Graphene / high-entropy alloy aluminum-based wear-resistant coating processing method

By synergistically strengthening aluminum-based materials with high-entropy alloys and graphene, and utilizing interface modification and FSP technology, the problem of poor bonding between ceramic particles and nano-carbon materials and the metal matrix was solved, thereby improving the material's strength and wear resistance.

CN119040882BActive Publication Date: 2026-11-20NANCHANG UNIV +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411247347.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2026-11-20
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

In existing particle-reinforced aluminum matrix composites, the poor interfacial bonding between ceramic particles and nano-carbon materials and the metal matrix results in low content of reinforcing phase, easy separation, and difficulty in improving the strength and toughness of the material.

Method used

Aluminum-based materials are synergistically reinforced with high-entropy alloys and graphene. By combining interface modification methods with FSP technology, a trace interface reaction between the high-entropy alloy and the graphene layer is promoted to form an optimized interface bond. The graphene layer is also introduced to improve the self-lubricating effect.

Benefits of technology

The increased content of the reinforcing phase enhances the strength and wear resistance of the material while maintaining the toughness of the matrix, thus avoiding problems caused by ceramic or carbon materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040882B_ABST
    Figure CN119040882B_ABST
Patent Text Reader

Abstract

A kind of processing method of graphene / high-entropy alloy aluminum-based wear-resistant coating, graphene after surface activation is added to magnesium chloride solution to form basic suspension, then mixed with high-entropy alloy powder and calcined to prepare spinel transition layer;Surface composite forming is carried out using improved FSP technology;After removing the oxide film of base material, blind holes are processed on the surface of aluminum matrix in array arrangement;High-entropy alloy is added in the blind hole, compacted, and sealed with needleless stirring head;Then, using needleless stirring head, FSP is prepared under different process parameters along the center line of blind hole;By controlling angle, heat and multiple parameters, sufficient heat input and plastic flow are ensured. Asymmetric rolling technology is used for surface strengthening, reducing bending and improving extrusion ratio. The present application has the advantages of simplicity, safety, low cost, easy operation and controllability, and the interface wetting combination is more advantageous, the material surface hardness is optimized, and the composite material can be further improved by adding the proportion of reinforcing phase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials preparation technology. Background Technology

[0002] Currently, there is relatively much research on the preparation process of particle-reinforced aluminum matrix composites both domestically and internationally. The reinforcing phases are mostly high-strength ceramic particles or carbon materials, such as SiC particles and GNPs, all of which are suitable for industrial production. These reinforcing phases not only effectively improve the overall properties of the material, such as strength and hardness, but nano-carbon materials can also further enhance surface hardness due to their good self-lubricating and heat dissipation properties. However, these materials have significant drawbacks. The bonding between ceramic particles and nano-carbon materials and the metal matrix is ​​relatively weak, resulting in poor interfacial bonding. This leads to problems such as low content in preparation and application, easy separation at the interface, difficulty in dispersion, the generation of fracture sources, and a significant decrease in the toughness of the composite material. This limits their application in the field of metal matrix reinforcement or surface modification. Although some patents show that nano-carbon materials can optimize the bonding with the matrix to a certain extent through interface modification, the interface optimization materials are usually mainly ceramic nanoparticles (CN111286634 B, CN 111363942 B, CN109590459A), resulting in relatively weak improvement in interfacial bonding with the matrix. Significantly increasing the application of graphene and reinforcing phases in aluminum-based materials remains a challenge. High-entropy alloys have attracted considerable attention due to their high hardness, high strength, corrosion resistance, and high-temperature thermal stability. Furthermore, due to their inherent metal-metal interfacial bonding characteristics, high-entropy alloys exhibit good interfacial wettability and compatibility with magnesium / aluminum alloy matrices. If high-entropy alloys could be used in conjunction with traditional nano-carbon as a reinforcing phase to strengthen aluminum alloys, and if the interface between graphene and high-entropy alloys could be strengthened and this hybrid reinforcing phase applied to the surface of aluminum-based composite materials, the bottleneck of traditional ceramic reinforcing phases in strengthening and toughening could be overcome. This would allow for an increase in the reinforcing phase content while further improving material strength and wear resistance. However, to date, no similar literature has been reported. Summary of the Invention

[0003] The purpose of this invention is to provide a method for processing a graphene / high-entropy alloy aluminum-based wear-resistant coating. This method utilizes a high-entropy alloy with a small amount of graphene to prepare the aluminum alloy wear-resistant coating. This invention employs an interface modification method combined with FSP (friction stir processing) technology to promote a micro-interfacial reaction between the high-entropy alloy and the graphene layer, ultimately optimizing the interface with the aluminum substrate. This increases bonding while introducing the graphene layer to enhance self-lubrication. Furthermore, due to its metallic properties, the reinforced coating prepared by this method does not reduce the toughness of the substrate, avoiding some of the problems caused by ceramic or carbon materials.

[0004] This invention is achieved through the following technical solution.

[0005] The present invention discloses a method for processing a graphene / high-entropy alloy aluminum-based wear-resistant coating, comprising the following steps.

[0006] (1) Graphene purification: 95-99% graphene is immersed in 60-80% nitric acid alcohol at room temperature for 1-3 hours to remove impurities, followed by dilution, centrifugation and drying.

[0007] (2) Add the graphene obtained in step (1) to a magnesium chloride solution with a concentration of 15~25wt.% and sonicate for 10~15min with an ultrasonic power ≥150W, wherein the molar ratio of graphene to magnesium chloride is 0.3~0.8:1.

[0008] (3) Place the TRIS buffer into the solution obtained in step (2) to adjust its pH value to 8-9, and continue sonication for about 3-6 hours to obtain a graphene suspension.

[0009] (4) The resulting graphene suspension was then introduced into a spherical volumetric flask and immersed in an oil bath for 1-2 hours until it reached a viscous consistency. The volumetric flask was stoppered with a syringe inserted at the top, and the temperature was controlled at 70-90°C.

[0010] (5) Place 75~85 vol.% of micron-sized (5~15μm) high-entropy alloy powder in a viscous liquid, mix and sonicate for 10~30 min, and then let it stand to deposit for 3~7 h.

[0011] (6) After drying the high-entropy alloy graphene powder obtained in step (4), vacuum calcinate it at a temperature of 430~550℃ for a time of 40~120min.

[0012] (7) The mixed powder obtained in step (5) is ball-milled at a low speed of 100~130 rad for 4~7 h to reduce cold welding.

[0013] (8) Use 800~1200# sandpaper to polish the surface of the aluminum plate in batches to remove the oxide film. Use drilling equipment to process blind holes with a top diameter of 3~6mm, a bottom conical shape and a depth of 3~5mm on the aluminum alloy surface. The blind holes are arranged in an array with a longitudinal and transverse spacing of 4~6mm. After cleaning the surface with 0.4Vol.%HF alcohol solution, add the pre-treated high-entropy alloy into the blind holes and continuously compact it. Then use a needleless stirring head to seal the holes.

[0014] (9) After sealing, FSP tests were conducted under different process parameters along the centerline of the blind hole using a needleless stirring head. The diameter of the stirring head was φ10 mm to φ20 mm, the rotation speed was 600-1000 rpm, and the moving speed was 20-60 mm / min. The stirring head was perpendicular to the plate or inclined at 0-7° to the feed speed direction, and the shoulder shaft was pressed down by 1.5-2 mm. During the preparation of composite materials by FSP, sufficient heat input is required to ensure that the matrix material can undergo plastic flow, thereby avoiding processing defects; at the same time, it is necessary to ensure that no serious interfacial reaction occurs between the reinforcing phase and the matrix.

[0015] (10) Surface strengthening is achieved by using asymmetric rolling technology, wherein the rolling speed of the upper horizontal shaft is controlled at 12-25 rpm, and the downward pressure is 1 / 3 to 1 / 2 of the tapered hole. The lower horizontal shaft is controlled at a non-uniform speed, which is 5-7 rpm slower than the upper horizontal shaft.

[0016] The reaction equation of this invention is as follows (introduced by AlCoCrFeNi high-entropy alloy powder).

[0017] Eq: MgCl2+@GNPs =Mg + @GNPs+2Cl - (1) Al2O3(s)+ MgO(s)=MgO·Al2O3 (2) Al2O3+Fe=N(Fe, Al)2O4 (3) 4Al + 3C = Al4C3 (4).

[0018] The technical effects of this invention are as follows: (1) Magnesium ions adsorbed on the surface of graphene form a precipitate in a weakly alkaline environment and are further calcined to generate magnesium oxide, which then reacts with aluminum in the high-entropy alloy to form a reaction transition layer and further promotes the reaction in the subsequent FSP. Compared with traditional chemical plating, the interfacial adhesion is more advantageous, ensuring that graphene can be better bonded to the high-entropy alloy or the matrix. (2) The formation of carbon-aluminum compounds between graphene and aluminum at the interface further optimizes the bonding, thereby improving the bonding of carbon materials once again. (3) Compared with the direct use of graphene, high-entropy alloy powder is introduced. The nano-carbon material has good self-lubrication and heat dissipation properties, which further optimizes the surface hardness of the material and reduces the problem of increased adhesive wear caused by the increase in heat. At the same time, the metallic properties of the high-entropy alloy further increase the proportion of reinforcing phase that can be added to the composite material. Therefore, the novel graphene / high-entropy alloy aluminum-based material has a wider range of applications. Attached Figure Description

[0019] Figure 1 The image shows the SEM microstructure of the ball-milled alloy powder and graphene.

[0020] Figure 2 TEM image of the composite microstructure in 2014 aluminum alloy.

[0021] Figure 3 These are high-entropy particles in composite materials. Detailed Implementation

[0022] For ease of understanding, the present invention will be described in detail below with reference to specific embodiments. Example 1

[0023] A method for processing a graphene / high-entropy alloy aluminum-based wear-resistant coating includes the following steps.

[0024] (1) Graphene purification: 99% graphene was immersed in 70% nitric acid alcohol at room temperature for 2 hours to remove impurities, followed by conventional dilution, centrifugation and drying.

[0025] (2) Add the graphene obtained in step (1) to a magnesium chloride solution with a concentration of 20 wt.% and sonicate for 15 min with an ultrasonic power of 150 W. The molar ratio of graphene to magnesium chloride is 0.3:1.

[0026] (3) Place the TRIS buffer into the solution obtained in step (2) to adjust its pH value to 8.5, and continue sonication for about 5 hours to obtain a graphene suspension.

[0027] (4) The resulting graphene suspension was then introduced into a spherical volumetric flask and immersed in an oil bath for 2 hours until it became viscous. The volumetric flask was stopped with a cork and a syringe was inserted into the top. The temperature was controlled at 90°C.

[0028] (5) The graphene viscous liquid obtained in step (4) is mixed with 80 vol.% of micron-sized (5~20μm) gas-atomized CoNiFeAlCr high-entropy alloy powder and ultrasonicated for 20 min, and then allowed to stand for 5 h for deposition.

[0029] (6) After drying the high-entropy alloy mixed powder obtained in step (5), vacuum calcinate it at a temperature of 500℃ for 100 min.

[0030] (7) The mixed powder obtained in step (6) is ball-milled at a low speed of 120 rad for 5 hours to reduce cold welding.

[0031] (8) Use 800, 900, 100, and 1200# sandpaper to polish the surface of the 2014 aluminum plate four times to remove the oxide film. Use a drilling machine to process blind holes with a diameter of 2 mm and a depth of 5 mm on the aluminum alloy surface. The blind holes are arranged in an array with a longitudinal and transverse spacing of 5 mm. After applying 0.4 Vol.% HF alcohol solution to the surface, add the pre-treated high-entropy alloy into the blind holes, with the ratio controlled at 5 Wt.% to the substrate, and continuously compact it. Then, use a needleless stirring head to seal the holes.

[0032] (9) After the hole sealing treatment, FSP test was carried out under different process parameters along the center line of the blind hole using a needle stirring head. The diameter of the stirring head was φ15 mm, the rotation speed was 600 rpm, and the moving speed was 40 mm / min. The stirring head was perpendicular to the plate and the shoulder shaft was pressed down by 1.8 mm.

[0033] (10) Surface strengthening is achieved using asymmetric rolling technology, where the upper horizontal axis rolling speed is controlled at 25 rpm, and the lower pressure is 1 / 3 of the tapered hole. The lower horizontal axis rotation speed is 20 rpm. Compared to the substrate, the hardness is increased by approximately 64.7%. Compared to graphene of the same volume (6~6.5 Vol.%), the hardness is increased by 36.4%. Example 2

[0034] A method for processing a graphene / high-entropy alloy aluminum-based wear-resistant coating includes the following steps.

[0035] (1) Graphene purification: 95% graphene was immersed in 60% nitric acid alcohol at room temperature for 3 hours to remove impurities, followed by conventional dilution, centrifugation and drying.

[0036] (2) Add the graphene obtained in step (1) to a magnesium chloride solution with a concentration of 25 wt.% and sonicate for 10 min with an ultrasonic power of 200 W. The molar ratio of graphene to magnesium chloride is 0.8:1.

[0037] (3) Place the TRIS buffer into the solution obtained in step (2) to adjust its pH value to 8, and continue sonication for about 4 hours to obtain a graphene suspension.

[0038] (4) The resulting graphene suspension was then introduced into a spherical volumetric flask and immersed in an oil bath for 1 hour until it became viscous. The volumetric flask was stopped with a cork and a syringe was inserted into the top. The temperature was controlled at 90°C.

[0039] (5) The graphene powder obtained in step (4) is mixed with 85 vol.% of micron-sized (5~20μm) gas-atomized CoNiFeAlCr high-entropy alloy powder and ultrasonicated for 25 min, and then allowed to stand for deposition for 4 h.

[0040] (6) After drying the high-entropy alloy mixed powder obtained in step (5), vacuum calcination is carried out at a temperature of 550℃ for a time of 40min.

[0041] (7) The mixed powder obtained in step (6) is ball-milled at a low speed of 110 rad for 7 hours to reduce cold welding.

[0042] (8) The surface of the 2014 aluminum plate was polished in four batches using 800, 900, 100, and 1200# sandpaper to remove the oxide film. Blind holes with a diameter of 2.5 mm and a depth of 4.5 mm were machined on the aluminum alloy surface using a drilling machine. The blind holes were arranged in an array with a longitudinal and transverse spacing of 4.5 mm. After applying 0.4 Vol.% HF alcohol solution to the surface, the pre-treated high-entropy alloy was added into the blind holes, with a ratio of 7 Wt.% to the substrate, and continuously compacted. Then, the holes were sealed using a needleless stirring head.

[0043] (8) After the hole sealing treatment, FSP tests were conducted under different process parameters along the center line of the blind hole using a needleless stirring head. The diameter of the stirring head was φ15 mm, the rotation speed was 600 rpm, and the moving speed was 25 mm / min. The stirring head was tilted 5° to the plate and the shoulder shaft was pressed down 1.5 mm.

[0044] (9) Surface strengthening is achieved using asymmetric rolling technology, where the upper horizontal axis rolling speed is controlled at 25 rpm, and the lower pressure is 1 / 3 of the tapered hole. The lower horizontal axis rotation speed is 22 rpm. This yields the desired wear-resistant graphene / high-entropy alloy composite reinforced aluminum matrix composite material. Compared to the matrix, the hardness is increased by approximately 69.2%. Compared to graphene of the same volume (7~7.5 Vol.%), the hardness is increased by 32.6%. Example 3

[0045] A method for processing a graphene / high-entropy alloy aluminum-based wear-resistant coating includes the following steps.

[0046] (1) Graphene purification: 99% graphene was immersed in 80% nitric acid alcohol at room temperature for 1-3 hours to remove impurities, followed by dilution, centrifugation and drying.

[0047] (2) Add the graphene obtained in step (1) to a magnesium chloride solution with a concentration of 15 wt.% and sonicate for 15 min. The sonic power is 180 W. The molar ratio of graphene to magnesium chloride is 0.5:1.

[0048] (3) Place the TRIS buffer into the solution obtained in step (2) to adjust its pH value to 9, and continue sonication for about 3 hours to obtain a graphene suspension.

[0049] (4) The resulting graphene suspension was then introduced into a spherical volumetric flask and immersed in an oil bath for 2 hours until it became viscous. The volumetric flask was stopped with a cork and a syringe was inserted into the top. The temperature was controlled at 90°C.

[0050] (5) Place 75 vol.% of micron-sized (5~15 μm) high-entropy alloy powder in a viscous liquid, mix and sonicate for 30 min, and then let it stand to deposit for 7 h.

[0051] (6) The high-entropy alloy graphene powder obtained in step (4) is dried and then vacuum calcined at a temperature of 520°C for 60 minutes.

[0052] (7) The mixed powder obtained in step (5) is ball-milled at a low speed of 120 rad for 4 to 7 hours to reduce cold welding.

[0053] (8) Use 800~1200# sandpaper to polish the surface of the aluminum plate in batches to remove the oxide film. Use drilling equipment to process blind holes with a top diameter of 3~6mm, a bottom conical shape and a depth of 3~5mm on the aluminum alloy surface. The blind holes are arranged in an array with a longitudinal and transverse spacing of 4mm. After cleaning the surface with 0.4Vol.%HF alcohol solution, add the pre-treated high-entropy alloy into the blind holes and continuously compact it. Then use a needleless stirring head to seal the holes.

[0054] (9) After the hole sealing treatment, FSP tests were conducted under different process parameters using a needleless stirring head along the center line of the blind hole. The diameter of the stirring head was φ20 mm, the rotation speed was 800 rpm, and the moving speed was 30 mm / min. The stirring head was perpendicular to the plate or tilted 3° to the feed speed direction, and the shoulder shaft was pressed down 2 mm.

[0055] (10) Surface strengthening is achieved by asymmetric rolling technology, wherein the rolling speed of the upper horizontal shaft is controlled at 25 rpm, and the downward pressure is 1 / 3 of that of the tapered hole. The lower horizontal shaft is controlled by non-uniform speed, which is 18 rpm less than the speed of the upper horizontal shaft.

Claims

1. A method for processing a graphene / high-entropy alloy aluminum-based wear-resistant coating, characterized in that: Includes the following steps: (1) Immerse 95-99% graphene in 60-80% nitric acid alcohol at room temperature for 1-3 hours to remove impurities, then dilute, centrifuge and dry. (2) Add the graphene obtained in step (1) to a magnesium chloride solution with a concentration of 15~25wt.% and sonicate for 10~15min with an ultrasonic power ≥150W, wherein the molar ratio of graphene to magnesium chloride is 0.3~0.8:1; (3) Add TRIS buffer to the mixed solution obtained in step (2) to adjust its pH value to 8-9, and continue sonication for 3-6 hours to obtain graphene suspension; (4) The obtained graphene suspension is introduced into a spherical volumetric flask and immersed in an oil bath and heated for 1-2 hours until it becomes viscous; the volumetric flask is stopped with a cork and a syringe is inserted at the top, and the temperature is controlled at 70-90℃. (5) Place 75-85 vol.% of 5-15 μm CoNiFeAlCr high-entropy alloy powder in a viscous liquid, mix and sonicate for 10-30 min, and then let it stand to deposit for 3-7 h; (6) The high-entropy alloy graphene powder obtained in step (4) is dried and then vacuum calcined at a temperature of 430~550℃ for a time of 40~120min. (7) The mixed powder obtained in step (5) is ball-milled at a low speed of 100~130 rad for 4~7 h. (8) Use 800~1200# sandpaper to polish the surface of the aluminum plate in batches to remove the oxide film; use drilling equipment to process blind holes with a top diameter of 3~6mm, a bottom cone shape and a depth of 3~5mm on the surface of the aluminum alloy. The horizontal and vertical spacing of the blind holes on the surface is 4~6mm and they are arranged in an array; after cleaning the surface with 0.4Vol.%HF alcohol solution, add the treated high entropy alloy into the blind holes and continuously compact it. Then use a needleless stirring head to seal the holes. (9) After the hole sealing treatment, the FSP test under different process parameters was carried out along the center line of the blind hole using a needleless stirring head; the diameter of the stirring head was φ10 mm~ф20 mm, the rotation speed was 600-1000 rpm, the moving speed was 20-60 mm / min, and the stirring head was perpendicular to the plate or inclined at 0~7° to the feed speed direction, and the shoulder shaft was pressed down by 1.5~2 mm; (10) Surface strengthening is carried out by asymmetric rolling technology, wherein the rolling speed of the upper horizontal shaft is controlled at 12-25 rpm and the downward pressure is 1 / 3 to 1 / 2 of the tapered hole; the lower horizontal shaft is controlled by non-uniform speed, which is 5-7 rpm less than the speed of the upper horizontal shaft.

Citation Information

Patent Citations

  • Method for laser cladding of wear-resistant coating on graphene reinforced Co-Cr-Fe-Ni-W high-entropy alloy

    CN117286485A

  • Metal matrix carbon nanocomposite manufacturing method

    KR1020140050807A