability by adding a curing accelerator. As the curing accelerator, it is preferable to generate anions by irradiation of ultraviolet light or visible light or heating to promote the curing reaction, or to generate cations by irradiation of ultraviolet light or visible light or heating to promote the curing reaction.
[0171] Examples of the anionic curing accelerator include imidazoles such as 2-methylimidazole, 2-ethylimidazole, and 2-ethyl-4-methylimidazole, trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, preferably 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene. In addition, examples include phosphines such as triphenylphosphine, tetrabutylammonium salts, triisopropylmethylammonium salts, trimethyldecylammonium salts, hexadecyltrimethylammonium salts, and quaternary ammonium salts such as hexadecyltrimethylammonium hydroxide.
[0172] Examples of the cationic hardening accelerator include quaternary phosphonium salts such as triphenylbenzylphosphonium salt, triphenylethylphosphonium salt, and tetrabutylphosphonium salt (the counter ions of the quaternary salts are halogen, organic acid ions, hydroxide ions, etc., and are not particularly limited, but organic acid ions and hydroxide ions are particularly preferred), transition metal compounds (transition metal salts) such as tin octylate, zinc carboxylates (zinc 2-ethylhexanoate, zinc stearate, zinc behenate, zinc myristate), and zinc phosphates (zinc octyl phosphate, zinc stearyl phosphate), but are not limited to these. In addition, one type may be used, or a plurality of types may be used in combination.
[0173] The amount of the curing accelerator to be added is 0.01 to 5.0 parts by mass, as necessary, based on 100 parts by mass of the total nonvolatile matter excluding the inorganic filler (filler) in the curable resin composition.
[0174] [Polymerization initiator]
[0175] The curable resin composition of this embodiment can also improve the curability by adding a polymerization initiator. The polymerization initiator is a compound that can polymerize olefin functional groups such as ethylenic unsaturated bonds, and includes: olefin metathesis polymerization initiator, anionic polymerization initiator, cationic polymerization initiator, and free radical polymerization initiator. Among them, it is preferred to use a free radical polymerization initiator with curability and moderate stability. In the case of olefin metathesis polymerization initiators such as Schrock catalysts with platinum as the central metal, anionic polymerization initiators such as BuLi, and cationic polymerization initiators such as triethylaluminum, they react with moisture in the air and have poor stability.
[0176] A free radical polymerization initiator refers to a compound that initiates a chain polymerization reaction by generating free radicals through irradiation with ultraviolet light or visible light or heating. Usable free radical polymerization initiators include organic peroxides, azo compounds, and 1,2-tetraphenylethylene glycol (Benzopinacol). Organic peroxides are preferably used in terms of controlling the curing temperature, suppressing degassing, and having little effect on the electrical properties of the decomposed product.
[0177] Examples of the organic peroxide include ketone peroxides such as methyl ethyl ketone peroxide and acetylacetone peroxide, diacyl peroxides such as benzoyl peroxide, diisopropyl peroxides such as dialkyl peroxides such as 1,3-bis-(tert-butylperoxyisopropyl)-benzene, peroxyketals such as tert-butyl peroxybenzoate and 1,1-di-tert-butylperoxycyclohexane, α-cumyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, tert-butyl peroxypivalate, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, and tert-butyl peroxy-2-ethylhexanoate. The alkyl peresters of tert-amyl ethylhexanoate, tert-butyl peroxy-2-ethylhexanoate, tert-amyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxybenzoate, di-2-ethylhexyl peroxydicarbonate, bis(4-tert-butylcyclohexyl) peroxydicarbonate, tert-butyl peroxyisopropyl carbonate, 1,6-bis(tert-butylperoxycarbonyloxy)hexane, etc., peroxycarbonates, tert-butyl hydroperoxide, isopropyl hydroperoxide, tert-butyl peroxyoctanoate, lauroyl peroxide, etc., but are not limited to these. In addition, one kind can be used, and multiple kinds can also be used in combination. Among the above-mentioned organic peroxides, preferably ketone peroxides, diacyl peroxides, hydroperoxides, dialkyl peroxides, peroxyketals, alkyl peresters, peroxycarbonates, etc., more preferably dialkyl peroxides.
[0178] Examples of the azo compound include, but are not limited to, azobisisobutyronitrile, 4,4'-azobis(4-cyanovaleric acid), and 2,2'-azobis(2,4-dimethylvaleronitrile).
[0179] The amount of the polymerization initiator added is preferably 0.01 to 5 parts by mass, particularly preferably 0.01 to 3 parts by mass, based on 100 parts by mass of the total nonvolatile matter excluding the inorganic filler (filler) in the curable resin composition. If the amount of the polymerization initiator used is less than 0.01 parts by mass, the molecular weight may not be sufficiently extended during the polymerization reaction, and if it is more than 5 parts by mass, the dielectric properties such as the dielectric constant and the dielectric loss tangent may be impaired.
[0180] [Flame retardant]
[0181] The curable resin composition of the present embodiment may use a flame retardant. Examples of the flame retardant include halogen flame retardants, inorganic flame retardants (antimony compounds, metal hydroxides, nitrogen compounds, boron compounds, etc.), phosphorus flame retardants, etc., but phosphorus flame retardants are preferred from the viewpoint of achieving halogen-free flame retardancy.
[0182] As the above-mentioned phosphorus flame retardant, it can be a reactive phosphorus flame retardant or an additive phosphorus flame retardant. As a specific example, it can be listed: trimethyl phosphate, triethyl phosphate, tricresyl phosphate, trixylene phosphate, cresol diphenyl phosphate, cresol-di-2,6-xylene phosphate, 1,3-phenylene bis (dixylene phosphate), 1,4-phenylene bis (dixylene phosphate), 4,4'-biphenyl (dixylene phosphate) and other phosphates, 9,10-dihydro-9-oxy-10-phosphaphenanthrene-10-oxide, 10 (2,5-dihydroxyphenyl) -10H-9-oxy-10-phosphaphenanthrene-10-oxide and other phosphanes, and phosphorus containing epoxy compounds, red phosphorus, etc. obtained by reacting epoxy resin with the active hydrogen of the above-mentioned phosphanes, but it is not limited to these. In addition, one type can be used, and multiple types can also be used in combination. Among the above-mentioned exemplified substances, phosphates, phosphanes or phosphorus-containing epoxy compounds are preferred, and 1,3-phenylenebis(dixylene phosphate), 1,4-phenylenebis(dixylene phosphate), 4,4′-biphenyl(dixylene phosphate) or phosphorus-containing epoxy compounds are particularly preferred.
[0183] The content of the flame retardant is preferably in the range of 0.1 to 0.6 parts by mass, based on 100 parts by mass of the total nonvolatile matter excluding the inorganic filler (filler) in the curable resin composition. If it is less than 0.1 parts by mass, the flame retardancy may be insufficient, and if it is more than 0.6 parts by mass, the hygroscopicity and dielectric properties of the cured product may be adversely affected.
[0184] [Light stabilizer]
[0185] The curable resin composition of the present embodiment may use a light stabilizer. The light stabilizer is a hindered amine light stabilizer, and particularly preferably HALS (Hindered Amine Light Stabilizers). Examples of HALS include a reaction product of dibutylamine and 1,3,5-triazine and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl-1,6-hexamethylenediamine and N-(2,2,6,6-tetramethyl-4-piperidinyl)butylamine, a reaction product of dimethyl succinate-1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidinyl, poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidinyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidinyl)imino]}〕, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)〔〔3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl〕methyl〕butyl malonate, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) sebacate, bis(1-octyloxy-2,2,6,6-tetramethyl-4-piperidinyl) sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) 2-(3,5-di-tert-butyl-4-hydroxybenzyl)-2-n-butyl malonate, etc., but are not limited to these. In addition, one kind may be used or a plurality of kinds may be used in combination.
[0186] The content of the light stabilizer is preferably in the range of 0.001 to 10 parts by mass, based on 100 parts by mass of the total nonvolatile matter excluding the inorganic filler (filler) in the curable resin composition. If it is less than 0.001 parts by mass, the light stabilization effect may not be fully exerted, and if it is more than 10 parts by mass, the hygroscopicity and dielectric properties of the cured product may be adversely affected.
[0187] [Binder resin]
[0188] The curable resin composition of this embodiment can use a binder resin. Examples of the binder resin include butyral resins, acetal resins, acrylic resins, epoxy-nylon resins, NBR-phenol resins, epoxy-NBR resins, and silicone resins, but are not limited to these. In addition, one type may be used, or multiple types may be used in combination.
[0189] The amount of the binder resin added is preferably within a range that does not impair the flame retardancy and heat resistance of the cured product, and is preferably 0.05 to 50 parts by mass, more preferably 0.05 to 20 parts by mass, based on 100 parts by mass of the total non-volatile matter excluding the inorganic filler (filler) in the curable resin composition.
[0190] [additive]
[0191] The curable resin composition of the present embodiment may contain additives, such as modified acrylonitrile copolymers, polyethylene, fluororesins, silicone gels, silicone oils, surface treatment agents for fillers of silane coupling agents, release agents, colorants such as carbon black, phthalocyanine blue, and phthalocyanine green.
[0192] The amount of the additive added is preferably 1,000 parts by mass or less, more preferably 700 parts by mass or less, based on 100 parts by mass of the curable resin composition.
[0193] The curable resin composition of this embodiment may further include epoxy resins, active ester compounds, phenol resins, amine resins, maleimide compounds, compounds with ethylenically unsaturated bonds, isocyanate resins, polyamide resins, polyimide resins, cyanate resins, etc. One type may be used or multiple types may be used in combination. Among these compounds, in terms of the balance of heat resistance, adhesion, and dielectric properties, it is preferred to include compounds with ethylenically unsaturated bonds and cyanate resins. By including these compounds, the brittleness of the hardened material can be improved and the adhesion to metal can be improved, and the cracks of the package can be suppressed during reflow soldering and reliability tests such as hot and cold cycles.
[0194] Unless otherwise specified, relative to the compound shown in the aforementioned formula (1), the usage amount of the above-mentioned compound is preferably less than 10 times by mass, more preferably less than 5 times by mass, and particularly preferably less than 3 times by mass. In addition, the preferred lower limit is more than 0.1 times by mass, more preferably more than 0.25 times by mass, and more preferably more than 0.5 times by mass. By being set to within the above range, the effect of each compound to be added can be added while utilizing the effect of the heat resistance and dielectric properties of the compound shown in the aforementioned formula (1). For these components, the components exemplified below can be used.
[0195] [Epoxy resin]
[0196] The epoxy resin includes the following preferred epoxy resins, but is not limited thereto. The epoxy resin may be in a liquid or solid state, and may be used alone or in combination of two or more.
[0197] Examples of the liquid epoxy resin include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol AF epoxy resin, naphthalene epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, phenol novolac epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane epoxy resin, cyclohexanedimethanol epoxy resin, glycidyl amine epoxy resin, and epoxy resin having a butadiene structure. Specific examples include: "RE310S", "RE410S" (all manufactured by Nippon Kayaku Co., Ltd., bisphenol A type epoxy resin), "RE303S", "RE304S", "RE403S", "RE404S" (all manufactured by Nippon Kayaku Co., Ltd., bisphenol F type epoxy resin), "HP4032", "HP4032D", "HP4032SS" (all manufactured by DIC Corporation, naphthalene type epoxy resin), "828US", "jER828EL", "825", "828E L" (above, manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin), "jE807", "1750" (above, manufactured by Mitsubishi Chemical Corporation, bisphenol F type epoxy resin), "jER152" (manufactured by Mitsubishi Chemical Corporation, phenol novolac type epoxy resin), "630", "630LSD" (above, manufactured by Mitsubishi Chemical Corporation, glycidylamine type epoxy resin), "ZX1059" (manufactured by Nippon Steel & Sumitomo Metal Chemicals, a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin), "EX-721" (Nagase ChemteX, glycidyl ester type epoxy resin), "CELLOXIDE 2021P" (Daicel, alicyclic epoxy resin with an ester skeleton), "PB-3600" (Daicel, epoxy resin with a butadiene structure), "ZX1658", "ZX1658GS" (above, Nippon Steel & Sumitomo Metal Chemical Co., Ltd., liquid 1,4-glycidyl cyclohexane type epoxy resin), etc. These may be used alone or in combination of two or more.
[0198] As the solid epoxy resin, for example, there can be mentioned: biphenylol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, phenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, onion type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, tetraphenylethane type epoxy resin, preferably naphthol type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, and biphenyl type epoxy resin. Specific examples include: "HP4032H" (manufactured by DIC Corporation, naphthalene-type epoxy resin), "HP-4700", "HP-4710" (the above are manufactured by DIC Corporation, naphthalene-type tetrafunctional epoxy resins), "N-690" (manufactured by DIC Corporation, cresol novolac-type epoxy resin), "N-695" (manufactured by DIC Corporation, cresol novolac-type epoxy resin), "HP-7200" (manufactured by DIC Corporation, dicyclopentadiene-type epoxy resin), "HP-7200", "HP-7200HH", "HP-7200H" (the above are manufactured by DIC Corporation, dicyclopentadiene-type epoxy resin), epoxy resin), "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP-6000" (above, DIC Corporation, naphthylene ether type epoxy resin), "EPPN-502H" (Nippon Kayaku Co., Ltd., phenol type epoxy resin), "NC-7000L", "NC-7300" (above, Nippon Kayaku Co., Ltd., naphthol-cresol novolac type epoxy resin), "NC-3000H", "NC-3000", "NC-3000L", "NC-3100" (above, Nippon Kayaku Co., Ltd., naphthol-cresol novolac type epoxy resin), "NC-3000H", "NC-3000", "NC-3000L", "NC-3100" (above, Nippon Kayaku Co., Ltd., naphthol-cresol novolac type epoxy resin), ", Nippon Kayaku Co., Ltd., biphenyl aralkyl type epoxy resin), "XD-1000-2L", "XD-1000-L", "XD-1000-H", "XD-1000-H" (above, Nippon Kayaku Co., Ltd., dicyclopentadiene type epoxy resin), "ESN475V" (Nippon Steel & Sumitomo Metal Chemical Co., Ltd., naphthol type epoxy resin), "ESN485" (Nippon Steel & Sumitomo Metal Chemical Co., Ltd., naphthol phenolic type epoxy resin), "YX-4000H", "YX-4000", "YL6121" (above, Mitsubishi Chemical Co., Ltd., biphenyl type epoxy resin), "Y X-4000HK" (manufactured by Mitsubishi Chemical Corporation, dimethylphenol type epoxy resin), "YX-8800" (manufactured by Mitsubishi Chemical Corporation, onion type epoxy resin), "PG-100", "CG-500" (manufactured by Osaka Gas Chemical Co., Ltd., fluorene type epoxy resin), "YL-7760" (manufactured by Mitsubishi Chemical Corporation, bisphenol AF type epoxy resin), "YL-7800" (manufactured by Mitsubishi Chemical Corporation, fluorene type epoxy resin), "jER1010" (manufactured by Mitsubishi Chemical Corporation, solid bisphenol A type epoxy resin), "jER1031S" (manufactured by Mitsubishi Chemical Corporation, tetraphenylethane type epoxy resin), etc.These may be used alone or in combination of two or more.
[0199] [Active ester compound]
[0200] Active ester compounds refer to compounds containing at least one ester bond in the structure, and having aliphatic chains, aliphatic rings or aromatic rings bonded to both sides of the ester bond. As active ester compounds, for example, compounds having two or more highly reactive ester groups in one molecule, such as phenolic esters, thiophenolic esters, N-hydroxylamine esters, esters of heterocyclic hydroxyl compounds, etc., can be cited, which are obtained by condensation reaction of at least one compound of a carboxylic acid compound, an acyl chloride, or a thiocarboxylic acid compound, and at least one compound of a hydroxyl compound or a thiol compound. In particular, from the viewpoint of improving heat resistance, it is preferably obtained from a carboxylic acid compound, an acyl chloride and a hydroxyl compound, and as a hydroxyl compound, a phenolic compound or a naphthol compound is preferably used. One active ester compound can be used alone, or two or more can be used in combination.
[0201] Examples of the carboxylic acid compound include benzoic acid, acetic acid, succinic acid, maleic acid, itaconic acid, phthalic acid, isophthalic acid, terephthalic acid, and pyrophyllic acid.
[0202] Examples of the acid chloride include acetyl chloride, acryloyl chloride, methacryloyl chloride, malonyl chloride, succinoyl chloride, diglycine chloride, glutaric acid dichloride, suberic acid dichloride, sebacic acid dichloride, adipic acid dichloride, dodecanedioyl chloride, nonanoyl chloride, 2,5-furandicarboxylic acid chloride, phthaloyl chloride, isophthaloyl chloride, terephthaloyl chloride, trimellitic acid chloride, bis(4-chlorocarbonylphenyl) ether, 4,4′-diphenyldicarbonyl chloride, and 4,4′-azobisbenzoyl dichloride.
[0203] Examples of the phenol compound and the naphthol compound include hydroquinone, resorcinol, bisphenol A, bisphenol F, bisphenol S, acid phenolphthalein, methylated bisphenol A, methylated bisphenol F, methylated bisphenol S, phenol, o-cresol, m-cresol, p-cresol, catechol, α-naphthol, β-naphthol, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, dihydroxybenzophenone, trihydroxybenzophenone, tetrahydroxybenzophenone, phloroglucinol, benzenetriol, dicyclopentadiene-type diphenol compounds, phenol novolac, and phenol resins described below. Here, the "dicyclopentadiene-type diphenol compound" refers to a diphenol compound obtained by condensing one dicyclopentadiene molecule with two phenol molecules.
[0204] As preferred specific examples of active ester compounds, there can be cited: active ester compounds comprising a dicyclopentadiene type diphenol structure, active ester compounds comprising a naphthalene structure, active ester compounds comprising an acetylated product of phenol novolac, active ester compounds comprising a benzoylated product of phenol novolac, compounds described in Example 2 of International Publication No. 2020 / 095829, and compounds disclosed in International Publication No. 2020 / 059625. Among them, more preferred are active ester compounds comprising a naphthalene structure and active ester compounds comprising a dicyclopentadiene type diphenol structure. The dicyclopentadiene type diphenol structure represents a divalent structural unit consisting of phenylene-dicyclopentene-phenylene.
[0205] Commercially available active ester compounds include, for example, "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", "HPC-8000H-65TM", "EXB-8000L-65TM", and "EXB-8150-65T" (manufactured by DIC Corporation) as active ester compounds containing a dicyclopentadiene-type diphenol structure, and "EXB9416-70BK" (manufactured by DIC Corporation) as active ester compounds containing a naphthalene structure. Examples of active ester compounds containing acetylated products of phenol novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation), examples of active ester compounds containing benzoylated products of phenol novolac include "YLH1026", "YLH1030" and "YLH1048" (manufactured by Mitsubishi Chemical Corporation), examples of active ester curing agents belonging to acetylated products of phenol novolac include "DC808" (manufactured by Mitsubishi Chemical Corporation), and examples of active ester curing agents containing phosphorus atoms include "EXB-9050L-62M" manufactured by DIC Corporation.
[0206] Regarding the mixing ratio of the active ester compound and the epoxy resin, the ratio (α / β) of the active ester equivalent (α) to the epoxy equivalent (β) is preferably 0.5 to 1.5, more preferably 0.8 to 1.2, and even more preferably 0.90 to 1.10. Outside the above range, there is a concern that too much epoxy group or active ester group will remain in the system, and there is a concern that the characteristics will deteriorate in a high temperature storage test (150°C, 1000 hours, etc.) and a long-term reliability test under high temperature and high humidity conditions (temperature: 85°C, humidity: 85%, etc.).
[0207] [Phenolic resin]
[0208] Phenolic resin means a compound having two or more phenolic hydroxyl groups in the molecule. As phenolic resin, for example, reactants of phenols and aldehydes, reactants of phenols and diene compounds, reactants of phenols and ketones, reactants of phenols and substituted biphenyls, reactants of phenols and substituted phenyls, reactants of bisphenols and aldehydes, etc. can be cited, but it is not limited to these. In addition, one type can be used, and multiple types can also be used in combination.
[0209] Specific examples of the above-mentioned raw materials are shown below, but the raw materials are not limited to these.
[0210] <Phenols>
[0211] Phenol, alkyl-substituted phenol, aromatic-substituted phenol, hydroquinone, resorcinol, naphthol, alkyl-substituted naphthol, dihydroxybenzene, alkyl-substituted dihydroxybenzene, dihydroxynaphthalene, etc.
[0212] <Aldehydes>
[0213] Formaldehyde, acetaldehyde, alkyl aldehydes, benzaldehyde, alkyl-substituted benzaldehyde, hydroxybenzaldehyde, naphthaldehyde, glutaraldehyde, phthalaldehyde, crotonaldehyde, cinnamaldehyde, furfural, etc.
[0214] <Diene compounds>
[0215] Dicyclopentadiene, terpenes, vinylcyclohexene, norbornadiene, vinylnorbornene, tetrahydroindene, divinylbenzene, divinylbiphenyl, diisopropenylbiphenyl, butadiene, isoprene, etc.
[0216] <Ketones>
[0217] Acetone, methyl ethyl ketone, methyl isobutyl ketone, acetophenone, benzophenone, fluorenone, etc.
[0218] <Substituted biphenyls>
[0219] 4,4'-bis(chloromethyl)-1,1'-biphenyl, 4,4'-bis(methoxymethyl)-1,1'-biphenyl, 4,4'-bis(hydroxymethyl)-1,1'-biphenyl, etc.
[0220] <Substituted phenyl groups>
[0221] 1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene, 1,4-bis(hydroxymethyl)benzene, etc.
[0222] [Amine resin]
[0223] Amine resin refers to a compound having two or more amino groups in the molecule. Examples of amine resins include diaminodiphenylmethane, diaminodiphenyl sulfone, isophoronediamine, naphthalenediamine, aniline phenol formaldehyde (a reaction product of aniline and formalin), N-toluidine phenol formaldehyde (a reaction product of N-toluidine and formalin), o-ethylaniline phenol formaldehyde (a reaction product of o-ethylaniline and formalin), a reaction product of 2-toluidine and formalin, a reaction product of 2,6-diisopropylaniline and formalin, a reaction product of 2,6-diethylaniline and formalin, a reaction product of 2-ethyl-6-ethylaniline and formalin, a reaction product of 2,6-xylaniline and formalin, an aniline resin obtained by the reaction of aniline and xylene chloride, The reaction products of aniline and substituted biphenyls (4,4'-bis(chloromethyl)-1,1'-biphenyl and 4,4'-bis(methoxymethyl)-1,1'-biphenyl, etc.) described in Japanese Patent No. 6429862, the reaction products of aniline and substituted phenyls (1,4-bis(chloromethyl)benzene, 1,4-bis(methoxymethyl)benzene and 1,4-bis(hydroxymethyl)benzene, etc.), 4,4'-(1,3-phenylenediisopropylidene)dianiline, 4,4'-(1,4-phenylenediisopropylidene)dianiline, the reaction products of aniline and diisopropenylbenzene, dimer diamine, etc. are not limited thereto. In addition, one kind may be used or a plurality of kinds may be used in combination.
[0224] [Maleimide compounds]
[0225] The maleimide compound means a compound having one or more maleimide groups in the molecule. The curable resin composition of the present embodiment may contain a maleimide compound. Examples of the maleic imide compound include 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, m-phenylene bismaleimide, 2,2'-bis[4-(4-maleimide phenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenyl sulfone bismaleimide, 1,3-bis(3-maleimide phenoxy)benzene, 1,3-bis(4-maleimide phenoxy)benzene), Xylo c-type maleic imide compound (ANILIX maleic imide, manufactured by Mitsui Chemicals FINE Co., Ltd.), biphenyl aralkyl type maleic imide compound (a compound solidified by distilling off the solvent from a resin solution containing a maleic imide compound (M2) under reduced pressure as described in Example 4 of JP-A-2009-001783), bisamino isopropylphenylbenzene type maleic imide (maleic imide compound described in International Publication No. 2020 / 054601), maleic imide compound having an indane structure as described in Japanese Patent No. 6629692 or International Publication No. 2020 / 217679, MATERIAL STAGE Vol.18, No.12 2019 "~Continued·Epoxy resin CAS number word~Curing agent CAS number memorandum No. 31 Bismaleimide (1)", and MATERIAL STAGE Vol.19, No.2 2019 "~Continued·Epoxy resin CAS number word~Curing agent CAS number memorandum No. 32 Bismaleimide (2)", etc. disclosed, but are not limited to these. In addition, one kind may be used, or a plurality of kinds may be used in combination.
[0226] Relative to the compound shown in the aforementioned formula (1), the addition amount of the maleimide compound is preferably less than 10 times by mass, more preferably less than 5 times by mass, and particularly preferably less than 3 times by mass. In addition, the preferred lower limit is more than 0.01 times by mass, more preferably more than 0.1 times by mass. Belonging to the above range, the heat resistance, dielectric properties, and low water absorption of the compound shown in the aforementioned formula (1) can be exerted.
[0227] [Compounds containing ethylenically unsaturated bonds]
[0228] The compound containing an ethylenically unsaturated bond means a compound having one or more ethylenically unsaturated bonds that are polymerizable by heat or light in the molecule, regardless of whether a polymerization initiator is used or not.
[0229] Examples of compounds containing ethylenically unsaturated bonds include, but are not limited to, the reaction products of the aforementioned phenol resin and a halogen compound containing an ethylenically unsaturated bond (chloromethylstyrene, allyl chloride, methallyl chloride, acryloyl chloride, methacryloyl chloride, etc.), the reaction products of phenols containing an ethylenically unsaturated bond (2-allylphenol, 2-propenylphenol, 4-allylphenol, 4-propenylphenol, eugenol, isoeugenol, etc.) and a halogen compound (1,4-bis(chloromethyl)benzene, 4,4'-bis(chloromethyl)biphenyl, 4,4'-difluorobenzophenone, 4,4'-dichlorobenzophenone, 4,4'-dibromobenzophenone, cyanuric chloride, etc.), the reaction products of epoxy resins or alcohols and (meth)acrylic acids (acrylic acid, methacrylic acid, etc.), and acid-modified products thereof. In addition, one type may be used, or a plurality of types may be used in combination.
[0230] [Isocyanate resin]
[0231] The isocyanate resin means a compound having two or more isocyanate groups in the molecule. As isocyanate resins, for example, aromatic diisocyanates such as p-phenylene diisocyanate, m-phenylene diisocyanate, p-xylylene diisocyanate, m-xylylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, and naphthalene diisocyanate, aliphatic or alicyclic diisocyanates such as isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, hydrogenated xylylene diisocyanate, norbornene diisocyanate, and lysine diisocyanate, biuret forms of one or more isocyanate monomers, polyisocyanates such as isocyanate forms obtained by tripolymerization of the above diisocyanate compounds, and polyisocyanates obtained by urea reaction of the above isocyanate compounds with polyol compounds, but are not limited thereto. In addition, one type may be used, or a plurality of types may be used in combination.
[0232] [Polyamide resin]
[0233] Examples of the polyamide resin include reaction products of at least one of diamine, diisocyanate, and oxazoline with dicarboxylic acid, reaction products of diamine and acid chloride, and ring-opening polymers of lactam compounds.
[0234] Specific examples of the above-mentioned raw materials are shown below, but the raw materials are not limited to these.
[0235] <Diamine>
[0236] Ethylenediamine, trimethylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decanediamine, undecanediamine, dodecanediamine, tridecanediamine, tetradecanediamine, pentadecanediamine, hexadecanediamine, heptadecanediamine, octadecanediamine, nonadecanediamine, eicosanediamine, 2-methyl-1,5-diaminopentane, 2-methyl-1,8-diaminooctane, di Polydiamine, cyclohexanediamine, bis-(4-aminocyclohexyl)methane, bis(3-methyl-4-aminocyclohexyl)methane, benzyl diamine, norbornane diamine, isophorone diamine, bisaminomethyl tricyclodecane, phenylenediamine, diethyltoluenediamine, naphthalene diamine, diaminodiphenylmethane, bis(4-amino-3,5-dimethylphenyl)methane bis(4-amino-3,5-diethylphenyl)methane, 4,4'-methylenebis-o-methyl Aniline, 4,4'-methylenebis-o-ethylaniline, 4,4'-methylenebis-2-ethyl-6-toluidine, 4,4'-methylenebis-2,6-diisopropylaniline, 4,4-ethylenedianiline, diaminodiphenyl sulfone, diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4-bis(4-aminophenoxy)biphenyl, 2,2-bis[4-(4-aminophenoxy) )phenyl]propane, bis[4-(4-aminophenoxy)phenyl]sulfone, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-(1,3-phenylenediisopropylidene)dianiline, 4,4'-(1,4-phenylenediisopropylidene)dianiline, 9,9-bis(4-aminophenyl)fluorene, 2,7-diaminofluorene, aminobenzylamine, diaminobenzophenone, etc.
[0237] <Diisocyanate>
[0238] Phenyl diisocyanate, toluene diisocyanate, 1,3-bis(isocyanatomethyl)benzene, 1,3-bis(isocyanatomethyl)cyclohexane, bis(4-isocyanatophenyl)methane, isophorone diisocyanate, 1,3-bis(2-isocyanato-2-propyl)benzene, 2,2-bis(4-isocyanatophenyl)hexafluoropropane, dicyclohexylmethane-4,4'-diisocyanate, etc.
[0239] <Dicarboxylic acid>
[0240] Oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, terephthalic acid, isophthalic acid, 5-hydroxyisophthalic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, 5-sodium sulfonate of isophthalic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, cyclohexanedicarboxylic acid, biphenyldicarboxylic acid, naphthalene dicarboxylic acid, benzophenone dicarboxylic acid, furandicarboxylic acid, 4,4'-dicarboxy diphenyl ether, 4,4'-dicarboxy diphenyl sulfide, etc.
[0241] <Acid chloride>
[0242] Acetyl chloride, acryloyl chloride, methacryloyl chloride, malonyl chloride, succinoyl chloride, diglycine chloride, glutaric acid dichloride, suberic acid dichloride, sebacic acid dichloride, adipic acid dichloride, dodecanoyl chloride, nonanoyl chloride, 2,5-furandicarboxylic acid chloride, phthaloyl chloride, isophthaloyl chloride, terephthaloyl chloride, trimesoyl chloride, bis(4-chlorocarbonylphenyl) ether, 4,4'-diphenyldicarbonyl chloride, 4,4'-azodibenzoyl chloride, etc.
[0243] <Lactam>
[0244] ε-caprolactam, ω-undecanolactam, ω-laurolactam, etc.
[0245] [Polyimide resin]
[0246] Examples of the polyimide resin include, but are not limited to, a reaction product of the aforementioned diamine and the tetracarboxylic dianhydride exemplified below.
[0247] <Tetracarboxylic dianhydride>
[0248] 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-cyclohexene-1,2-dicarboxylic anhydride, pyromelitic dianhydride, 1,2,3,4-benzenetetracarboxylic anhydride, 3,3',4,4'-benzophenonetetracarboxylic anhydride, 2,2',3,3'-benzophenonetetracarboxylic anhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic anhydride, 2,2',3,3'-biphenyltetracarboxylic anhydride, methylene-4,4'-diphthalic anhydride, 1,1-ethylene-4,4'-diphthalic anhydride, 2,2'-propylene-4,4'-diphthalic anhydride, 1,2-ethylene-4 ,4'-diphthalic dianhydride, 1,3-trimethylene-4,4'-diphthalic dianhydride, 1,4-tetramethylene-4,4'-diphthalic dianhydride, 1,5-pentamethylene-4,4'-diphthalic dianhydride, 4,4'-oxydiphthalic dianhydride, thio-4,4'-diphthalic dianhydride, sulfonyl-4,4'-diphthalic dianhydride, 1,3-bis(3,4-dicarboxyphenyl)phthalic dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,3-bis[2-(3,4-dicarboxyphenyl)-2-propyl]phthalic dianhydride, 1,4-bis[2-(3,4-dicarboxyphenyl)-2-propyl]phthalic dianhydride 1,3-bis(3,4-dicarboxyphenyl)-1,1,3,3-tetramethyldisiloxane dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 2,3,6,7-oniontetracarboxylic dianhydride, 1,2,7 ,8-phenanthrene tetracarboxylic dianhydride, ethylene tetracarboxylic dianhydride, 1,2,3,4-butane tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride), cyclopentane tetracarboxylic dianhydride, cyclohexane-1,2,3,4-tetracarboxylic dianhydride, cyclohexane-1,2,4,5-tetracarboxylic dianhydride, 3,3',4,4'-dicyclohexyl tetracarboxylic dianhydride, carbonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, methylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 1,2-ethylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 1,1-ethylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, 2,2-propylene-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, oxy-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, thio-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, sulfonyl-4,4'-bis(cyclohexane-1,2-dicarboxylic acid) dianhydride, bicyclo[2,2,2]oct-7-ene-2,3,5,6-tetracarboxylic acid dianhydride, rel-[1S,5R,6R]-3-oxabicyclo[3, 2,1] octan-2,4-dione-6-spiro-3'-(tetrahydrofuran-2',5'-dione), 4-(2,5-dioxo-tetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride, ethylene glycol-bis-(3,4-dicarboxylic anhydride phenyl) ether, 4,4'-biphenyl bis(trimellitic acid monoester anhydride), 9,9'-bis(3,4-dicarboxyphenyl)fluorene dianhydride, etc.
[0249] [Cyanate ester resin]
[0250] The cyanate resin is a cyanate compound obtained by reacting a phenol resin with a cyanogen halide, and specific examples thereof include dicyanate benzene, tricyanate benzene, dicyanate naphthalene, dicyanate biphenyl, 2,2'-bis(4-cyanate phenyl) propane, bis(4-cyanate phenyl) methane, bis(3,5-dimethyl-4-cyanate phenyl) methane, 2,2'-bis(3,5-dimethyl-4-cyanate phenyl) propane, 2,2'-bis(4-cyanate phenyl) ethane, 2,2'-bis(4-cyanate phenyl) hexafluoropropane, bis(4-cyanate phenyl) sulfone, bis(4-cyanate phenyl) sulfide, phenol novolac cyanate, phenol-dicyclopentadiene cocondensate in which a hydroxyl group is converted into a cyanate group, etc., but the present invention is not limited thereto. In addition, one type may be used, or a plurality of types may be used in combination.
[0251] Furthermore, the cyanate ester compound whose synthesis method is described in Japanese Patent Application Laid-Open No. 2005-264154 is particularly preferred as the cyanate ester compound because of its low hygroscopicity, flame retardancy, and excellent dielectric properties.
[0252] In order to trimerize the cyanate groups to form s-triazine rings as required, the cyanate resin may contain a catalyst such as zinc naphthenate, cobalt naphthenate, copper naphthenate, lead naphthenate, zinc octylate, tin octylate, lead acetylacetonate, dibutyltin maleate, etc.
[0253] The catalyst is used in an amount of preferably 0.0001 to 0.10 parts by mass, more preferably 0.00015 to 0.0015 parts by mass, based on 100 parts by mass of the cyanate ester resin.
[0254] The curable resin composition of the present embodiment is obtained by preparing the above-mentioned components at a predetermined ratio, pre-curing at 130 to 180° C. for 30 to 500 seconds, and post-curing at 150 to 200° C. for 2 to 15 hours to achieve a sufficient curing reaction, thereby obtaining the cured product of the present embodiment. Alternatively, the components of the curable resin composition may be uniformly dispersed or dissolved in a solvent, etc., and cured after removing the solvent.
[0255] The preparation method of the curable resin composition of the present embodiment is not particularly limited, but the components may be uniformly mixed or prepolymerized. For example, a mixture containing the compound represented by the above formula (1) and other compounds may be heated in the presence or absence of a curing accelerator or a polymerization initiator, and in the presence or absence of a solvent, thereby prepolymerizing. Similarly, amine compounds, compounds having ethylenically unsaturated bonds, maleimide compounds, cyanate compounds, compounds such as polybutadiene and its modified products, polystyrene and its modified products, inorganic fillers, and other additives may be added and prepolymerized. The mixing or prepolymerization of the components may be performed in the absence of a solvent, for example, using an extruder, a kneader, a roller press, etc., and in the presence of a solvent, using a reactor with a stirring device, etc.
[0256] As a method of uniform mixing, kneading is performed at a temperature in the range of 50 to 100°C using a kneader, a roller press, a planetary mixer, etc. to obtain a uniform resin composition. The obtained resin composition can also be crushed and then molded into a cylindrical ingot with a molding machine such as a tablet press, or made into a granular powder, or a powdery molded body, or these compositions can be melted on a surface support to form a sheet with a thickness of 0.05 mm to 10 mm, thereby obtaining a curable resin composition molded body. The obtained molded body becomes a non-sticky molded body at 0 to 20°C, and the fluidity and curability are hardly reduced even if stored at -25 to 0°C for more than 1 week.
[0257] The obtained molded body can be molded into a hardened product using a transfer molding machine or a compression molding machine.
[0258] The curable resin composition of the present embodiment may also be added with an organic solvent to form a varnish-like composition (hereinafter referred to as varnish). If necessary, the curable resin composition of the present embodiment is dissolved in a solvent such as toluene, xylene, acetone, methyl ethyl ketone, methyl isobutyl ketone, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, etc. to form a varnish, which is impregnated into a substrate such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, paper, etc. and heated and dried, and the obtained prepreg is hot-pressed to obtain a cured product of the curable resin composition of the present embodiment. At this time, the amount of the solvent used in the mixture of the curable resin composition of the present embodiment and the solvent is 10 to 70% by weight, preferably 15 to 70% by weight. In addition, if it is a liquid composition, a cured resin containing carbon fibers can be directly obtained by, for example, RTM.
[0259] In addition, the curable composition of this embodiment can also be used as a modifier for a film-type composition. Specifically, it can be used in the case of improving flexibility in the B-stage. Such a film-type resin composition is obtained by applying the curable resin composition of this embodiment as the aforementioned curable resin composition varnish on a release film, removing the solvent under heating, and then performing B-stage to obtain a sheet-like adhesive. This sheet-like adhesive can be used as an interlayer insulating layer in a multilayer substrate, etc.
[0260] The curable resin composition of the present embodiment can also be melted by heating, reduced in viscosity, and impregnated with reinforcing fibers such as glass fibers, carbon fibers, polyester fibers, polyamide fibers, and alumina fibers to obtain a prepreg. As specific examples thereof, glass fibers such as E glass cloth, D glass cloth, S glass cloth, Q glass cloth, spherical glass cloth, NE glass cloth, and T glass cloth, inorganic fibers other than glass, and organic fibers such as poly(p-phenylene terephthalamide) (Kevlar (registered trademark), manufactured by DuPont), wholly aromatic polyamide, polyester, poly(p-phenylene benzoxazole), polyimide, and carbon fibers can be cited, but are not limited to these. The shape of the substrate is not particularly limited, but examples thereof include woven fabrics, non-woven fabrics, rovings, and chopped strand mats. In addition, as a weaving method for the woven fabric, plain weave fabrics, basket weave fabrics, and twill fabrics are known, and can be appropriately selected and used from these well-known materials according to the intended use and performance. In addition, it is preferred to use a woven fabric that has been subjected to fiber opening treatment or a glass woven fabric that has been surface treated with a silane coupling agent or the like. The thickness of the substrate is not particularly limited, but is preferably about 0.01 to 0.4 mm. In addition, a prepreg can also be obtained by impregnating the reinforcing fiber in the above-mentioned varnish and heating and drying it.
[0261] In addition, the above-mentioned prepreg can also be used to manufacture a laminate. As long as the laminate has more than one prepreg, there is no particular limitation and it can have any other layers. As a manufacturing method for the laminate, there is no particular limitation, and a generally known method can be appropriately applied. For example, when the metal foil-clad laminate is formed, a multi-stage press, a multi-stage vacuum press, a continuous molding machine, a high-pressure tank molding machine, etc. can be used to obtain a laminate by stacking the above-mentioned prepregs on each other and heating and pressurizing. At this time, the heating temperature is not particularly limited, but is preferably 65 to 300°C, more preferably 120 to 270°C. In addition, the pressurization pressure is not particularly limited, but if the pressure is too large, it is difficult to adjust the solid content of the resin of the laminate and the quality is unstable. In addition, if the pressure is too small, bubbles will appear and the adhesion between the layers will deteriorate. Therefore, it is preferably 2.0 to 5.0MPa, and more preferably 2.5 to 4.0MPa. The laminate of this embodiment can be preferably used as a metal foil-clad laminate described later by having a layer composed of metal foil.
[0262] The above-mentioned prepreg is cut into a desired shape, and after being laminated with copper foil or the like as needed, the laminate is pressed by a press molding method, an autoclave molding method, a sheet winding molding method, etc., while the curable resin composition is heated and cured, thereby obtaining an electrical and electronic laminate (printed wiring board) or a carbon fiber reinforced material.
[0263] The curable resin composition of the present embodiment can also be used as a resin sheet. As a method for obtaining a resin sheet from the curable resin composition of the present embodiment, for example, a method of applying the curable resin composition on a support film (support) and then drying it to form a resin composition layer on the support film can be cited. In the case where the curable resin composition of the present embodiment is used for a resin sheet, the film softens under the lamination temperature conditions (70°C to 140°C) in the vacuum lamination method, and at the same time as the lamination of the circuit substrate, it is important to show fluidity (resin flow) that allows the resin to fill the vias or through holes present in the circuit substrate, and it is preferred to formulate the above-mentioned components that exhibit such characteristics. In addition, in the obtained resin sheet and circuit substrate (copper laminate, etc.), there is no phenomenon of locally different characteristic values due to phase separation, etc., and in order to show certain performance in any part, appearance uniformity is required.
[0264] Here, the through hole of the circuit board has a diameter of 0.1 to 0.5 mm and a depth of 0.1 to 1.2 mm, which is preferably a range in which resin filling can be performed. In addition, when laminating both surfaces of the circuit board, it is desirable to fill the through hole by about 1 / 2.
[0265] As a specific method for producing the aforementioned resin sheet, there can be cited a method in which an organic solvent is formulated into a varnished resin composition, the varnished resin composition is applied to the surface of a support film (Y), and the organic solvent is dried by further heating or blowing hot air to form a resin composition layer (X).
[0266] As the organic solvent used here, it is preferred to use ketones such as acetone, methyl ethyl ketone, and cyclohexanone, acetates such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate, carbitols such as cellosolve and butyl carbitol, aromatic hydrocarbons such as toluene and xylene, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, etc., and it is preferably used in a ratio of 30 to 60% by mass of non-volatile matter.
[0267] In addition, the thickness of the aforementioned resin composition layer (X) formed must be more than the thickness of the conductor layer. Since the thickness of the conductor layer possessed by the circuit substrate is in the range of 5 to 70 μm, the thickness of the aforementioned resin composition layer (X) preferably has a thickness of 10 to 100 μm. In addition, the aforementioned resin composition layer (X) in the present embodiment can be protected by a protective film described later. By protecting with a protective film, dust etc. can be prevented from adhering to the surface of the resin composition layer and scratches on the surface of the resin composition layer.
[0268] The supporting film and the protective film include polyolefins such as polyethylene, polypropylene, and polyvinyl chloride, polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate, polycarbonate, polyimide, and release paper or metal foils such as copper foil and aluminum foil. In addition, the supporting film and the protective film may be subjected to MAD treatment, corona treatment, and release treatment. The thickness of the supporting film is not particularly limited, but is used in the range of 10 to 150 μm, preferably 25 to 50 μm. In addition, the thickness of the protective film is preferably 1 to 40 μm.
[0269] The support film (Y) is peeled off after being laminated on the circuit board or after forming the insulating layer by heat curing. After the resin composition layer constituting the resin sheet is heat cured, the support film (Y) is peeled off to prevent the adhesion of dust and the like during the curing step. When peeling off after curing, the support film is subjected to release treatment in advance.
[0270] In addition, a multilayer printed circuit board can be manufactured from the resin sheet obtained according to the above. For example, in the case where the resin composition layer (X) is protected by a protective film, after peeling these, the layer (X) of the resin composition is laminated on one or both sides of the circuit substrate in a manner that directly contacts the circuit substrate, for example, by a vacuum lamination method. The lamination method may be batch type or continuous type using a roller press. In addition, as needed, the resin sheet and the circuit substrate may be heated (preheated) as needed before lamination. The lamination conditions are preferably set to a crimping temperature (lamination temperature) of 70 to 140°C and a crimping pressure of 1 to 11 kgf / cm 2 (9.8×10 4 to 107.9×10 4 N / m 2 ), stack the layers under reduced pressure with air pressure below 20 mmHg (26.7 hPa).
[0271] In addition, the curable resin composition of this embodiment can be used to manufacture a semiconductor device. Examples of the semiconductor device include DIP (dual in-line package), QFP (quad flat package), BGA (ball grid array), CSP (crystal size package), SOP (small outline package), TSOP (thin small outline package), TQFP (thin quad flat package), etc.
[0272] The curable resin composition of the present embodiment and its cured product can be used in a wide range of fields. Specifically, it can be used in various applications such as molding materials, bonding agents, composite materials, coatings. Due to the cured product of the curable resin composition recorded in the present embodiment showing excellent heat resistance and dielectric properties, it is therefore preferred to be used in electrical and electronic components such as semiconductor element sealants, liquid crystal display element sealants, organic EL element sealants, laminates (printed wiring boards, BGA substrates, assembly substrates, etc.) and carbon fiber reinforced plastics, glass fiber reinforced plastics, etc. Lightweight high-strength structural materials composite materials, 3D printing, etc.
[0273] [Example]
[0274] Next, the present invention will be described in more detail by way of examples. Hereinafter, unless otherwise specified, parts are parts by mass. However, the present invention is not limited to these examples.
[0275] Various analytical methods used in the Examples are described below.
[0276] <Weight average molecular weight (Mw), number average molecular weight (Mn), GPC area percentage of the total amount of the compound in which n in the above formula (1) is 1>
[0277] The weight average molecular weight (Mw) and the number average molecular weight (Mn) were calculated in terms of polystyrene using a polystyrene standard solution.
[0278] GPC: Online degasser (DGU-20A3R), binary liquid transfer device (LC-20AD), autosampler (SIL-20AHT), differential refractive index detector (RID-20A), column oven (CTO-20A), system controller (CBM-20A) (all made by Shimadzu Corporation)
[0279] Column: Shodex KF-603×1, KF-602.5×1, KF-602×1, KF-601×1 (all made by Showa Denko Co., Ltd.)
[0280] Protection column: Shodex KF-G 4A (manufactured by Showa Denko Co., Ltd.)
[0281] Combined eluent: tetrahydrofuran
[0282] Flow rate: 1.5ml / min.
[0283] Column temperature: 40℃
[0284] Detection: RI (differential refractive index detector)
[0285] The slice data of the chromatogram is obtained, and the ratio (area percentage) of the area of the slice data corresponding to the compound where n is 1 in formula (1) to the sum of the areas (time-integrated values of signal values) of the slice data corresponding to the compound represented by formula (1) is calculated.
[0286] <Content ratio of the compounds represented by formulas (2) to (4)>
[0287] HP-LC: binary liquid transfer device (LC-20AB), online degasser (DGU-20A3), autosampler (SIL-20A), column oven (CTO-20A), system controller (CBM-20A), photodiode array detector (SPD-M20A) (all made by Shimadzu Corporation)
[0288] Column: ODS-2 (manufactured by GL Sciences)
[0289] Combined eluent: tetrahydrofuran: water = 3:1 (no gradient)
[0290] Flow rate: 0.5ml / min.
[0291] Column temperature: 40℃
[0292] Detection: PDA (Photodiode Array Detector)
[0293] Detector: 274nm
[0294] In the chromatogram obtained by high performance liquid chromatography (HP-LC), the sum of the peak areas (α) of the compounds represented by formulae (2) to (4) and the peak area (β) of the compound wherein n is 1 in formula (1) are calculated, and (α / β) is calculated.
[0295] <Structural Analysis>
[0296] LC-MS: Ultra-high performance liquid chromatography (UHPLC) system (Ultimate 3000), mass spectrometer (Q-Exactive (registered trademark)) (both manufactured by Thermo Fisher Scientific Inc.)
[0297] Column: ODS-2 (manufactured by GL Sciences)
[0298] Combined eluent: tetrahydrofuran: water = 3:1 (no gradient)
[0299] Flow rate: 0.5ml / min.
[0300] Ionization mode: ESI
[0301] Mass range: m / z = 150-2000
[0302] [Synthesis example 1]
[0303] In a flask equipped with a thermometer, a cooling tube, and a stirrer, an aspirator and a base trap were set. 370.1 parts of (2-bromoethyl)benzene (manufactured by Tokyo Chemical Industry Co., Ltd.), 175.1 parts of α,α'-dichloro-p-xylene (manufactured by Tokyo Chemical Industry Co., Ltd.), and 27.3 parts of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) were placed in the flask, and the generated hydrogen chloride was collected with the base trap while reacting at 130°C for 6 hours. 50 parts of methanol and 700 parts of cyclohexane were added, and after neutralization with 56.8 parts of a 30% aqueous sodium hydroxide solution, the organic layer was washed 5 times with 100 parts of water. The solvent and excess (2-bromoethyl)benzene were distilled off under heating and reduced pressure to obtain 380 parts (Mn: 938, Mw: 1290) of a compound (BEB-1) having a (2-bromoethyl)benzene structure represented by the following formula (6) as a liquid resin. The GPC chart of the obtained compound is shown in Figure 1 The average value of the repeating unit n calculated based on the area percentage of the GPC chart is ave The ratio (area percentage) of the area of the compound having a structure in which n is 1 in the formula (6) to the total area of the compound having a structure represented by the formula (6) in the GPC chart was 45%.
[0304]
[0305] [Example 1]
[0306] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 300 parts of BEB-1 obtained in Synthesis Example 1, 245 parts of toluene, 735 parts of dimethyl sulfoxide, 0.15 parts of 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxide free radical, and 146.4 parts of a 50wt% sodium hydroxide aqueous solution were added, and the reaction was continued at 40°C for 6 hours. After adding 100 parts of water and washing the organic layer, the organic layer was returned to the reaction container. 735 parts of dimethyl sulfoxide and 9.8 parts of a 50wt% sodium hydroxide aqueous solution were added, and the reaction was again carried out at 40°C for 1 hour. 1050 parts of toluene were added, and the organic layer was repeatedly washed with 100 parts of water until the waste water was neutral. The mixture was concentrated under reduced pressure using an evaporator to obtain 180 parts of a compound (O-1) having two or more styrene structures in the molecule represented by the following formula (7). The GPC chart of the obtained compound is shown in Figure 2 In addition, the obtained compound 1 H-NMR data (deuterated chloroform) are shown in Figure 3 .exist 1 The signals derived from the vinyl group were observed at 5.10-5.30 ppm, 5.50-5.85 ppm, and 6.60-6.80 ppm in the H-NMR chart. The average value of the repeating unit n calculated from the area percentage of the GPC chart was ave The ratio (area percentage) of the area of the compound having a structure in which n is 1 in the GPC chart to the total area of the compound having the structure represented by the formula (7) is 40% (the average molecular weight of the resin component is Mn: 803, Mw: 1190). The LC-MS chart is shown in Figure 4 , the HP-LC graph is shown in Figure 5 . Compounds V to Y shown in Table 1 (Table 1 records representative structural formulas) were detected by LC-MS analysis. In compound W, the positions of the 2-phenylethanol structure and the styrene structure are in no particular order. In compound X, the positions of the 2-phenylethanol structure, the styrene structure and the 2-phenylacetaldehyde structure are in no particular order. In compound Y, the positions of the 2-phenylethanol structure and the ethylbenzene structure are in no particular order, and the phenethyl group can be bonded to any aromatic ring.
[0307]
[0308] [Table 1]
[0309]
[0310] [Example 2]
[0311] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 300 parts of BEB-1 obtained in Synthesis Example 1, 245 parts of toluene, 735 parts of dimethyl sulfoxide, 0.15 parts of 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxide free radical, and 107.4 parts of a 50wt% sodium hydroxide aqueous solution were added, and the reaction was continued at 40°C for 6 hours. After adding 100 parts of water and washing the organic layer, the organic layer was returned to the reaction container. 735 parts of dimethyl sulfoxide and 9.8 parts of a 50wt% sodium hydroxide aqueous solution were added, and the reaction was again carried out at 40°C for 1 hour. 1050 parts of toluene were added, and the organic layer was repeatedly washed with 100 parts of water until the waste water was neutral. The mixture was concentrated under reduced pressure using an evaporator to obtain 180 parts of a compound (O-2) having two or more styrene structures in the molecule represented by the aforementioned formula (7). The GPC graph of the obtained compound is shown in Figure 6 The average value of the repeating unit n calculated based on the area percentage of the GPC chart is ave The ratio (area percentage) of the area of the compound having a structure in which n is 1 in the formula (7) to the total area of the compound having the structure represented by the formula (7) in the GPC chart is 41% (the average molecular weight of the resin component is Mn: 799, Mw: 1297). The HP-LC chart is shown in Figure 7 .
[0312] [Example 3]
[0313] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 300 parts of BEB-1 obtained in Synthesis Example 1, 375 parts of toluene, 1125 parts of dimethyl sulfoxide, 0.15 parts of 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxide free radical, and 146.4 parts of a 50wt% sodium hydroxide aqueous solution were added, and the reaction was continued at 40°C for 6 hours. After adding 100 parts of water and washing the organic layer, the organic layer was returned to the reaction container. 735 parts of dimethyl sulfoxide and 9.8 parts of a 50wt% sodium hydroxide aqueous solution were added, and the reaction was again carried out at 40°C for 1 hour. 1050 parts of toluene were added, and the organic layer was repeatedly washed with 100 parts of water until the waste water was neutral. The mixture was concentrated under reduced pressure using an evaporator to obtain 180 parts of a compound (O-3) having two or more styrene structures in the molecule represented by the aforementioned formula (7). The GPC graph of the obtained compound is shown in Figure 8 The average value of the repeating unit n calculated based on the area percentage of the GPC chart is ave The ratio (area percentage) of the area of the compound having a structure in which n is 1 in the formula (7) to the total area of the compound having the structure represented by the formula (7) in the GPC chart is 35% (the average molecular weight of the resin component is Mn: 834, Mw: 1170). The HP-LC chart is shown in Fig. 9 .
[0314] [Example 4]
[0315] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 300 parts of BEB-1 obtained in Synthesis Example 1, 245 parts of toluene, 735 parts of dimethyl sulfoxide, 0.15 parts of 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxide free radical, and 146.4 parts of a 50wt% sodium hydroxide aqueous solution were added, and the reaction was continued at 25°C for 6 hours. After adding 100 parts of water and washing the organic layer, the organic layer was returned to the reaction container. 735 parts of dimethyl sulfoxide and 9.8 parts of a 50wt% sodium hydroxide aqueous solution were added, and the reaction was again carried out at 25°C for 1 hour. 1050 parts of toluene were added, and the organic layer was repeatedly washed with 100 parts of water until the waste water was neutral. The evaporator was used to concentrate under reduced pressure to obtain 180 parts of a compound (O-4) having two or more styrene structures in the molecule represented by the aforementioned formula (7). The GPC chart of the obtained compound is shown in Fig.10 The average value of the repeating unit n calculated based on the area percentage of the GPC chart is ave The ratio (area percentage) of the area of the compound having a structure in which n is 1 in the GPC chart to the total area of the compound having the structure represented by the formula (7) is 41% (the average molecular weight of the resin component is Mn: 802, Mw: 1291). The HP-LC chart is shown in Fig.11 .
[0316] [Comparative Synthesis Example 1]
[0317] In a flask equipped with a thermometer, a cooling tube, and a stirrer, an aspirator and an alkali trap are set. 296 parts of (2-bromoethyl)benzene (manufactured by Tokyo Chemical Industry Co., Ltd.), 70 parts of α,α'-dichloro-p-xylene (manufactured by Tokyo Chemical Industry Co., Ltd.), and 18.4 parts of methanesulfonic acid (manufactured by Tokyo Chemical Industry Co., Ltd.) are placed in the flask, and the generated hydrogen chloride is collected with an alkali trap while reacting at 130°C for 6 hours. 50 parts of methanol and 700 parts of cyclohexane are added, and after neutralization with 26.8 parts of a 30% aqueous sodium hydroxide solution, the organic layer is washed 5 times with 100 parts of water. The solvent and excess (2-bromoethyl)benzene are distilled off under heating and reduced pressure to obtain 171 parts (Mn: 793, Mw: 970) of a compound (BEB-2) having a (2-bromoethyl)benzene structure represented by the above formula (6) as a liquid resin. The GPC chart of the obtained compound is shown in Fig.12 The average value of the repeating unit n calculated from the area percentage of the GPC chart is ave n is 1.6. In the GPC chart, the ratio of the area of the compound having the structure in which n is 1 in formula (6) to the total area of the compound having the structure represented by formula (6) (GPC area percentage) is 65%.
[0318] [Comparative Synthesis Example 2]
[0319] In a flask equipped with a thermometer, a cooling tube, and a stirrer, 22 parts of BEB-2 obtained in Comparative Synthesis Example 1, 50 parts of toluene, 150 parts of dimethyl sulfoxide, 15 parts of water, and 5.4 parts of sodium hydroxide were added, and the reaction was continued at 40°C for 6 hours. 100 parts of toluene were added, and the organic layer was repeatedly washed with 100 parts of water until the waste water was neutral. The evaporator was used to concentrate under reduced pressure to obtain 12.5 parts of a compound (O-5) having two or more styrene structures in the molecule represented by the aforementioned formula (7). The GPC chart of the obtained compound is shown in Fig.13 The average value of the repeating unit n calculated based on the area percentage of the GPC chart is ave The ratio of the area of the compound having the structure in which n is 1 in the formula (7) to the total area of the compound having the structure represented by the formula (7) (GPC area percentage) was 65% (the average molecular weight of the resin component was Mn: 624, Mw: 778). The HP-LC graph is shown in Fig.14 .
[0320] As molecular weight data of compounds O-1 to O-5, the number average molecular weight (Mn), weight average molecular weight (Mw) and area percentage of the compound where n is 1 in formula (1) are taken as "n=1 content (GPC area %)", the sum α of the peak areas of the compounds represented by formulas (2) to (4) in the chromatogram obtained by HPLC is taken as "the total content of compounds V to Y in each compound (HP-LC area)", the peak area β of the compound where n is 1 in formula (1) is taken as "n=1 content (HP-LC area)", and the value of α divided by β (α / β) are recorded in Table 2.
[0321] [Table 2]
[0322]
[0323] [Examples 5 to 8, Comparative Example 1]
[0324] <Stability test after solvent dissolution>
[0325] After preparing 1.2 g of compounds O-1 to O-5 and 0.8 g of toluene in a 5 mL glass sample bottle, a roll mixer (MIX-ROTAR VMR-5: manufactured by AS ONE) was used to stir at 100 rpm for 1 hour at 25°C to prepare a 60 wt% toluene solution of each compound. The obtained solution was stored in a freezer at -18°C, and the sample was taken out after 10 minutes and evaluated according to the following criteria. The results are shown in Table 3.
[0326] ·No crystal precipitation: ○
[0327] · Crystallization: ×
[0328] <Dielectric constant test and dielectric loss tangent test>
[0329] Compounds O-1 to O-5 were vacuum pressed while being held by mirror copper foil (T4X: manufactured by Futian Metal Copper Foil Co., Ltd.) and cured at 220°C for 2 hours. Thereafter, the samples were cut into a sample size of 1.7 mm in width × 100 mm in length × 0.2 mm in thickness using a laser cutter, and tested by the cavity resonator perturbation method using a 10 GHz cavity resonator manufactured by ATE Co., Ltd. The evaluation results are shown in Table 3.
[0330] [Table 3]
[0331]
[0332] From the results in Table 3, it was confirmed that Examples 5 to 8 had excellent stability after solvent dissolution and excellent dielectric properties.
[0333] This application claims priority based on Japanese patent application No. 2022-54487 filed on March 29, 2022.
Claims
1. A compound represented by the following formula (1), wherein the compound in which n in the formula (1) is 1 accounts for less than 50% of the total amount of the compound in terms of GPC area percentage; In formula (1), the multiple Rs independently represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms; p and r are integers from 0 to 4, and q is an integer from 0 to 3; n is a repetition number, and the average value of n is n ave Conform to 1≤n ave ≤20.
2. The compound according to claim 1, in, The value of α / β, which is the sum of the peak areas α of the compounds represented by the following formulae (2) to (4) divided by the peak area β of the compound represented by the formula (1) where n is 1, is 0.10 or less; In formula (2), the multiple Rs each independently represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms; the multiple s each independently represent an integer from 0 to 4; In formula (3), the multiple Rs each independently represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms; the multiple As each independently represent any one of the following formulae (3-a) to (3-c); the multiple s each independently represent an integer from 0 to 4, and t is an integer from 0 to 3; In formulae (3-a) to (3-c), * represents the position of bonding to the aromatic ring of the compound of formula (3); In formula (4), multiple Rs are independently a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms; multiple Bs are independently the following formula (4-d) or (4-e); D is the following formula (4-f); multiple ss are independently an integer from 0 to 4, and t is an integer from 0 to 3; one of the five ms in formula (4) is 1, and the remaining four are 0; In formulae (4-d) to (4-f), * represents a position bonded to the aromatic ring of the compound of formula (4).
3. The compound according to claim 1 or 2, in, In the formula (1), p=0, q=0, and r=0.
4. A compound according to any one of claims 1 to 3, in, The compound represented by the formula (1) is derived from the compound represented by the following formula (5); In formula (5), multiple Rs exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms; p and r are integers from 0 to 4, q is an integer from 0 to 3, n is a repetition number, and the average value of n is n ave Conform to 1≤n ave ≤20; X represents a halogen atom.
5. The mixture according to any one of claims 1 to 4, further comprising a polymerization inhibitor. 6 . A curable resin composition comprising the compound according to claim 1 , or the mixture according to claim 5 . 7 . The curable resin composition according to claim 6 , comprising at least one of a polyphenylene ether compound, polybutadiene and a modified product thereof, and polystyrene and a modified product thereof. 8 . The curable resin composition according to claim 6 , comprising a radical polymerization initiator. 9 . A cured product obtained by curing the compound according to claim 1 , the mixture according to claim 5 , or the curable resin composition according to claim 6 .
10. A method for producing a compound represented by the following formula (1), comprising subjecting a compound represented by the following formula (5) to a dehydrohalogenation reaction in the presence of a basic catalyst in a solvent having an amount of 4 to 7 times the weight of the compound represented by the following formula (5); In formula (1), the multiple Rs exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms; p and r are integers from 0 to 4, q is an integer from 0 to 3, n is a repetition number, and the average value of n is n ave Conform to 1≤n ave ≤20; In formula (5), multiple Rs exist independently and represent a hydrocarbon group or a halogenated alkyl group having 1 to 10 carbon atoms; p and r are integers from 0 to 4, q is an integer from 0 to 3, n is a repetition number, and the average value of n is n ave Conform to 1≤n ave ≤20; X represents a halogen atom.
11. A method for producing the compound according to claim 10, in, The solvent is a mixed solvent of an aprotic polar solvent and a water-insoluble solvent.
12. The method for producing the compound according to claim 11, in, The usage amount of the aprotic polar solvent is 1 to 10 times the weight of the water-insoluble solvent.
13. A method for producing a compound according to claim 11 or 12, in, Dimethyl sulfoxide was used as the aprotic polar solvent, and toluene was used as the water-insoluble solvent.
Citation Information
Patent Citations
Curable resin composition, prepreg, metal-clad laminate, printed wiring board
JP2020105352A
Compound, mixture, curable resin composition and cured product thereof, and compound production method
WO2021100658A1
Resin composition, prepreg using same, film with resin, metal foil with resin, metal-clad laminate, and wiring board
WO2022244728A1