A ternary eutectic solid-state electrolyte, a preparation method thereof and a solid-state lithium battery

By mixing ternary eutectic solvent with polymer solution, a low-cost, high-performance ternary eutectic solid electrolyte is prepared, solving the problems of high cost and low ionic conductivity of composite electrolytes, and achieving high safety and high energy density of lithium batteries.

CN119050455BActive Publication Date: 2026-11-24CHINA UNIV OF PETROLEUM (BEIJING)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411150292.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2026-11-24
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Existing composite solid electrolytes suffer from problems such as high cost, complex preparation process and low ionic conductivity, making it difficult to meet the requirements of lithium-ion batteries in terms of high safety, high energy density and low cost.

Method used

A ternary eutectic solid electrolyte was prepared by mixing a ternary eutectic solvent with a polymer solution, adjusting the interface smoothness through hydrogen bonds in the deep eutectic solvent, and combining it with fluoroethylene carbonate to improve ionic conductivity and thermal stability. This simplified the preparation process and reduced costs.

Benefits of technology

The prepared ternary eutectic solid electrolyte has low cost, good flexibility, thermal stability, high ionic conductivity and high safety, and exhibits excellent cycle stability and safety, making it suitable for lithium batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention discloses a ternary eutectic solid electrolyte, its preparation method, and a solid-state lithium battery. The preparation method of the ternary eutectic solid electrolyte of this invention includes the following steps: S1, mixing a lithium-ion-containing hydrogen bond acceptor and a hydrogen bond donor to obtain a deep eutectic solvent; S2, mixing the deep eutectic solvent with a modifier to obtain a ternary eutectic solvent; the modifier includes one or more of ethylene carbonate, vinylene carbonate, and fluoroethylene carbonate; S3, dissolving a polymer in an organic solvent to obtain a polymer solution; S4, mixing the ternary eutectic solvent and the polymer solution uniformly to obtain a ternary eutectic polymer solution; S5, drying and molding the ternary eutectic polymer solution to obtain the ternary eutectic solid electrolyte. The ternary eutectic solid electrolyte of this invention exhibits excellent ionic conductivity, strong mechanical properties, flame retardancy, stable interfacial properties, and superior safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a ternary eutectic solid electrolyte, its preparation method, and a solid-state lithium battery, belonging to the field of solid-state battery solid electrolyte preparation technology. Background Technology

[0002] Lithium-ion batteries, as a highly sought-after energy storage device, are currently widely used in various electronic products, electric vehicles, energy storage systems, and other special-purpose equipment. In the coming decades, global demand for lithium-ion batteries will undoubtedly continue to grow, especially in the electric vehicle sector and various electronic products. Simultaneously, with industrial development and increasing societal demands, higher requirements are being placed on lithium-ion batteries, such as long lifespan, high charge / discharge speed, high safety, high environmental friendliness, high energy density, and low cost. However, current lithium-ion battery systems face several problems, including high safety risks and low energy density, and cannot meet these requirements. Therefore, there is an urgent need to develop new types of lithium batteries.

[0003] Commercial all-solid-state lithium batteries have attracted much attention due to their high energy density and safety. Utilizing solid-state electrolytes can improve battery energy density and enhance safety by avoiding the use of organic electrolytes. Currently, solid-state electrolytes are mainly classified into three categories: polymer solid-state electrolytes, inorganic solid-state electrolytes, and composite solid-state electrolytes. However, inorganic solid-state electrolytes exhibit poor compatibility with the electrode interface. Polymer solid-state electrolytes are more flexible and can reduce interfacial impedance. The most promising research area currently is composite solid-state electrolytes, which can maximize the advantages of different electrolyte combinations. The matrix of composite solid-state electrolytes is mainly composed of polymers. Polymers such as polyethylene oxide (PEO), polyethylene glycol diacrylate (PEGDA), polyacrylonitrile (PAN), polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), and polymethyl methacrylate (PMMA) have been studied. Improving the ionic conductivity of composite solid-state electrolytes through modification with inorganic fillers and plasticizers has been a key research focus. For example, adding two-dimensional hydroxyapatite (HAP) nanomaterials and N-methylpyrrolidone (NMP) to a PVDF-HFP polymer matrix can improve the ionic conductivity of solid electrolytes. Succinate (SCN) can be used to create new ion transport pathways, enhance the mechanical properties of the electrolyte, and prevent the formation of lithium dendrites. The addition of the plasticizer succinate (SN) reduces the crystallinity of PEO, resulting in an ionic conductivity of 2.57 × 10⁻⁶ at 30°C. -4S cm⁻¹, with a lithium-ion transfer number of 0.6. PEO also helps reduce crystallinity. It is evident that modification can further improve the performance of the composite electrolyte. However, composite electrolytes still suffer from numerous problems, such as high cost, complex preparation processes, and low ionic conductivity. To address these issues, this invention modifies the polymer solid electrolyte using a modifier, aiming to further reduce production costs, simplify the preparation method, and improve ionic conductivity, flame retardancy, thermal stability, and safety. Summary of the Invention

[0004] The purpose of this invention is to provide a ternary eutectic solid electrolyte, its preparation method, and a solid lithium battery. The preparation method of this solid electrolyte is simple and low in cost, and the prepared solid electrolyte has good flexibility, thermal stability, self-extinguishing property, high ionic conductivity, an electrochemical window of 4.6V, long cycle stability at high rates, and high safety.

[0005] To achieve the above objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides a method for preparing a ternary eutectic solid electrolyte, comprising the following steps: S1. Mix the hydrogen bond acceptor and hydrogen bond donor containing lithium ions to obtain a deep eutectic solvent; S2. Mix the deep eutectic solvent and the modifier to obtain a ternary eutectic solvent; The modifier includes one or more of ethylene carbonate (EC), vinylene carbonate (VC), and fluoroethylene carbonate (FEC). S3. Dissolve the polymer in an organic solvent to obtain a polymer solution; The polymer includes one or more of poly(vinylidene fluoride-co-hexafluoropropylene), polyethylene oxide, polyethylene glycol diacrylate, polyacrylonitrile, polyvinylidene fluoride, and polymethyl methacrylate. S4. Mix the ternary eutectic solvent and the polymer solution evenly to obtain a ternary eutectic polymer solution; S5. The ternary eutectic polymer solution is dried and shaped to obtain the ternary eutectic solid electrolyte.

[0006] Based on the above technical solution, this invention first mixes a deep eutectic solvent with modifiers such as fluoroethylene carbonate to obtain a ternary eutectic solvent; then, the ternary eutectic solvent is mixed with a solution of polymers such as poly(vinylidene fluoride-co-hexafluoropropylene), and dried to obtain a solid electrolyte. On the one hand, by binding the ternary eutectic solvent into the three-dimensional network of the polymer, the large number of hydrogen bonds present in the DESs of the ternary eutectic solvent can adjust the smoothness of the interface, thereby reducing the interfacial impedance of the solid-solid interface; on the other hand, the deep eutectic solvent can interact with fluoroethylene carbonate, which can improve ionic conductivity and thermal stability, and promote the uniform deposition of metallic lithium and the stable formation of the SEI layer in the solid state.

[0007] In the above-mentioned method for preparing ternary eutectic solid electrolyte, the lithium-ion-containing hydrogen bond acceptor includes any one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium dioxalate borate, lithium difluorooxalate borate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium nitrate, lithium chloride, and lithium difluorophosphate. The hydrogen bond donor is any one of N-methylacetamide, acetamide, butyramide, propionamide, N,N-dimethylpropenylurea, methyl pyruvate dimethyl sulfone, ethylene carbonate, succinate, and 2,2'-dithiopyridine. The molar ratio of the lithium-ion-containing hydrogen bond acceptor to the hydrogen bond donor is 1:(2-6), including but not limited to 1:(3-4), 1:4 or 1:3.

[0008] As an example, the lithium-ion-containing hydrogen bond acceptor is lithium bis(trifluoromethanesulfonyl)imide, and the hydrogen bond donor is N-methylacetamide or succinate. The molar ratio of lithium bis(trifluoromethanesulfonyl)imide to N-methylacetamide is preferably 1:4, and the molar ratio of lithium bis(trifluoromethanesulfonyl)imide to succinate is 1:4 or 1:3. The purity of the lithium bis(trifluoromethanesulfonyl)imide is ≥99.99%.

[0009] In the above-described method for preparing ternary eutectic solid electrolyte, the volume ratio of the deep eutectic solvent to the modifier is (3-6):1, including but not limited to 4:1. As an example, the modifier is fluoroethylene carbonate, and the volume ratio of the deep eutectic solvent to the fluoroethylene carbonate is 4:1.

[0010] In the above-mentioned method for preparing ternary eutectic solid electrolyte, the number average molecular weight of the polymer is 100,000 to 1,000,000, including but not limited to 130,000 and 149,000 to 151,000; as an example, the polymer is poly(vinylidene fluoride-co-hexafluoropropylene); or, the polymer is poly(vinylidene fluoride-co-hexafluoropropylene) and polyacrylonitrile in a mass ratio of 10:1 or 5:1.

[0011] The organic solvent can be any good solvent for the polymer, including but not limited to N,N-dimethylformamide; The mass ratio of the polymer to the organic solvent is 1:(4-6), including but not limited to 1:6 or 1:5; as an example, the mass ratio of the poly(vinylidene fluoride-co-hexafluoropropylene) to the N,N-dimethylformamide is 1:6; or, the total amount of the poly(vinylidene fluoride-co-hexafluoropropylene) and the polyacrylonitrile to the N,N-dimethylformamide is 1:5; In the above-mentioned method for preparing ternary eutectic solid electrolyte, the mass ratio of the ternary eutectic solvent to the polymer solution is 1:(2-5), such as mixing 3.5g of the polymer solution with 0.8mL of the ternary eutectic solvent.

[0012] In the above-described method for preparing the ternary eutectic solid electrolyte, the method further includes the following step before drying and molding: ultrasonically treating the ternary eutectic polymer solution to remove air bubbles from the solution. As an example, the ultrasonic treatment is performed in an ultrasonic oscillator for 0.5 hours.

[0013] In the above-described method for preparing ternary eutectic solid electrolyte, the drying and molding step is further described as follows: the ternary eutectic polymer solution is poured into a mold for drying; specifically, the ternary eutectic solid electrolyte is dropped onto polytetrafluoroethylene molds with circular grooves of different depths, and the thickness of the solid electrolyte is controlled by controlling the amount of dropping; through the above treatment, a large number of bubbles can be avoided in the dried electrolyte; preferably, the drying treatment is to first dry at 40-60 degrees Celsius (e.g., 50 degrees Celsius) for 2-5 hours, and then vacuum dry at 60-80 degrees Celsius (e.g., 70 degrees Celsius) for 4-6 hours. Specifically, the slow evaporation of the organic solvent at 40-60 degrees Celsius first avoids excessively rapid solvent evaporation, which could lead to bubble formation and large-area shrinkage of the electrolyte. Vacuum drying at 60-80 degrees Celsius further ensures complete solvent evaporation, preventing the organic solvent from reacting with the electrode.

[0014] Secondly, the present invention provides a ternary eutectic solid electrolyte obtained by any of the preparation methods described above. When storing the ternary eutectic solid electrolyte of the present invention, the dried solid electrolyte is transferred while still hot to an anhydrous and oxygen-free glove box. Then, the membrane is peeled off using rubber tweezers, and the resulting ternary eutectic solid electrolyte is sealed and stored in the glove box. During operation, the membrane should be peeled off slowly from the rounded edge towards the center to avoid curling of the electrolyte.

[0015] Thirdly, the present invention provides a solid-state lithium battery, comprising a positive electrode, a negative electrode, and the aforementioned ternary eutectic solid electrolyte.

[0016] Specifically, the cathode can be one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, or ternary cathode materials (such as nickel cobalt manganese NCM ternary cathode material or nickel cobalt aluminum NCA ternary cathode material).

[0017] Specifically, the negative electrode can be one of lithium metal, graphite, lithium titanate, or silicon. The graphite can be pre-lithiated graphite.

[0018] As an example, the solid-state lithium battery is a coin cell or a pouch cell. In this invention, the pouch cell prepared from the ternary eutectic solid electrolyte exhibits excellent cycle performance and high safety.

[0019] The present invention has the following beneficial effects: 1) The preparation method of the ternary eutectic solid electrolyte of the present invention is simple and the preparation cost is low.

[0020] 2) The ternary eutectic solid electrolyte of the present invention has excellent ionic conductivity, strong mechanical properties, flame retardancy, stable interfacial properties and excellent safety.

[0021] 3) In the ternary eutectic solid electrolyte of the present invention, the deep eutectic solvent and fluoroethylene carbonate work synergistically to improve ionic conductivity and thermal stability, and promote uniform deposition of metallic lithium.

[0022] 4) In the deep eutectic solvent of the ternary eutectic solid electrolyte of the present invention, N-methylacetamide selectively occupies the lithium dissolution sheath, triggering a concentration gradient, thereby promoting the decomposition of fluoroethylene carbonate and promoting the formation of the inorganic solid electrolyte interphase layer, thereby improving long-cycle performance.

[0023] 5) The present invention can prepare solid electrolytes with normal voltage and high voltage solid electrolytes by mixing poly(vinylidene fluoride-co-hexafluoropropylene) with polyacrylonitrile polymer and obtaining a deep eutectic solvent with succinic acid and lithium bis(trifluoromethanesulfonyl)imide.

[0024] 6) The Li / / P-0.8-FEC / / LFP button cell assembled with the ternary eutectic solid electrolyte of the present invention exhibits excellent stability in multiple charge-discharge cycles, and can stably cycle 500 times under 1C conditions.

[0025] 7) The ternary eutectic solid electrolyte of the present invention is used to assemble a pouch cell with a eutectic solid electrolyte, which exhibits stable cycle performance under 1C conditions.

[0026] 8) The pouch battery assembled with the ternary eutectic solid electrolyte of the present invention has undergone rigorous safety testing, proving its excellent safety and stability. Attached Figure Description

[0027] Figure 1 This is a process flow diagram for preparing a ternary eutectic solid electrolyte in one embodiment of the present invention; Figure 2 The image shows the flame retardancy test data of the ternary eutectic solid electrolyte prepared in Example 1 of this invention. Figure 3 This is a graph showing the thermal stability test data of the ternary eutectic solid electrolyte prepared in Example 2 of the present invention; Figure 4 The image shows the long-cycle performance of a Li / / P-0.8-FEC / / LFP coin cell assembled with the ternary eutectic solid electrolyte prepared in Example 3 of this invention. Figure 5 The cycling performance diagram shows the Gr / / P-0.8-FEC / / LFP pouch cell assembled with the ternary eutectic solid electrolyte prepared in Example 5 of this invention. Figure 6 Safety performance test diagram of Gr / / P-0.8-FEC / / LFP pouch cell assembled with the ternary eutectic solid electrolyte prepared in Example 5. Detailed Implementation

[0028] The present invention will now be described in further detail with reference to specific embodiments. The given embodiments are merely illustrative of the invention and not intended to limit its scope. The embodiments provided below can serve as a guide for further improvements by those skilled in the art and do not constitute a limitation on the invention in any way.

[0029] Unless otherwise specified, the methods used in the following embodiments are conventional methods, performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Unless otherwise specified, the materials and reagents used in the following embodiments are commercially available.

[0030] The purity of LiTFSI in the following examples is ≥99.99%.

[0031] The purity of N,N-dimethylformamide in the following examples is ≥99.9%.

[0032] Example 1: Preparation of ternary eutectic solid electrolyte according to Figure 1 The process flow diagram shown illustrates the preparation of a ternary eutectic solid electrolyte. The specific steps are as follows: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetamide were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain deep eutectic solvent, which was then stored in the glove box.

[0033] (2) Preparation of ternary eutectic solvent: Mix 0.8 ml of the deep eutectic solvent obtained in step (1) with 0.2 ml of fluoroethylene carbonate and stir at room temperature for 1 h to obtain the ternary eutectic solvent.

[0034] (3) Preparation of solid electrolyte base solution: 0.523g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 was completely dissolved in 3.021g of organic solvent N,N-dimethylformamide to obtain solid electrolyte base solution.

[0035] (4) Preparation of ternary eutectic polymer solution: Mix all the solid electrolyte substrate solution obtained in step (3) with 0.8 ml of ternary eutectic solvent obtained in step (2) and stir evenly for 1 h to obtain ternary eutectic polymer solution.

[0036] (5) Solution casting: Transfer the solid electrolyte base solution obtained in step (4) to an ultrasonic oscillator and sonicate for 0.5 h to make a large number of bubbles in the solution disappear. Then, use a pipette to slowly draw up the solution, try to avoid the generation of bubbles, and cast it evenly and in appropriate amount into the polytetrafluoroethylene mold.

[0037] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold is transferred to a 50°C drying oven and dried for 6 hours. Then it is transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.647 mm thick solid electrolyte membrane.

[0038] (7) Storage of solid electrolyte: While the dried solid electrolyte is still hot, transfer it to an anhydrous and oxygen-free glove box, and then use rubber tweezers to peel off the membrane and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0039] Example 2: Preparation of ternary eutectic solid electrolyte according to Figure 1 The process flow diagram shown illustrates the preparation of a ternary eutectic solid electrolyte. The specific steps are as follows: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetamide were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain deep eutectic solvent, which was then stored in the glove box.

[0040] (2) Preparation of ternary eutectic solvent: Mix 0.8 ml of the deep eutectic solvent obtained in step (1) with 0.2 ml of fluoroethylene carbonate to obtain ternary eutectic solvent.

[0041] (3) Preparation of solid electrolyte base solution: 0.511g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 was completely dissolved in 3.014g of organic solvent N,N-dimethylformamide to obtain solid electrolyte base solution.

[0042] (4) Preparation of ternary eutectic polymer solution: Mix all the solid electrolyte substrate solution obtained in step (3) with 0.8 ml of ternary eutectic solvent obtained in step (2) and stir evenly for 1 h to obtain ternary eutectic polymer solution.

[0043] (5) Solution casting: Transfer the solid electrolyte base solution obtained in step (4) to an ultrasonic oscillator and sonicate for 0.5 h to make a large number of bubbles in the solution disappear. Then, use a pipette to slowly draw up the solution, try to avoid the generation of bubbles, and cast it evenly and in appropriate amount into the polytetrafluoroethylene mold.

[0044] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold is transferred to a 50°C drying oven and dried for 6 hours. Then it is transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.747 mm thick solid electrolyte membrane.

[0045] (7) Storage of solid electrolyte: While the dried solid electrolyte is still hot, transfer it to an anhydrous and oxygen-free glove box, and then use rubber tweezers to peel off the membrane and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0046] Example 3: Preparation of ternary eutectic solid electrolyte according to Figure 1 The process flow diagram shown illustrates the preparation of a ternary eutectic solid electrolyte. The specific steps are as follows: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetamide were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain deep eutectic solvent, which was then stored in the glove box.

[0047] (2) Preparation of ternary eutectic solvent: Mix 0.8 ml of the deep eutectic solvent obtained in step (1) with 0.2 ml of fluoroethylene carbonate to obtain ternary eutectic solvent.

[0048] (3) Preparation of solid electrolyte base solution: 0.506g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 was completely dissolved in 3.021g of organic solvent N,N-dimethylformamide to obtain solid electrolyte base solution.

[0049] (4) Preparation of ternary eutectic polymer solution: Mix all the solid electrolyte substrate solution obtained in step (3) with 0.8 ml of ternary eutectic solvent obtained in step (2) and stir evenly for 1 h to obtain ternary eutectic polymer solution.

[0050] (5) Solution casting: Transfer the solid electrolyte base solution obtained in step (4) to an ultrasonic oscillator and sonicate for 0.5 h to make a large number of bubbles in the solution disappear. Then, use a pipette to slowly draw up the solution, try to avoid the generation of bubbles, and cast it evenly and in appropriate amount into the polytetrafluoroethylene mold.

[0051] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold is transferred to a 50°C drying oven and dried for 6 hours. Then it is transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.671 mm thick solid electrolyte membrane.

[0052] (7) Storage of solid electrolyte: While the dried solid electrolyte is still hot, transfer it to an anhydrous and oxygen-free glove box, and then use rubber tweezers to peel off the membrane and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0053] Example 4: Preparation of ternary eutectic solid electrolyte according to Figure 1 The process flow diagram shown illustrates the preparation of a ternary eutectic solid electrolyte. The specific steps are as follows: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetamide were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain deep eutectic solvent, which was then stored in the glove box.

[0054] (2) Preparation of ternary eutectic solvent: Mix 0.8 ml of the deep eutectic solvent obtained in step (1) with 0.2 ml of fluoroethylene carbonate to obtain ternary eutectic solvent.

[0055] (3) Preparation of solid electrolyte base solution: 0.532g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 was completely dissolved in 3.033g of organic solvent N,N-dimethylformamide to obtain solid electrolyte base solution.

[0056] (4) Preparation of ternary eutectic polymer solution: Mix all the solid electrolyte substrate solution obtained in step (3) with 0.8 ml of ternary eutectic solvent obtained in step (2) and stir evenly for 1 h to obtain ternary eutectic polymer solution.

[0057] (5) Solution casting: Transfer the solid electrolyte base solution obtained in step (4) to an ultrasonic oscillator and sonicate for 0.5 h to make a large number of bubbles in the solution disappear. Then, use a pipette to slowly draw up the solution, try to avoid the generation of bubbles, and cast it evenly and in appropriate amount into the polytetrafluoroethylene mold.

[0058] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold is transferred to a 50°C drying oven and dried for 6 hours. Then it is transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a 0.731 mm thick solid electrolyte membrane.

[0059] (7) Storage of solid electrolyte: While the dried solid electrolyte is still hot, transfer it to an anhydrous and oxygen-free glove box, and then use rubber tweezers to peel off the membrane and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0060] Example 5: Preparation of ternary eutectic solid electrolyte according to Figure 1 The process flow diagram shown illustrates the preparation of a ternary eutectic solid electrolyte. The specific steps are as follows: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetamide were mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain deep eutectic solvent, which was then stored in the glove box.

[0061] (2) Preparation of ternary eutectic solvent: Mix 0.8 ml of the deep eutectic solvent obtained in step (1) with 0.2 ml of fluoroethylene carbonate to obtain ternary eutectic solvent.

[0062] (3) Preparation of solid electrolyte base solution: 0.527g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 was completely dissolved in 3.016g of organic solvent N,N-dimethylformamide to obtain solid electrolyte base solution.

[0063] (4) Preparation of ternary eutectic polymer solution: Mix all the solid electrolyte substrate solution obtained in step (3) with 0.8 ml of ternary eutectic solvent obtained in step (2) and stir evenly for 1 h to obtain ternary eutectic polymer solution.

[0064] (5) Solution casting: Transfer the solid electrolyte base solution obtained in step (4) to an ultrasonic oscillator and sonicate for 0.5 h to make a large number of bubbles in the solution disappear. Then, use a pipette to slowly draw up the solution, try to avoid the generation of bubbles, and cast it evenly and in appropriate amount into the polytetrafluoroethylene mold.

[0065] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold is transferred to a 50°C drying oven and dried for 6 hours. Then it is transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a solid electrolyte membrane with a thickness of 0.691.

[0066] (7) Storage of solid electrolyte: While the dried solid electrolyte is still hot, transfer it to an anhydrous and oxygen-free glove box, and then use rubber tweezers to peel off the membrane and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0067] Example 6: Preparation of ternary eutectic solid electrolyte and Figure 1 The process flow diagram is similar; the ternary eutectic solid electrolyte is prepared according to the following steps: (1) Preparation of deep eutectic solvent: LiTFSI and N-methylacetyl are mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain deep eutectic solvent, which is then stored in the glove box.

[0068] (2) Preparation of ternary eutectic solvent: Mix 0.8 ml of the deep eutectic solvent obtained in step (1) with 0.2 ml of fluoroethylene carbonate to obtain ternary eutectic solvent.

[0069] (3) Preparation of solid electrolyte base solution: 0.527g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 and 0.052g of polyacrylonitrile (average molecular weight 149,000~151,000) were completely dissolved in 3.022g of organic solvent N,N-dimethylformamide to obtain solid electrolyte base solution.

[0070] (4) Preparation of ternary eutectic polymer solution: Mix all the solid electrolyte substrate solution obtained in step (3) with 0.8 ml of ternary eutectic solvent obtained in step (2) and stir evenly for 1 h to obtain ternary eutectic polymer solution.

[0071] (5) Solution casting: Transfer the solid electrolyte base solution obtained in step (4) to an ultrasonic oscillator and sonicate for 0.5 h to make a large number of bubbles in the solution disappear. Then, use a pipette to slowly draw up the solution, try to avoid the generation of bubbles, and cast it evenly and in appropriate amount into the polytetrafluoroethylene mold.

[0072] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold is transferred to a 50°C drying oven and dried for 6 hours. Then it is transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a solid electrolyte membrane with a thickness of 0.741.

[0073] (7) Storage of solid electrolyte: While the dried solid electrolyte is still hot, transfer it to an anhydrous and oxygen-free glove box, and then use rubber tweezers to peel off the membrane and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0074] Example 7: Preparation of ternary eutectic solid electrolyte and Figure 1 The process flow diagram is similar; the ternary eutectic solid electrolyte is prepared according to the following steps: (1) Preparation of deep eutectic solvent: LiTFSI and succinate are mixed in a glove box at a molar ratio of 1:4 and magnetically stirred at room temperature to obtain deep eutectic solvent, which is then stored in the glove box.

[0075] (2) Preparation of ternary eutectic solvent: Mix 0.8 ml of the deep eutectic solvent obtained in step (1) with 0.2 ml of fluoroethylene carbonate to obtain ternary eutectic solvent.

[0076] (3) Preparation of solid electrolyte base solution: 0.517g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 and 0.112g of polyacrylonitrile (average molecular weight 149,000~151,000) were completely dissolved in 3.024g of organic solvent N,N-dimethylformamide to obtain solid electrolyte base solution.

[0077] (4) Preparation of ternary eutectic polymer solution: Mix all the solid electrolyte substrate solution obtained in step (3) with 0.8 ml of ternary eutectic solvent obtained in step (2) and stir evenly for 1 h to obtain ternary eutectic polymer solution.

[0078] (5) Solution casting: Transfer the solid electrolyte base solution obtained in step (4) to an ultrasonic oscillator and sonicate for 0.5 h to make a large number of bubbles in the solution disappear. Then, use a pipette to slowly draw up the solution, try to avoid the generation of bubbles, and cast it evenly and in appropriate amount into the polytetrafluoroethylene mold.

[0079] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold is transferred to a 50°C drying oven and dried for 6 hours. Then it is transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a solid electrolyte membrane with a thickness of 0.721.

[0080] (7) Storage of solid electrolyte: While the dried solid electrolyte is still hot, transfer it to an anhydrous and oxygen-free glove box, and then use rubber tweezers to peel off the membrane and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0081] Example 8: Preparation of ternary eutectic solid electrolyte and Figure 1The process flow diagram is similar; the ternary eutectic solid electrolyte is prepared according to the following steps: (1) Preparation of deep eutectic solvent: LiTFSI and succinate are mixed in a glove box at a molar ratio of 1:3 and magnetically stirred at room temperature to obtain deep eutectic solvent, which is then stored in the glove box.

[0082] (2) Preparation of ternary eutectic solvent: Mix 0.8 ml of the deep eutectic solvent obtained in step (1) with 0.2 ml of fluoroethylene carbonate to obtain ternary eutectic solvent.

[0083] (3) Preparation of solid electrolyte base solution: 0.527g of poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of Mn ~130,000 and 0.051g of polyacrylonitrile (average molecular weight 149,000~151,000) were completely dissolved in 3.012g of organic solvent N,N-dimethylformamide to obtain solid electrolyte base solution.

[0084] (4) Preparation of ternary eutectic polymer solution: Mix all the solid electrolyte substrate solution obtained in step (3) with 0.8 ml of ternary eutectic solvent obtained in step (2) and stir evenly for 1 h to obtain ternary eutectic polymer solution.

[0085] (5) Solution casting: Transfer the solid electrolyte base solution obtained in step (4) to an ultrasonic oscillator and sonicate for 0.5 h to make a large number of bubbles in the solution disappear. Then, use a pipette to slowly draw up the solution, try to avoid the generation of bubbles, and cast it evenly and in appropriate amount into the polytetrafluoroethylene mold.

[0086] (6) Solid electrolyte molding: The cast polytetrafluoroethylene mold is transferred to a 50°C drying oven and dried for 6 hours. Then it is transferred to a 70°C vacuum drying oven and vacuum dried for 4 hours to obtain a solid electrolyte membrane with a thickness of 0.718.

[0087] (7) Storage of solid electrolyte: While the dried solid electrolyte is still hot, transfer it to an anhydrous and oxygen-free glove box, and then use rubber tweezers to peel off the membrane and seal the obtained ternary eutectic solid electrolyte in the glove box.

[0088] Comparative Example 1 The comparative example uses a method similar to that used in Example 1. The difference is that in step (1), LiTFSI and N-methylacetamide are mixed in a molar ratio of 1:3 and magnetically stirred at room temperature to obtain a deep eutectic solvent.

[0089] Comparative Example 2 The comparative example uses a method similar to that used in Example 1. The difference is that in step (2), the ternary eutectic solvent is prepared by mixing 0.8 ml of the deep eutectic solvent obtained in step (1) with 0.4 ml of fluoroethylene carbonate.

[0090] Comparative Example 3 The method used in this comparative example is similar to that used in Example 1. The difference is that in step (3), the solid electrolyte base solution is prepared by completely dissolving poly(vinylidene fluoride-co-hexafluoropropylene) with a molecular weight of 50,000 using 3.006g of organic solvent N,N-dimethylformamide.

[0091] Comparative Example 4 The comparative example uses a method similar to that used in Example 1. The difference is that in step (4), the ternary eutectic polymer solution is prepared by mixing all the solid electrolyte substrate solution obtained in step (3) with 0.6 ml of ternary eutectic solvent and stirring for 1 hour.

[0092] Comparative Example 5 The method used in this comparative example is similar to that used in Example 1. The difference is that in step (5) solution casting, the solid electrolyte base solution obtained in step (4) is not ultrasonicated. Instead, the solution is drawn up with a pipette and cast into a polytetrafluoroethylene mold in an appropriate amount.

[0093] Comparative Example 6 The method used in this comparative example is similar to that used in Example 1. The difference is that in step (6) solid electrolyte molding, the cast polytetrafluoroethylene mold is transferred to a 50°C drying oven and dried for 2 hours, and then transferred to a 60°C vacuum drying oven for vacuum drying for 2 hours.

[0094] Test Implementation Examples I. Flame retardant properties The test method is as follows: The ternary eutectic solid electrolyte obtained in Example 1 is burned with an open flame. After the ternary eutectic solid electrolyte is ignited, the time required for it to self-extinguish is recorded.

[0095] Test results are as follows Figure 2 As shown, the ternary eutectic solid electrolyte of the present invention self-extinguishes 0.3 seconds after ignition, indicating that the ternary eutectic solid electrolyte has good self-extinguishing properties and excellent safety after being ignited by an open flame.

[0096] II. Thermal stability The testing methods are as follows: Thermogravimetric analysis and DSC analysis were performed on the ternary eutectic solid electrolyte in Example 2. PVDF-HFP represents a single poly(vinylidene fluoride-co-hexafluoropropylene), P-0.8 represents a ternary eutectic solid electrolyte prepared with only 0.8 ml of deep eutectic solvent, and P-0.8-FEC represents the ternary eutectic solid electrolyte in Example 2. All three samples exhibited stability at 120 °C. However, the deep eutectic solvent showed significant weight loss at 120 °C, 300 °C, and 450 °C, indicating the decomposition of residual water, the deep eutectic solvent, and poly(vinylidene fluoride-co-hexafluoropropylene), respectively. This may be due to the influence of the deep eutectic solvent on the poly(vinylidene fluoride-co-hexafluoropropylene) structure. The collapse of the poly(vinylidene fluoride-co-hexafluoropropylene) structure during deep eutectic solvent decomposition may lead to a decrease in the decomposition temperature. Figure 3 The results show that the glass transition temperature (Tg) of P-0.8-FEC decreased from 147℃ to 142℃ after the addition of fluoroethylene carbonate, indicating a decrease in its crystallinity. However, the addition of fluoroethylene carbonate did not significantly affect the melting temperature (Tm), suggesting that the deep eutectic solvent established a stable structure with poly(vinylidene fluoride-co-hexafluoropropylene).

[0097] III. Battery Performance 1. Button cell battery The solid electrolytes prepared in Examples 1-8 and Comparative Examples 1-6 were used to assemble Li / / P-0.8-FEC / / LFP coin cells (CR2032) (positive electrode material: lithium iron phosphate; negative electrode material: lithium metal; solid electrolyte: ternary eutectic solid electrolyte). The specific capacity and capacity retention of the coin cells were tested under 1C conditions at 25 degrees Celsius.

[0098] The experimental results are shown in Table 1.

[0099] The discharge specific capacity and capacity retention of the solid electrolyte-assembled Li / / P-0.8-FEC / / LFP coin cells prepared in Examples 1-8 under 1C conditions are shown in Table 1. The long-cycle diagram of the solid electrolyte-assembled Li / / P-0.8-FEC / / LFP coin cell in Example 3 is shown in Table 1. Figure 4 .

[0100] Table 1. Battery material performance of each embodiment and comparative example

[0101] As shown in Table 1, the coin cell assembled with solid electrolyte in Example 1 has a discharge specific capacity of 139.7 mAh g⁻¹ after 500 long-cycle discharge. -1The capacity retention rate was 97.7%; the coin cell assembled with solid electrolyte in Example 2 had a discharge specific capacity of 140.1 mAh g after 500 long-cycle discharge. -1 The capacity retention rate was 98.8%; the coin cell assembled with solid electrolyte in Example 3 had a discharge specific capacity of 138.7 mAh g after 500 long-cycle discharge. -1 The capacity retention rate was 97.9%; the coin cell assembled with solid electrolyte in Example 4 had a discharge specific capacity of 139.9 mAh g after 500 long-cycle discharge. -1 The capacity retention rate was 98.3%; the coin cell assembled with solid electrolyte in Example 6 had a discharge specific capacity of 126.3 mAh g after 500 long-cycle discharge. -1 The capacity retention rate was 96.2%. The coin cell assembled with the solid electrolyte in Example 7 had a discharge specific capacity of 121.3 mAh g⁻¹ after 500 long-cycle discharge events. -1 The capacity retention rate was 97.2%. Example 8: A coin cell assembled with a solid electrolyte exhibited a discharge specific capacity of 118.7 mAh g⁻¹ after 500 long-cycle discharge. -1 The capacity retention rate was 96.5%. This demonstrates that the Li / / solid electrolyte / / LFP coin cell assembled using the solid electrolyte prepared with the ternary eutectic solvent of this invention can cycle stably under 1C conditions, with a maximum capacity of 140.1 mAh g⁻¹. -1 It has a high discharge specific capacity and a capacity retention rate of 98.8%, exhibiting good charge and discharge performance.

[0102] The comparison results between Example 1 and Comparative Example 1 show that different proportions of deep eutectic solvents result in different ionic conductivity, which affects the final cycle performance of the lithium battery.

[0103] The comparison results between Example 1 and Comparative Example 2 show that an appropriate amount of ethylene carbonate is more conducive to ion transport and stable SEI layer formation, thereby improving its cycle performance. However, more fluoroethylene carbonate will cause side reactions, affecting the decomposition of lithium salt and leading to a decrease in battery cycle performance.

[0104] The comparison results of Example 1 and Comparative Example 3 show that the degree of polymerization of the PVDF-HFP substrate affects the ion transport efficiency and mechanical properties of the polymer electrolyte after film formation, which in turn affects the cycle performance of the final lithium battery.

[0105] The comparison results between Example 1 and Comparative Example 4 show that different amounts of ternary deep eutectic solvent directly affect the ionic conductivity and ion transport efficiency, which in turn affects the cycle performance of the final lithium battery.

[0106] The comparison results between Example 1 and Comparative Example 5 show that the solution without ultrasonication contains very fine bubbles, which generate bubbles during evaporation and film formation, affecting the mechanical properties of the electrolyte and the battery cycle performance.

[0107] The comparison results between Example 1 and Comparative Example 6 show that the drying temperature and drying time after casting also affect the cycle performance of lithium batteries.

[0108] 2. Soft-pack battery The ternary eutectic solid electrolyte prepared in Example 5 was used to assemble a single-layer pouch cell (positive electrode material: lithium iron phosphate, negative electrode material: pre-lithiated graphite, solid electrolyte: ternary eutectic solid electrolyte) Gr / / P-0.8-FEC / / LFP. The pouch cell assembly was as follows: the prepared lithium iron phosphate and graphite electrodes were used as the positive and negative electrodes, respectively, and the ternary eutectic solid electrolyte was placed in the middle. Then, the stacked batteries were placed in an aluminum-plastic film battery casing and vacuum-sealed using a pouch side sealer.

[0109] The specific capacity and capacity retention of this pouch cell were tested at 1C at room temperature. The long-cycle diagram of this pouch cell at 1C is shown below. Figure 5 As can be seen, the eutectic solid electrolyte pouch battery assembled with the ternary eutectic solid electrolyte of the present invention exhibits stable cycle performance under 1C conditions.

[0110] The safety performance of the pouch cell was tested using the following steps: A single-layer pouch cell of Gr / / P-0.8-FEC / / LFP was assembled using the ternary eutectic solid electrolyte prepared in Example 5. A puncture test was then performed after assembly. Puncture test: The puncture test was conducted at room temperature using the puncture mode of an MSK-TE905 testing instrument. The puncture duration was 1 second, the puncture location was 32 mm, and the puncture diameter was 0.25 cm. The voltage change during the puncture test is shown in [the figure]. Figure 6 The results showed that the battery voltage dropped sharply at the moment of needle puncture, but did not lead to a complete short circuit. After the puncture process, the battery voltage recovered to its original level before puncture. Furthermore, the pouch battery did not exhibit thermal runaway before or after puncture, which is a very safe phenomenon. This demonstrates that the ternary eutectic solid electrolyte pouch battery assembled with the present invention possesses excellent safety and stability.

[0111] The present invention has been described in detail above. Those skilled in the art will recognize that the invention can be practiced in a wide range of ways with equivalent parameters, concentrations, and conditions without departing from its spirit and scope. While specific embodiments have been provided, it should be understood that further modifications can be made to the invention. In summary, according to the principles of the invention, this application is intended to include any changes, uses, or improvements to the invention, including modifications made using conventional techniques known in the art that depart from the scope disclosed herein.

Claims

1. A method for preparing a ternary eutectic solid electrolyte, characterized in that, Includes the following steps: S1. Mix the hydrogen bond acceptor and hydrogen bond donor containing lithium ions to obtain a deep eutectic solvent; The lithium-ion-containing hydrogen bond acceptor includes any one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium dioxaborate, lithium difluorooxaborate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium perchlorate, lithium nitrate, lithium chloride, and lithium difluorophosphate. The hydrogen bond donor includes any one of N-methylacetamide, acetamide, butyramide, propionamide, N,N-dimethylpropenylurea, methyl pyruvate dimethyl sulfone, ethylene carbonate, succinate, and 2,2'-dithiopyridine. The molar ratio of the lithium-ion-containing hydrogen bond acceptor to the hydrogen bond donor is 1:(2-6). S2. Mix the deep eutectic solvent and the modifier to obtain a ternary eutectic solvent; The modifier includes one or more of ethylene carbonate, vinylene carbonate, and fluoroethylene carbonate; The volume ratio of the deep eutectic solvent to the modifier is (3-6):1; S3. Dissolve the polymer in an organic solvent to obtain a polymer solution; The polymer includes one or more of poly(vinylidene fluoride-co-hexafluoropropylene), polyethylene oxide, polyethylene glycol diacrylate, polyacrylonitrile, polyvinylidene fluoride, and polymethyl methacrylate. The mass ratio of the polymer to the organic solvent is 1:(4-6); The mass ratio of the ternary eutectic solvent to the polymer solution is 1:(2-5); S4. Mix the ternary eutectic solvent and the polymer solution evenly to obtain a ternary eutectic polymer solution; S5. The ternary eutectic polymer solution is dried and shaped to obtain the ternary eutectic solid electrolyte.

2. The method for preparing the ternary eutectic solid electrolyte according to claim 1, characterized in that: The number average molecular weight of the polymer is 100,000 to 1,000,000.

3. The method for preparing the ternary eutectic solid electrolyte according to any one of claims 1-2, characterized in that: The method further includes the following step before the drying and molding: ultrasonic treatment of the ternary eutectic polymer solution to remove air bubbles in the solution.

4. The method for preparing the ternary eutectic solid electrolyte according to any one of claims 1-2, characterized in that: The drying and molding steps are as follows: the ternary eutectic polymer solution is poured into a mold for drying.

5. The method for preparing the ternary eutectic solid electrolyte according to claim 4, characterized in that: The drying process involves first drying at 40–60 degrees Celsius for 2–5 hours, and then vacuum drying at 60–80 degrees Celsius for 4–6 hours.

6. The ternary eutectic solid electrolyte obtained by the preparation method according to any one of claims 1-5.

7. A solid-state lithium battery, characterized in that, It includes a positive electrode, a negative electrode, and the ternary eutectic solid electrolyte as described in claim 6.

8. The solid-state lithium battery according to claim 7, characterized in that: The solid-state lithium battery is a button cell or a pouch cell.