Composite negative electrode material, preparation method thereof, negative electrode sheet and sodium ion battery
By coating the surface of activated carbon with asphalt to seal the pores, a composite negative electrode material was prepared, which solved the problems of low initial efficiency of hard carbon and large specific surface area of activated carbon, and improved the energy density and cycle performance of sodium-ion batteries.
Patent Information
- Application Number
- CN202411176342.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Existing hard carbon anode materials have low initial efficiency and low compaction, resulting in poor performance of sodium-ion batteries. Activated carbon, when used as an anode material, has a large specific surface area, low initial coulombic efficiency, and large irreversible capacity.
A composite negative electrode material was prepared by coating asphalt on the surface of activated carbon using a solid-phase mixing coating method to seal some of the open pores. This material was then applied to the negative electrode sheet in sodium-ion batteries.
It improves the energy density and cycle performance of sodium-ion batteries, reduces irreversible sodium adsorption and electrolyte decomposition, and enhances the initial coulombic efficiency and reversible capacity.
Smart Images

Figure CN119038523B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of sodium-ion battery technology, and particularly relates to a composite negative electrode material and its preparation method, a negative electrode sheet, and a sodium-ion battery. Background Technology
[0002] With the rapid development of renewable energy technologies, the requirements for energy storage are becoming increasingly economical and secure. The widespread use of lithium-ion batteries has also exacerbated the scarcity of lithium resources, which will severely limit the future development of the energy storage sector. Compared to lithium-ion batteries, sodium-ion batteries have advantages such as abundant reserves, wide distribution, and lower cost, and are expected to become the mainstream in the future energy storage field, offering more possibilities for development.
[0003] In the field of sodium-ion battery anode materials, the graphite structure, which is originally suitable for lithium-ion battery anodes, is difficult to apply to sodium-ion battery anodes because the atomic radius of sodium is much larger than that of lithium. Amorphous carbon is considered a more suitable anode material for sodium-ion batteries due to its good sodium storage capacity, high reversible specific capacity, good cycle performance, and obvious commercialization trend. Amorphous carbon can be divided into soft carbon and hard carbon. Soft carbon usually refers to carbon materials that can be graphitized after high-temperature treatment (above 2800℃), and its disordered structure is easily eliminated; it is also called easily graphitized carbon. Hard carbon usually refers to carbon that is difficult to completely graphitize even after high-temperature treatment (above 2800℃), and its disordered structure is difficult to eliminate at high temperatures; it is also called difficult-to-graphitize carbon. Hard carbon is currently the most widely chosen anode material for sodium-ion batteries due to its advantages such as good conductivity, high sodium storage capacity, small volume deformation after sodium intercalation, environmental friendliness, and low redox potential. However, the low initial efficiency and low compaction of hard carbon also limit its application. Sodium-ion batteries made of hard carbon have poor performance, so further regulation is needed.
[0004] Activated carbon has attracted much attention due to its high specific surface area, low cost, tunable pore structure, and good electrical conductivity, electrochemical stability, and thermal stability. However, activated carbon contains a large number of micropores and mesopores, with a specific surface area ranging from 500 to 2000 m². 2 Directly using activated carbon as the anode material for sodium-ion batteries often results in poor performance, exhibiting low initial coulombic efficiency and large irreversible capacity during discharge. However, the microporous structure of activated carbon itself is beneficial for sodium storage. Therefore, using activated carbon as a raw material and controlling its pore structure through various methods to prepare carbon materials can improve the sodium storage capacity of hard carbon anodes. Summary of the Invention
[0005] The purpose of this invention is to overcome the above-mentioned problems in the prior art and provide a composite negative electrode material. This composite negative electrode material is made by coating a layer of asphalt on the surface of activated carbon through a solid-phase mixing coating method, which can seal some of the open pores of activated carbon, greatly reduce the specific surface area of the material, and reduce the active sites on the material surface that come into contact with the electrolyte. This composite negative electrode material is applied to a negative electrode sheet, and the negative electrode sheet is applied to a sodium-ion battery. This sodium-ion battery has high energy density and good cycle performance.
[0006] To achieve the above-mentioned technical objectives and effects, the present invention is implemented through the following technical solution:
[0007] An embodiment of the first aspect of the present invention provides a method for preparing a composite negative electrode material, the method comprising the following steps:
[0008] S101: After pulverizing activated carbon and asphalt separately, they are made into fine activated carbon powder and fine asphalt powder. The fine activated carbon powder and fine asphalt powder are then mixed in a VC mixer to prepare fine powder raw materials.
[0009] S102: After adding a crosslinking agent to the fine powder raw material, continue mixing. After mixing evenly, carry out a crosslinking reaction at low temperature to prepare the precursor material.
[0010] S103: The precursor material is carbonized at high temperature in an inert gas atmosphere and then cooled to prepare a composite anode material.
[0011] Furthermore, the activated carbon is any one or more of wood-based activated carbon, coal-based activated carbon, coconut shell activated carbon, and fruit shell activated carbon, mixed in any proportion;
[0012] The asphalt is any one or more of petroleum asphalt, coal tar pitch, and natural asphalt mixed in any proportion;
[0013] The crosslinking agent is either p-toluenesulfonic acid or terephthalaldehyde;
[0014] The inert gas is any one or more of nitrogen, helium, and argon mixed in any proportion.
[0015] Furthermore, the D50 of the activated carbon fine powder is not greater than 5 μm;
[0016] The D50 of the asphalt powder is not greater than 3 μm.
[0017] Further, in step S101, the mass ratio of activated carbon fine powder to asphalt fine powder in the fine powder raw material is (2-4):1.
[0018] Furthermore, in step S102, the mass ratio of the fine powder raw material to the crosslinking agent is 2:1.
[0019] Furthermore, in step S102, the crosslinking reaction temperature is 120-280℃, and the crosslinking reaction time is 2-10h.
[0020] Furthermore, in step S103, the high-temperature carbonization temperature is 1200-1500℃, and the high-temperature carbonization time is 2-5h.
[0021] A second aspect of the present invention provides a composite anode material, which is prepared by the method for preparing the composite anode material provided in the first aspect of the present invention.
[0022] An embodiment of the third aspect of the present invention provides a negative electrode sheet, comprising, by weight percentage: 70-90% composite negative electrode material and 10-30% Super P-PVDF;
[0023] The composite anode material is prepared by the method for preparing composite anode materials provided in the first aspect of the present invention.
[0024] The Super P-PVDF is made by mixing ultrafine conductive carbon black and polyvinylidene fluoride in a mass ratio of 1:1.
[0025] An embodiment of the fourth aspect of the present invention provides a sodium-ion battery, including the negative electrode sheet provided in the embodiment of the third aspect of the present invention.
[0026] Compared with the prior art, the beneficial effects of the present invention are:
[0027] 1. This invention provides a composite anode material, which is prepared by crushing activated carbon and asphalt to a certain size, mixing them, adding a crosslinking agent after mixing, and performing crosslinking at a certain temperature to obtain a precursor material, and then carbonizing the precursor material at a high temperature to obtain the composite anode material.
[0028] 2. The composite negative electrode material provided by the present invention is made by coating a layer of asphalt on the surface of activated carbon through a solid-phase mixing coating method, which can seal some of the open pores of activated carbon, greatly reduce the specific surface area of the material, and reduce the active sites on the material surface that come into contact with the electrolyte. The composite negative electrode material is applied to the negative electrode sheet, and the negative electrode sheet is applied to the sodium-ion battery, which has high energy density and good cycle performance.
[0029] 3. In this invention, since the asphalt coating on the surface of activated carbon can close some of the open pores, the number of active sites on the material surface in contact with the electrolyte is reduced. Therefore, it can hinder some irreversible sodium adsorption, inhibit the decomposition of the electrolyte, and reduce the occurrence of side reactions. In addition, after closing a large number of open pores into closed pores, it is more conducive to the storage of sodium ions, thereby improving the initial coulombic efficiency and reversible capacity. Attached Figure Description
[0030] The accompanying drawings, which are included to provide a further understanding of the invention and form part of this application, illustrate exemplary embodiments of the invention and, together with their description, serve to explain the invention and do not constitute an undue limitation thereof. In the drawings:
[0031] Figure 1 This is a schematic diagram of the first charge and discharge of a sodium-ion battery prepared with the composite negative electrode material provided in Embodiment 1 of the present invention. Detailed Implementation
[0032] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0033] An embodiment of the first aspect of the present invention provides a method for preparing a composite negative electrode material, the method comprising the following steps:
[0034] S101: Activated carbon and asphalt are pulverized separately to make fine activated carbon powder and fine asphalt powder, wherein the D50 of the fine activated carbon powder is not greater than 5μm and the D50 of the fine asphalt powder is not greater than 3μm.
[0035] Then, the activated carbon powder and asphalt powder are mixed in a VC mixer at a mass ratio of (2-4):1 to prepare fine powder raw materials.
[0036] The activated carbon is any one or more of wood-based activated carbon, coal-based activated carbon, coconut shell activated carbon, and fruit shell activated carbon, mixed in any proportion;
[0037] Asphalt is any one or more of petroleum asphalt, coal tar pitch, and natural asphalt mixed in any proportion;
[0038] S102: After adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, the mixture is further mixed and after being mixed evenly, a crosslinking reaction is carried out at 120-280℃ for 2-10 hours to prepare the precursor material.
[0039] The crosslinking agent is either p-toluenesulfonic acid or terephthalaldehyde.
[0040] S103: The precursor material is carbonized at high temperature in an inert gas atmosphere, wherein the inert gas is any one or more of nitrogen, helium and argon mixed in any proportion, the high temperature carbonization temperature is 1200-1500℃, the high temperature carbonization time is 2-5h, and after high temperature carbonization, it is cooled to prepare the composite anode material.
[0041] The second aspect of the present invention provides a composite anode material, which is prepared by a method for preparing a composite anode material provided in the first aspect of the present invention.
[0042] An embodiment of the third aspect of the present invention provides a negative electrode sheet, which comprises, by weight percentage: 70-90% composite negative electrode material and 10-30% Super P-PVDF;
[0043] The composite anode material is prepared by the method for preparing composite anode materials provided in the first aspect of the present invention.
[0044] Super P-PVDF is made by mixing ultrafine conductive carbon black and polyvinylidene fluoride in a mass ratio of 1:1.
[0045] The fourth aspect of the present invention also provides a sodium-ion battery, including the negative electrode sheet provided in the third aspect of the present invention;
[0046] The sodium-ion battery also includes an electrolyte, a separator, and a positive electrode.
[0047] Specifically, the electrolyte uses EC (ethylene carbonate) and DEC (diethyl carbonate) as solvents and sodium hexafluorophosphate as solute. The volume ratio of EC to DEC in the electrolyte is 1:1, and the concentration of sodium hexafluorophosphate is 1 mol / L.
[0048] The diaphragm is made of glass fiber;
[0049] The positive electrode is a sodium plate.
[0050] The following are specific embodiments. Unless otherwise specified, all raw materials in the following embodiments can be obtained commercially.
[0051] In the following examples, the activated carbon is wood-based activated carbon, the asphalt is natural asphalt, the crosslinking agent is p-toluenesulfonic acid, and the inert gas is nitrogen.
[0052] Example 1
[0053] This embodiment provides a method for preparing a composite anode material, which includes the following steps:
[0054] S101: Activated carbon and asphalt are pulverized separately to make fine activated carbon powder and fine asphalt powder, wherein the D50 of the fine activated carbon powder is 5μm and the D50 of the fine asphalt powder is 3μm.
[0055] Next, fine activated carbon powder and fine asphalt powder are mixed in a VC mixer at a mass ratio of 3:1 to prepare fine powder raw materials.
[0056] S102: After adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, the mixture is further mixed. After the mixture is uniform, the temperature is raised to 160℃ at a rate of 2℃ / min and kept at the temperature for 5 hours to complete the crosslinking reaction, thereby preparing the precursor material.
[0057] S103: The precursor material is placed in an inert gas atmosphere and heated to 1400℃ at a heating rate of 5℃ / min. The temperature is maintained for 2 hours to complete the high-temperature carbonization. After high-temperature carbonization, the material is cooled to obtain the composite anode material.
[0058] Example 2
[0059] This embodiment provides a method for preparing a composite anode material, which includes the following steps:
[0060] S101: Activated carbon and asphalt are pulverized separately to make fine activated carbon powder and fine asphalt powder, wherein the D50 of the fine activated carbon powder is 5μm and the D50 of the fine asphalt powder is 3μm.
[0061] Next, fine activated carbon powder and fine asphalt powder are mixed in a VC mixer at a mass ratio of 3:1 to prepare fine powder raw materials.
[0062] S102: After adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, the mixture is further mixed. After the mixture is uniform, the temperature is raised to 120℃ at a rate of 2℃ / min and kept at the temperature for 5 hours to complete the crosslinking reaction, thereby preparing the precursor material.
[0063] S103: The precursor material is placed in an inert gas atmosphere and heated to 900°C at a heating rate of 5°C / min. The temperature is maintained for 3 hours to complete the high-temperature carbonization. After high-temperature carbonization, the material is cooled to obtain the composite anode material.
[0064] Example 3
[0065] This embodiment provides a method for preparing a composite anode material, which includes the following steps:
[0066] S101: Activated carbon and asphalt are pulverized separately to make fine activated carbon powder and fine asphalt powder, wherein the D50 of the fine activated carbon powder is 5μm and the D50 of the fine asphalt powder is 3μm.
[0067] Next, fine activated carbon powder and fine asphalt powder are mixed in a VC mixer at a mass ratio of 3:1 to prepare fine powder raw materials.
[0068] S102: After adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, the mixture is further mixed. After the mixture is uniform, the temperature is raised to 280℃ at a rate of 2℃ / min and kept at the temperature for 2 hours to complete the crosslinking reaction, thereby preparing the precursor material.
[0069] S103: The precursor material is placed in an inert gas atmosphere and heated to 1000℃ at a heating rate of 5℃ / min. The temperature is maintained for 2 hours to complete the high-temperature carbonization. After high-temperature carbonization, the material is cooled to obtain the composite anode material.
[0070] Example 4
[0071] This embodiment provides a method for preparing a composite anode material, which includes the following steps:
[0072] S101: Activated carbon and asphalt are pulverized separately to make fine activated carbon powder and fine asphalt powder, wherein the D50 of the fine activated carbon powder is 5μm and the D50 of the fine asphalt powder is 3μm.
[0073] Next, fine activated carbon powder and fine asphalt powder are mixed in a VC mixer at a mass ratio of 3:1 to prepare fine powder raw materials.
[0074] S102: After adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, the mixture is further mixed. After the mixture is uniform, the temperature is raised to 160℃ at a rate of 2℃ / min and kept at the temperature for 5 hours to complete the crosslinking reaction, thereby preparing the precursor material.
[0075] S103: The precursor material is placed in an inert gas atmosphere and heated to 1100℃ at a heating rate of 5℃ / min. The temperature is maintained for 2 hours to complete the high-temperature carbonization. After high-temperature carbonization, the material is cooled to obtain the composite anode material.
[0076] Example 5
[0077] This embodiment provides a method for preparing a composite anode material, which includes the following steps:
[0078] S101: Activated carbon and asphalt are pulverized separately to make fine activated carbon powder and fine asphalt powder, wherein the D50 of the fine activated carbon powder is 5μm and the D50 of the fine asphalt powder is 3μm.
[0079] Next, fine activated carbon powder and fine asphalt powder are mixed in a VC mixer at a mass ratio of 3:1 to prepare fine powder raw materials.
[0080] S102: After adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, the mixture is further mixed. After the mixture is uniform, the temperature is raised to 120℃ at a rate of 2℃ / min and kept at the temperature for 5 hours to complete the crosslinking reaction, thereby preparing the precursor material.
[0081] S103: The precursor material is placed in an inert gas atmosphere and heated to 1200℃ at a heating rate of 5℃ / min. The temperature is maintained for 2 hours to complete the high-temperature carbonization. After high-temperature carbonization, the material is cooled to obtain the composite anode material.
[0082] Example 6
[0083] This embodiment provides a method for preparing a composite anode material, which includes the following steps:
[0084] S101: Activated carbon and asphalt are pulverized separately to make fine activated carbon powder and fine asphalt powder, wherein the D50 of the fine activated carbon powder is 5μm and the D50 of the fine asphalt powder is 3μm.
[0085] Next, fine activated carbon powder and fine asphalt powder are mixed in a VC mixer at a mass ratio of 3:1 to prepare fine powder raw materials.
[0086] S102: After adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, the mixture is further mixed. After the mixture is uniform, the temperature is raised to 160℃ at a rate of 2℃ / min and kept at the temperature for 5 hours to complete the crosslinking reaction, thereby preparing the precursor material.
[0087] S103: The precursor material is placed in an inert gas atmosphere and heated to 1300℃ at a heating rate of 5℃ / min. The temperature is maintained for 2 hours to complete the high-temperature carbonization. After high-temperature carbonization, the material is cooled to obtain the composite anode material.
[0088] Example 7
[0089] This embodiment provides a method for preparing a composite anode material, which includes the following steps:
[0090] S101: Activated carbon and asphalt are pulverized separately to make fine activated carbon powder and fine asphalt powder, wherein the D50 of the fine activated carbon powder is 5μm and the D50 of the fine asphalt powder is 3μm.
[0091] Next, fine activated carbon powder and fine asphalt powder are mixed in a VC mixer at a mass ratio of 3:1 to prepare fine powder raw materials.
[0092] S102: After adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, the mixture is further mixed. After the mixture is uniform, the temperature is raised to 280℃ at a rate of 2℃ / min and kept at the temperature for 2 hours to complete the crosslinking reaction, thereby preparing the precursor material.
[0093] S103: The precursor material is placed in an inert gas atmosphere and heated to 1500℃ at a heating rate of 5℃ / min. The temperature is maintained for 2 hours to complete the high-temperature carbonization. After high-temperature carbonization, the material is cooled to obtain the composite anode material.
[0094] Example 8
[0095] This embodiment provides a method for preparing a composite anode material, which includes the following steps:
[0096] S101: Activated carbon and asphalt are pulverized separately to make fine activated carbon powder and fine asphalt powder, wherein the D50 of the fine activated carbon powder is 5μm and the D50 of the fine asphalt powder is 3μm.
[0097] Next, fine activated carbon powder and fine asphalt powder are mixed in a VC mixer at a mass ratio of 2:1 to prepare fine powder raw materials.
[0098] S102: After adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, the mixture is further mixed. After the mixture is uniform, the temperature is raised to 160℃ at a rate of 2℃ / min and kept at the temperature for 5 hours to complete the crosslinking reaction, thereby preparing the precursor material.
[0099] S103: The precursor material is placed in an inert gas atmosphere and heated to 1400℃ at a heating rate of 5℃ / min. The temperature is maintained for 2 hours to complete the high-temperature carbonization. After high-temperature carbonization, the material is cooled to obtain the composite anode material.
[0100] Example 9
[0101] This embodiment provides a method for preparing a composite anode material, which includes the following steps:
[0102] S101: Activated carbon and asphalt are pulverized separately to make fine activated carbon powder and fine asphalt powder, wherein the D50 of the fine activated carbon powder is 5μm and the D50 of the fine asphalt powder is 3μm.
[0103] Next, fine activated carbon powder and fine asphalt powder are mixed in a VC mixer at a mass ratio of 4:1 to prepare fine powder raw materials.
[0104] S102: After adding a crosslinking agent to the fine powder raw material, wherein the mass ratio of the fine powder raw material to the crosslinking agent is 2:1, the mixture is further mixed. After the mixture is uniform, the temperature is raised to 160℃ at a rate of 2℃ / min and kept at the temperature for 5 hours to complete the crosslinking reaction, thereby preparing the precursor material.
[0105] S103: The precursor material is placed in an inert gas atmosphere and heated to 1400℃ at a heating rate of 5℃ / min. The temperature is maintained for 2 hours to complete the high-temperature carbonization. After high-temperature carbonization, the material is cooled to obtain the composite anode material.
[0106] Comparative Example 1
[0107] This comparative example provides a method for preparing a composite anode material, which includes the following steps:
[0108] Activated carbon was pulverized to form fine activated carbon powder with a D50 of 5 μm. The fine activated carbon powder was heated to 1400°C in a tube furnace under a nitrogen atmosphere at a heating rate of 5°C / min and held at that temperature for 2 hours. After the reaction was completed, it was cooled to room temperature to prepare the negative electrode material.
[0109] The experimental conditions in Examples 1-9 and Comparative Example 1 are shown in Table 1.
[0110] Table 1
[0111]
[0112]
[0113] Performance testing
[0114] The composite anode materials prepared in Examples 1-9 and the anode material prepared in Comparative Example 1 were used in sodium-ion batteries, specifically as follows:
[0115] The sodium-ion battery includes a negative electrode, an electrolyte, a separator, and a positive electrode.
[0116] The composite anode materials prepared in Examples 1-9 and the anode material prepared in Comparative Example 1 were respectively mixed with SuperP-PVDF to prepare various mixtures. The mixtures consisted of 80% composite anode material and 20% SuperP-PVDF by mass percentage. The mixtures were then pressed into sheets to prepare anode sheets.
[0117] Super P-PVDF is a mixture of ultrafine conductive carbon black and polyvinylidene fluoride in a mass ratio of 1:1.
[0118] The electrolyte uses EC (ethylene carbonate) and DEC (diethyl carbonate) as solvents and sodium hexafluorophosphate as solute. The volume ratio of EC to DEC in the electrolyte is 1:1, and the concentration of sodium hexafluorophosphate is 1 mol / L.
[0119] The diaphragm is made of glass fiber;
[0120] The positive electrode is a sodium plate;
[0121] The components of the above sodium-ion battery—negative electrode, electrolyte, separator, and positive electrode—were processed into CR2032 coin cells, and their performance was tested. The test conditions were: first, a 0.1C rate discharge, then a 0.02mA constant current discharge, and then a 0.1C rate charge. The test results are shown in Table 1.
[0122] Table 1
[0123]
[0124]
[0125] As can be seen from the data in Table 1, compared with Comparative Example 1, the sodium-ion battery prepared by the composite negative electrode material provided in Examples 1-9 has better reversible capacity and first-efficiency than the Comparative Example.
[0126] Figure 1 This is a schematic diagram of the first charge and discharge of a sodium-ion battery prepared using the composite negative electrode material provided in Example 1.
[0127] The composite anode material provided by this invention is prepared by crushing activated carbon and asphalt to a certain size, mixing them, adding a crosslinking agent, and crosslinking them at a certain temperature to obtain a precursor material. The precursor material is then carbonized at a high temperature to obtain the composite anode material. The composite anode material is applied to a negative electrode sheet, and the negative electrode sheet is applied to a sodium-ion battery. The sodium-ion battery prepared has high energy density and good cycle performance.
[0128] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0129] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.
Claims
1. A method for preparing a composite negative electrode material, characterized in that, The preparation method includes the following steps: S101: After pulverizing activated carbon and asphalt separately, they are made into activated carbon fine powder and asphalt fine powder, wherein the D50 of the activated carbon fine powder is not greater than 5μm and the D50 of the asphalt fine powder is not greater than 3μm; the activated carbon fine powder and asphalt fine powder are mixed in a VC mixer at a mass ratio of (2-4):1 to prepare fine powder raw materials. S102: After adding the crosslinking agent to the fine powder raw material, continue mixing. The mass ratio of the fine powder raw material to the crosslinking agent is 2:
1. After mixing evenly, the temperature is raised to 160℃ at a rate of 2℃ / min and kept at the temperature for 5 hours to complete the crosslinking reaction. The precursor material is then prepared at low temperature. S103: The precursor material is carbonized at high temperature in an inert gas atmosphere and then cooled to prepare a composite anode material. The activated carbon is any one or more of wood-based activated carbon, coal-based activated carbon, coconut shell activated carbon, and fruit shell activated carbon, mixed in any proportion; The asphalt is any one or more of petroleum asphalt, coal tar pitch, and natural asphalt mixed in any proportion; The crosslinking agent is either p-toluenesulfonic acid or terephthalaldehyde; The inert gas is any one or more of nitrogen, helium, and argon mixed in any proportion; In step S103, the high-temperature carbonization temperature is 1200-1500℃, and the high-temperature carbonization time is 2-5h.
2. A composite negative electrode material, characterized in that, It is prepared by the method for preparing the composite negative electrode material according to claim 1.
3. A negative electrode sheet, characterized in that, By weight percentage, it includes: 70-90% composite anode material and 10-30% SuperP-PVDF; The composite anode material is prepared by the method for preparing the composite anode material according to claim 1; The Super P-PVDF is made by mixing ultrafine conductive carbon black and polyvinylidene fluoride in a mass ratio of 1:
1.
4. A sodium-ion battery, characterized in that, Includes the negative electrode sheet as described in claim 3.
Citation Information
Patent Citations
Sodium ion battery negative electrode material based on carbon material and pitch and preparation method and application thereof
CN109148838A
Oxidized asphalt-based hard carbon negative electrode material for sodium-ion battery and preparation method of oxidized asphalt-based hard carbon negative electrode material
CN115991467A
Sodium-ion battery carbon negative electrode material composite particle and preparation method and device thereof