Aluminum-magnesium-lithium alloy capable of reducing deformation and cracking as well as preparation method and application of aluminum-magnesium-lithium alloy

By optimizing the composition and process of Al-Mg-Li alloy and adding elements such as Cu and Zr, the problem of cracks and wrinkles during the deformation process of the alloy is solved, the thermal stability and thermal processing performance are improved, and the tensile strength is enhanced and elongation, improving the advantages of lightweight applications.

CN119040711APending Publication Date: 2024-11-29HUNAN ZHUOCHUANG PRECISION MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411498313.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-25
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Al-Mg-Li alloy is prone to cracks and wrinkles during deformation, and its forming performance is poor, and its tissue stability is affected by process parameters, making it difficult to improve thermal stability and thermal processing performance on the basis of ensuring mechanical properties.

Method used

By optimizing the alloy composition, adding Cu, Zr and other elements, the Cu content is controlled at 0.2-0.3%, the Mg content is 4.5-5.6%, and the Li content is 1.8-2.3%, and homogenization and rolling are carried out to control The heating speed and deformation amount reduce deformation and cracking.

Benefits of technology

It effectively improves the thermal stability and thermal processing performance of Al-Mg-Li alloy, reduces the tendency of deformation and cracking, and at the same time enhances the tensile strength and elongation, improving its advantages in lightweight applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040711A_ABST
    Figure CN119040711A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of aluminum alloy material preparation, and particularly relates to an aluminum-magnesium-lithium alloy capable of reducing deformation cracking and a preparation method and application thereof.The aluminum-magnesium-lithium alloy capable of reducing deformation cracking comprises, by weight, 0.2%-0.3% of Cu, 4.5%-5.6% of Mg, 1.8%-2.3% of Li, 0.08%-0.15% of refined metal and the balance A1 and inevitable impurities, the refined metal is one or more of Zr and Sc, and the inevitable impurities are one or more of Al, Mg and Li. According to the invention, on the basis of ensuring better mechanical properties, the thermal stability and the hot working property of the alloy are improved, and the strength and the ductility are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aluminum alloy material preparation, and in particular relates to an aluminum-magnesium-lithium alloy capable of reducing deformation and cracking, a preparation method and an application thereof. Background Art

[0002] Al-Mg-Li alloys offer excellent properties such as low density, high specific strength, and excellent corrosion resistance, making them widely used in aerospace, automotive, and other fields. Al-Mg-Li alloys can achieve a density of 2450-2500 kg / m³, which is lower than other Al-Li alloys such as Al-Cu-Li, offering advantages in lightweighting. In the aerospace sector, Al-Mg-Li alloys are used in the manufacture of key structural components such as aircraft fuselages, wings, and engine parts, reducing aircraft weight and improving flight performance.

[0003] Al-Mg-Li alloy is mainly composed of three elements: aluminum (Al), magnesium (Mg) and lithium (Li). Other trace elements may also be added to improve the alloy properties. The addition of magnesium improves the strength and corrosion resistance of the alloy; while the addition of lithium significantly reduces the density of the alloy while increasing the elastic modulus and specific strength.

[0004] "Microstructure and Properties of Al-Li-Cu-Mg Alloys," Xu Xiaochen, Shenyang Aerospace University, Master's Thesis, page 3 of the main text, June 2023. Table 1.1 outlines the development of aluminum-lithium alloy systems. The first-generation aluminum-lithium alloys primarily consisted of AA2020, VAD23, and 1420. Their primary characteristics were high strength and low plasticity, but their disadvantages included low ductility, fracture ductility, and high notch sensitivity, which can lead to stress concentration. The most notable characteristic of the second-generation aluminum-lithium alloys is their high lithium content, primarily represented by 8090, 2090, and 2091. High-lithium aluminum-lithium alloys exhibit significant thermal instability in the under-aged state, along with weaknesses such as crack segregation, strain localization, and anisotropy in mechanical properties. To address these issues, researchers in the third-generation aluminum-lithium alloys reduced the lithium content (<2%) and increased the Cu content to control the alloy's mechanical properties and thermal stability, thereby improving its hot workability. After extensive research, three major systems were finally developed: Al-Cu-Li system, Al-Li-Mg system and Al-Li-Cu-Mg-Zr system.

[0005] At present, Al-Li-Cu-Mg alloys generally adopt the third generation of low Li, high Cu approach to control their mechanical properties, thermal stability and hot working properties.

[0006] Due to its unique crystal structure and chemical composition, Al-Mg-Li alloys have poor plastic deformation capabilities at room temperature and generally require heating for deformation. However, even in the heated state, their formability remains relatively poor, prone to cracking, wrinkling, and other problems. During deformation, the structural stability of Al-Mg-Li alloys is easily affected by process parameters such as deformation temperature, deformation amount, and deformation speed. Summary of the Invention

[0007] The technical problem to be solved by the present invention is to provide an aluminum-magnesium-lithium alloy with reduced deformation and cracking, a preparation method and an application thereof, so as to improve the thermal stability and hot working performance of the alloy while ensuring that the alloy has good mechanical properties, and at the same time improve the strength and elongation.

[0008] An embodiment of the present invention provides an aluminum-magnesium-lithium alloy that reduces deformation cracking, comprising the following components in weight percentage: Cu: 0.2-0.3%, Mg: 4.5-5.6%, Li: 1.8-2.3%, refined metal: 0.08-0.15%, and the remainder is Al and unavoidable impurities, wherein the refined metal is one or more of Zr and Sc.

[0009] Preferably, the refining metal is Zr.

[0010] Preferably, the composition includes the following weight percentages: Cu: 0.22-0.28%, Mg: 4.7-5.3%, Li: 1.9-2.2%, refined metal: 0.09-0.14%, and the balance is Al and unavoidable impurities.

[0011] Preferably, it also includes one or more of Ti, Si, and Fe, and controls Ti≤0.05%, Si≤0.05%, and Fe≤0.07%.

[0012] Preferably, Ti: 0.02-0.045%, Si≤0.05%, Fe≤0.07%.

[0013] Preferably, the aluminum-magnesium-lithium alloy that reduces deformation cracking includes the following components in weight percentage: Cu: 0.22-0.28%, Mg: 4.7-5.3%, Li: 1.9-2.2%, Zr: 0.09-0.14%, Ti: 0.02%-0.045%, Si≤0.05%, Fe≤0.07%, and the balance is Al and unavoidable impurities.

[0014] The embodiment of the present invention provides a method for preparing the aluminum-magnesium-lithium alloy with reduced deformation and cracking, wherein each component alloy is smelted and cast to obtain an ingot; and then subjected to homogenization treatment and rolling to obtain.

[0015] Preferably, the homogenization treatment is to control the heating rate to be less than 60°C / h, heating to 455-465°C, keeping the temperature, and then cooling.

[0016] Preferably, the cooling method is to cool the ingot to 200° C. in the furnace, remove the ingot, and perform air cooling; after cooling, the ingot is sawn and milled to remove surface defects.

[0017] Preferably, the rolling temperature is 420-460° C., the deformation amount per pass is 10%-15%, and the total deformation amount is 40-50%.

[0018] The preparation method of the aluminum-magnesium-lithium alloy with reduced deformation cracking of the present application comprises the following specific steps: 1) Melting and casting: According to the ingredient requirements, weigh 99.95% aluminum ingots, 99.99% magnesium ingots, and aluminum-zirconium master alloys with corresponding contents and put them into the melting furnace. Before adding the materials, the melting furnace is vacuumed, preheated, and purged with argon. After adding the materials, the temperature is raised to 730±10°C for heating and melting. The melting time is 2-3 hours to obtain a lithium-free aluminum melt. The composition is adjusted in the furnace and lithium ingots and aluminum-titanium master alloys are added. The aluminum melt is degassed and refined using a rotor in the furnace. The medium is 99.99% pure argon. The refining time is 25-35 minutes. After refining, slag is skimmed. After the above steps are completed, the temperature of the aluminum melt is adjusted to 725±5°C. After standing for 20-40 minutes, casting begins. Before casting begins, the launder and online system are preheated, vacuumed, and purged with argon. After casting begins, the aluminum melt undergoes online processing, including wire feeding, degassing, and filtration. The ingot is finally semi-continuously cast to obtain an ingot.

[0019] 2) Homogenization treatment: The ingot is subjected to homogenization heat treatment in a trolley-type soaking furnace with argon gas as the atmosphere protection. The heating rate is less than 60℃ / h, and the temperature is raised to 460±5℃ for 25h. The cooling method is to cool the ingot to 200℃ with the furnace, open the furnace door and move it out of the furnace for air cooling. Machining: After the soaking ingot is cooled to below 60℃, the ingot is sawn and milled to remove surface defects. 3) Hot rolling: The homogenized and machined ingot is heated and rolled on a rolling mill at a temperature of 420-460°C. Four passes are performed, with a deformation of 10%-15% per pass and a total deformation of 60%. The rolling speed is 45 mm / s, and annealing is performed for 10 minutes between passes.

[0020] An embodiment of the present invention provides an aluminum-magnesium-lithium alloy with reduced deformation cracking, or an application of the aluminum-magnesium-lithium alloy with reduced deformation cracking obtained by the preparation method. The aluminum-magnesium-lithium alloy with reduced deformation cracking is used to prepare aerospace equipment.

[0021] The beneficial effect of the present invention is that, since Al-Mg-Li alloy shows low plasticity and poor machinability, and is prone to cracking during deformation. In order to improve the thermal cracking resistance of Al-Mg-Li alloy, the present invention optimizes the design of the alloy composition. Traditionally, the thermal cracking resistance is mainly improved by adding rare earth elements such as scandium and beryllium to Al-Mg-Li alloy, but the cost is high and it is difficult to purchase. The present invention adds a small amount of copper to Al-Mg-Li alloy (the copper content needs to be strictly controlled) so that the Cu element will segregate at the grain boundaries of the aluminum alloy. This segregation can improve the thermodynamic stability and fracture strength of the grain boundaries, enhance the bonding strength of the grain boundaries, thereby reducing the tendency to crack during rolling, and can simultaneously improve the tensile strength, yield strength and elongation. The present invention can effectively increase the application advantages of Al-Mg-Li alloy in lightweighting. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a picture of Comparative Example 1 after the first deformation.

[0023] Figure 2 This is a picture of Comparative Example 4 after the second deformation.

[0024] Figure 3 This is a picture of Example 1 after the fourth deformation. DETAILED DESCRIPTION

[0025] Example 1 A method for preparing an aluminum-magnesium-lithium alloy with reduced deformation and cracking, the specific process flow is as follows: 1) Ingredients: It is composed of the following components in percentage by weight: Cu: 0.24%, Mg: 5.0%, Li: 2.1%, Zr: 0.12%, Ti: 0.03%, Si: 0.03%, Fe: 0.05%, and the balance is Al and unavoidable impurities.

[0026] 2) Melting and casting: According to the material requirements, aluminum ingots with a corresponding content of 99.95%, magnesium ingots with a content of 99.99%, and aluminum-zirconium master alloys are weighed and put into a melting furnace. Before adding the materials, the melting furnace is evacuated, preheated, and purged with argon. After adding the materials, the temperature is raised to 730°C for heating and melting. The melting time is 2 hours to obtain a lithium-free aluminum melt. The composition is adjusted in the furnace and lithium ingots and aluminum-titanium master alloys are added. The aluminum melt is degassed and refined using a rotor in the furnace. The medium is 99.99% pure argon. The refining time is 30 minutes. After refining, slag is skimmed. After the above steps are completed, the temperature of the aluminum melt is adjusted to 725°C. After standing for 30 minutes, casting begins. Before casting begins, the launder and online system are preheated, evacuated, and purged with argon. After casting begins, the aluminum melt undergoes online processing, including wire feeding, degassing, and filtration. The ingot is finally semi-continuously cast to obtain an ingot.

[0027] 3) Homogenization treatment: The ingot is subjected to homogenization heat treatment in a trolley-type soaking furnace with argon gas as the atmosphere protection. The heating rate is 45°C / h, and the temperature is raised to 460°C for 25 hours. The cooling method is to cool the ingot to 200°C with the furnace door opened and moved out of the furnace for air cooling. Machining: After the soaking ingot is cooled to below 60°C, the ingot is sawn and milled to remove surface defects. 4) Hot Rolling: The homogenized and machined ingot was heated to 460°C and rolled on a rolling mill in four passes, with each pass deforming 10% for a total deformation of 40%. The rolling speed was 45 mm / s, and annealing was performed at 460°C for 10 minutes between passes. No cracking occurred during the four passes.

[0028] Example 2 The specific process is: 1) Ingredients: It is composed of the following components in percentage by weight: Cu: 0.28%, Mg: 5.1%, Li: 2.0%, Zr: 0.095%, Ti: 0.03%, Si: 0.03%, Fe: 0.05%, and the balance is Al and unavoidable impurities.

[0029] The remaining process steps and parameters were the same as those in Example 1. No cracking occurred during the four deformation passes.

[0030] Example 3 The specific process is: 1) The ingredients, smelting, casting and homogenization treatment are the same as those in Example 1.

[0031] 2) Hot Rolling: The homogenized and machined ingot was heated to 440°C and rolled on a rolling mill in four passes. Each pass resulted in an 8% deformation, for a total deformation of 32%. The rolling speed was 45 mm / s, and annealing was performed at 440°C for 10 minutes between passes. No cracking occurred during the four passes.

[0032] Comparative Example 1 The specific process is: 1) Ingredients: It is composed of the following components by weight percentage: Mg: 5.0%, Li: 2.1%, Zr: 0.12%, Ti: 0.03%, Si: 0.04%, Fe: 0.05%, no copper element is added, and the balance is Al and unavoidable impurities.

[0033] The remaining process steps and parameters were the same as those in Example 1. Cracking occurred in the first pass during the deformation process.

[0034] Comparative Example 2 1) Ingredients: It is composed of the following components in percentage by weight: Cu: 3%, Mg: 4.8%, Li: 2.1%, Zr: 0.12%, Ti: 0.03%, Si: 0.04%, Fe: 0.05%, and the balance is Al and unavoidable impurities.

[0035] The remaining process steps and parameters were the same as those in Example 1. Cracking occurred in the first pass during the deformation process.

[0036] Comparative Example 3 1) Ingredients: It is composed of the following components in percentage by weight: Cu: 3%, Mg: 5.0%, Li: 1.2%, Zr: 0.1%, Ti: 0.03%, Si: 0.04%, Fe: 0.05%, and the balance is Al and unavoidable impurities.

[0037] The remaining process steps and parameters were the same as those in Example 1. Cracking occurred during the second pass of the deformation process.

[0038] Comparative Example 4 1) Ingredients: It is composed of the following components in percentage by weight: Cu: 2.7%, Mg: 2.5%, Li: 2.2%, Zr: 0.09%, Ti: 0.03%, Si: 0.04%, Fe: 0.05%, and the balance is Al and unavoidable impurities.

[0039] The remaining process steps and parameters were the same as those in Example 1. Cracking occurred during the second pass of the deformation process.

[0040] Comparative Example 5 1) Ingredients: It is composed of the following components in percentage by weight: Cu: 2.7%, Mg: 0.3%, Li: 1.8%, Zr: 0.1%, Ti: 0.03%, Si: 0.04%, Fe: 0.05%, and the balance is Al and unavoidable impurities.

[0041] The remaining process steps and parameters were the same as those in Example 1. Cracking occurred during the second pass of the deformation process.

[0042] Comparative Example 6 1) Ingredients: It is composed of the following components in percentage by weight: Cu: 1.2%, Mg: 0.8%, Li: 2.2%, Zr: 0.11%, Ti: 0.03%, Si: 0.04%, Fe: 0.05%, and the balance is Al and unavoidable impurities.

[0043] The remaining process steps and parameters were the same as those in Example 1. Cracking occurred during the second pass of the deformation process.

[0044] The properties of the aluminum alloys of Examples 1-3 and Comparative Examples 1-6 were tested to obtain a performance test table as shown in Table 1.

[0045] Table 1 Performance test table

[0046] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of protection of the present application is limited to these examples. In line with the present application, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of different aspects of one or more embodiments of the present application as described above, which are not provided in detail for the sake of simplicity.

[0047] The one or more embodiments of this application are intended to encompass all such substitutions, modifications, and variations that fall within the broad scope of this application. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of one or more embodiments of this application should be included in the scope of protection of this application.

Claims

1. An aluminum-magnesium-lithium alloy with reduced deformation cracking, characterized in that: The invention comprises the following components in weight percentage: Cu: 0.2-0.3%, Mg: 4.5-5.6%, Li: 1.8-2.3%, refined metal: 0.08-0.15%, and the balance is Al and unavoidable impurities, wherein the refined metal is one or more of Zr and Sc.

2. The aluminum-magnesium-lithium alloy with reduced deformation cracking as claimed in claim 1, characterized in that: The refined metal is Zr.

3. The aluminum-magnesium-lithium alloy with reduced deformation cracking according to claim 1 or 2, characterized in that: The invention comprises the following components in weight percentage: Cu: 0.22-0.28%, Mg: 4.7-5.3%, Li: 1.9-2.2%, refined metal: 0.09-0.14%, and the balance is Al and unavoidable impurities.

4. The aluminum-magnesium-lithium alloy with reduced deformation cracking as claimed in claim 1 or 2, characterized in that: It also includes one or more of Ti, Si, and Fe, and controls Ti≤0.05%, Si≤0.05%, and Fe≤0.07%.

5. The aluminum-magnesium-lithium alloy with reduced deformation cracking as claimed in claim 4, characterized in that Ti: 0.02-0.045%, Si≤0.05%, Fe≤0.07%.

6. A method for preparing an aluminum-magnesium-lithium alloy with reduced deformation cracking as claimed in any one of claims 1 to 5, characterized in that: The component alloys are melted and cast to obtain ingots; then they are homogenized and rolled to obtain.

7. The preparation method according to claim 6, characterized in that: The homogenization treatment is to control the heating rate to be less than 60°C / h, heating to 455-465°C, keeping the temperature, and then cooling.

8. The preparation method according to claim 7, characterized in that: The cooling method is to cool the ingot to 200°C with the furnace, remove it and air cool it; after cooling, the ingot is sawn and milled to remove surface defects.

9. The preparation method according to any one of claims 6 to 8, characterized in that: The rolling temperature is 420-460℃, the deformation of each pass is 10%-15%, and the total deformation is 40-50%.

10. An application of an aluminum-magnesium-lithium alloy with reduced deformation cracking as claimed in any one of claims 1 to 5, or an aluminum-magnesium-lithium alloy with reduced deformation cracking obtained by the preparation method as claimed in any one of claims 6 to 9, characterized in that: The aluminum-magnesium-lithium alloy with reduced deformation cracking is used for preparing aerospace equipment.