Thermosensitive recording body

By combining a specific color developer with low-oil-absorption inorganic pigments and hollow particles in a thermal recorder, the problems of insufficient long-term preservation and heat resistance of existing thermal recorders are solved, and the high sensitivity and heat-resistant background fogging are improved.

CN119053452BActive Publication Date: 2026-11-24OJI HLDG CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380033793.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-09-22
Filing Date
2023-04-13
Publication Date
2026-11-24
Estimated Expiration
2043-04-13

AI Technical Summary

Technical Problem

Existing thermal recorders have shortcomings in terms of long-term preservation of printed materials and resistance to heat-induced background fogging, especially non-phenolic color developers which perform poorly at high temperatures.

Method used

A specific color developer is combined with an inorganic pigment with an oil absorption of less than 130 mL/100 g, and 5-(N-3-methylphenyl-sulfonamide)-N',N”-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureo)phenyl]benzenesulfonamide is added as a second color developer to the thermal recording layer. This is combined with hollow particles and a binder to form a base layer, thereby improving the heat resistance and sensitivity of the recording layer.

Benefits of technology

Significant improvements have been achieved in the long-term preservation of thermal recorders and resistance to thermal background fogging, with high sensitivity and excellent plasticizer resistance in the print head.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119053452B_ABST
    Figure CN119053452B_ABST
Patent Text Reader

Abstract

A thermal recorder is disclosed, which has at least sequentially formed, on a support, a base layer comprising hollow particles and a binder, and a thermal recording layer comprising a leuco dye and a developer. The thermal recorder comprises a compound represented by the following general formula (1) (where R...). 1 To R 5 The first colorimetric agent of the thermal recording layer is represented by hydrogen atom, halogen atom, nitro group, amino group, alkyl group, alkoxy group, aryloxy group, alkyl carbonyloxy group, aryl carbonyloxy group, alkyl carbonyl amino group, aryl carbonyl amino group, alkyl sulfonyl amino group, aryl sulfonyl amino group, monoalkyl amino group, dialkyl amino group, and aryl amino group; and satisfies requirement (A) or requirement (B), namely, (A) the base layer contains inorganic pigment I, and the thermal recording layer contains a pigment with an oil absorption of less than 130 ml / 100 g as inorganic pigment II, and (B) the thermal recording layer contains 5-(N-3-methylphenyl-sulfonamide)-N',N”-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureo)phenyl]benzenesulfonamide as the second colorimetric agent, wherein the content of the second colorimetric agent is 0.4 to 2.5 parts by mass relative to 1 part by mass of the first colorimetric agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to thermal recording devices. Background Technology

[0002] Thermal recorders, widely used in practical applications, record color images by utilizing a heating reaction between colorless or light-colored leuco dyes and phenols or organic acids. The advantages of such thermal recorders include, for example, the ability to form color images simply by applying heat, and furthermore, the recording devices used for them can be compact, easy to maintain, and generate less noise. For this reason, thermal recorders have been used in a wide range of technical fields as various information recording materials for printing devices such as label printers, automatic ticket vending machines, CD / ATMs, order output devices used in restaurants, and data output devices in scientific research equipment.

[0003] Typically, color developers containing phenolic hydroxyl groups have drawbacks such as poor thermal responsiveness and poor water resistance in the printing area, and phenolic compounds such as bisphenol A have endocrine problems. Therefore, mainly in Europe, there is an increasing demand for thermal recording paper containing non-phenolic color developers, and various new non-phenolic color developers have been developed.

[0004] For example, Patent Document 1 proposes a thermal recorder containing 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate as a non-phenolic developer, and reports that the printed portion exhibits excellent water resistance and the background shows high thermal stability. However, although such a developer has excellent heat resistance to background fogging at 90°C, the long-term preservation of the printed material is poor.

[0005] Patent document 2 reports that a combination of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate and a urea carbamate compound represented by the following formula (2) as a colorimetric agent has excellent printability.

[0006] However, in Patent Documents 1 and 2, the heat resistance to background fogging at a maximum of 90°C was only evaluated for such color developers. In the market, there is a recent demand for higher heat resistance, and heat resistance at 90°C is insufficient. Therefore, further improvements are needed.

[0007] Existing technical documents

[0008] Patent documents

[0009] Patent Document 1: JP6529197B

[0010] Patent Document 2: JP7072130B Summary of the Invention

[0011] The problem the invention aims to solve

[0012] A primary objective of this invention is to provide a thermal recorder that exhibits excellent long-term preservation properties in printing.

[0013] Another embodiment of the present invention aims to provide a thermal recorder with high sensitivity, excellent resistance to heat background fogging, and excellent plasticizer resistance of the printed portion.

[0014] Solution for solving the problem

[0015] To achieve the above-mentioned objective, the inventors conducted extensive research and discovered that the above-mentioned objective can be achieved by combining a specific color developer with an inorganic pigment having an oil absorption of less than 130 mL / 100 g and by combining a compound represented by the following formula (1) with the specific color developer. Based on this discovery, the present invention was completed. More specifically, the present invention provides the following thermal recorder.

[0016] Project 1.

[0017] A thermal recording device comprising, in sequence on a support, at least an undercoat layer and a thermal recording layer.

[0018] The base coat consists of hollow particles and a binder.

[0019] The thermal recording layer contains leuco dyes and developers.

[0020] The thermal recorder contains a compound represented by the following formula (1) as the first chromogenic agent of the thermal recording layer:

[0021]

[0022] Where R 1 To R 5 They may be the same or different, and each represents a hydrogen atom, halogen atom, nitro group, amino group, alkyl group, alkoxy group, aryloxy group, alkyl carbonyloxy group, aryl carbonyloxy group, alkyl carbonyl amino group, aryl carbonyl amino group, alkyl sulfonyl amino group, aryl sulfonyl amino group, monoalkyl amino group, dialkyl amino group, or aryl amino group.

[0023] The thermal recorder meets either requirement (A) or (B):

[0024] (A) The base layer contains inorganic pigment I, and the thermal recording layer contains inorganic pigment II with an oil absorption of less than 130 ml / 100 g; or

[0025] (B) The thermal recording layer contains 5-(N-3-methylphenyl-sulfonamide)-N',N”-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureo)phenyl]benzenesulfonamide as a second colorimetric agent, and contains the second colorimetric agent in an amount of 0.4 to 2.5 parts by mass relative to 1 part by mass of the first colorimetric agent.

[0026] Project 2.

[0027] According to the thermal recorder of Project 1, the compound represented by formula (1) is at least one selected from the group consisting of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, 2-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate and 4-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate.

[0028] Project 3.

[0029] According to the thermal recorder described in Project 1, the compound represented by formula (1) is 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate.

[0030] Project 4.

[0031] The thermal recorder according to any one of items 1 to 3 satisfies requirement (A).

[0032] Project 5.

[0033] According to the thermal recorder described in Project 4, the content of inorganic pigment I is less than 60% by mass based on the total solid content of the base coating.

[0034] Project 6.

[0035] According to the thermal recorder described in Project 4 or 5, the oil absorption of inorganic pigment I is less than 130 mL / 100 g.

[0036] Project 7.

[0037] The thermal recorder according to any one of items 4 to 6, wherein the oil absorption of inorganic pigment II is less than 65 mL / 100 g.

[0038] Project 8.

[0039] The thermal recorder according to any one of items 4 to 7, wherein the inorganic pigment II is at least one selected from the group consisting of calcium carbonate, aluminum hydroxide and clay.

[0040] Project 9.

[0041] The thermal recorder according to any one of items 1 to 3 meets requirement (B).

[0042] Project 10.

[0043] According to the thermal recorder of Project 9, the second colorimetric agent is contained in an amount of 0.9 to 2.5 parts by mass relative to 1 part by mass of the first colorimetric agent.

[0044] Project 11.

[0045] According to the thermal recorder described in Project 9 or 10, the second chromogenic agent is 5-(N-3-methylphenyl-sulfonamide)-N',N”-bis-(3-methylphenyl)-isophthalic acid diamide.

[0046] Project 12.

[0047] The thermal recorder according to any one of items 9 to 11, wherein the thermal recording layer comprises at least one sensitizer selected from the group consisting of dimethyl terephthalate, 1,2-di(3-methylphenoxy)ethane, stearamide and diphenyl sulfone.

[0048] Project 13.

[0049] The thermal recorder according to any one of items 9 to 11, wherein the thermal recording layer comprises at least one sensitizer selected from the group consisting of dimethyl terephthalate and 1,2-bis(3-methylphenoxy)ethane.

[0050] Project 14.

[0051] According to any one of items 4 to 8, the thermal recorder has a maximum particle size (D100) of 10 to 30 μm and an average particle size (D50) of 3 to 15 μm, a ratio of maximum particle size (D100) to average particle size (D50) of D100 / D50 of 1.8 to 3.0, and a volume percentage of hollow particles with a particle size of 2.0 μm or less of 1% or less.

[0052] Project 15.

[0053] According to any one of items 9 to 13, the thermal recorder has a maximum particle size (D100) of 10 to 30 μm and an average particle size (D50) of 4.0 to 15 μm, a ratio of the maximum particle size (D100) to the average particle size (D50) of D100 / D50 of 1.8 to 3.0, and a volume percentage of hollow particles with a particle size of 2.0 μm or less of 1% or less.

[0054] Project 16.

[0055] The thermal recorder according to any one of items 1 to 15, wherein the hollowness of the hollow particles is 80% to 98%.

[0056] Project 17.

[0057] According to any one of items 1 to 16, the content of hollow particles is 5% to 40% by mass based on the total solid content of the base coating.

[0058] Project 18.

[0059] The thermal recorder according to any one of items 1 to 17, wherein the binder of the undercoat comprises a binder resin having a glass transition temperature of -10°C or less.

[0060] Project 19.

[0061] The thermal recorder according to any one of items 1 to 17, wherein the binder of the undercoat comprises a binder resin having a glass transition temperature of -30°C or less.

[0062] Project 20.

[0063] The thermal recorder according to any one of items 1 to 19 further includes an adhesive layer on at least one surface of the support.

[0064] The effects of the invention

[0065] The thermal recorder of the present invention exhibits excellent long-term preservation of printed data.

[0066] According to another embodiment of the present invention, the thermal recorder has high sensitivity, excellent resistance to heat background fogging, and excellent resistance to plasticizers in the printing section. Detailed Implementation

[0067] In this specification, the terms "comprising" or "including" include the following concepts: "comprising", "consistently consisting of", and "comprises of".

[0068] In this specification, the numerical range indicated by “~ (to)” means the range of values ​​recorded before and after “~ (to)”, which include the lower limit and the upper limit.

[0069] As used herein, “latex” includes latex in the form of a gel or dry film formed by drying the dispersion medium.

[0070] This invention relates to a thermal recording device, which comprises at least a base coating layer and a thermal recording layer sequentially on a support.

[0071] The base coat consists of hollow particles and a binder.

[0072] The thermal recording layer contains leuco dyes and developers.

[0073] The thermal recorder contains a compound represented by the following formula (1) as the first chromogenic agent of the thermal recording layer:

[0074]

[0075] Where R 1 To R 5 They may be the same or different, and each represents a hydrogen atom, halogen atom, nitro group, amino group, alkyl group, alkoxy group, aryloxy group, alkyl carbonyloxy group, aryl carbonyloxy group, alkyl carbonyl amino group, aryl carbonyl amino group, alkyl sulfonyl amino group, aryl sulfonyl amino group, monoalkyl amino group, dialkyl amino group, or aryl amino group.

[0076] The thermal recorder meets either requirement (A) or (B):

[0077] (A) The base layer contains inorganic pigment I, and the thermal recording layer contains inorganic pigment II with an oil absorption of less than 130 ml / 100 g; or

[0078] (B) The thermal recording layer contains 5-(N-3-methylphenyl-sulfonamide)-N',N”-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureo)phenyl]benzenesulfonamide as a second colorimetric agent, and contains the second colorimetric agent in an amount of 0.4 to 2.5 parts by mass relative to 1 part by mass of the first colorimetric agent.

[0079] A thermal recorder having the above-mentioned characteristic (A) is called a "thermal recorder (A)", and a thermal recorder having the above-mentioned characteristic (B) is called a "thermal recorder (B)". They are described in detail below.

[0080] A. Thermal recording medium (A)

[0081] In this invention, the thermal recording body comprises at least a base coating layer and a thermal recording layer sequentially on the support.

[0082] The base coat consists of hollow particles, a binder, and inorganic pigment I.

[0083] The thermal recording layer contains leuco dyes, developers, and inorganic pigment II.

[0084] The compound represented by formula (1) (the first colorimetric agent) is used as the colorimetric agent.

[0085] Pigments containing oil absorption of less than 130ml / 100g are classified as inorganic pigments II.

[0086] support body

[0087] The support in this invention is not particularly limited in type, shape, or size. For example, high-quality paper (acidic paper, neutral paper), medium-quality paper, coated paper, art paper, cast-coated paper, cellophane, resin-laminated paper, polyolefin synthetic paper, synthetic fiber paper, nonwoven fabric, synthetic resin film, or various transparent supports can be appropriately selected and used. The thickness of the support is not particularly limited and is typically about 20–200 μm. The density of the support is not particularly limited and is preferably about 0.60–0.85 g / cm³. 3 .

[0088] Primer

[0089] The thermal recorder of the present invention has an undercoat between a support and a thermal recording layer, and the undercoat comprises hollow particles, a binder and an inorganic pigment I.

[0090] hollow particles

[0091] From the viewpoint of enhancing buffering, the hollow particles are preferably formed of organic resin. The undercoat containing hollow particles and therefore having excellent thermal insulation properties can prevent the diffusion of heat applied to the thermal recording layer and increase the sensitivity of the thermal recorder.

[0092] Based on the production method, hollow particles formed from organic resins can be divided into foamed and non-foamed types. Of these two types, foamed hollow particles generally have a larger average particle size and a higher hollowness ratio than non-foamed hollow particles. Therefore, compared to non-foamed hollow particles, foamed hollow particles offer better sensitivity and image quality.

[0093] Non-foamed hollow particles can be produced by polymerizing seeds in solution, polymerizing other resins to coat the seeds, and removing the internal seeds through swelling and dissolution to create voids inside. Internal seeds can also be removed using alkaline aqueous solutions or similar methods through swelling and dissolution. Non-foamed hollow particles with relatively large average particle sizes can also be produced through alkaline swelling treatment of core-shell particles in which alkaline-swellable core particles coat a non-alkaline-swellable shell.

[0094] Foamed hollow granules can be produced by preparing granules in which volatile liquid is sealed in resin, and by evaporating and expanding the liquid in the granules while the resin is softened by heating.

[0095] In the production process of foamed hollow particles, heating causes the liquid inside the particles to expand, thereby increasing the hollowness and providing excellent thermal insulation. Therefore, using foamed hollow particles can improve the sensitivity of the thermal recorder and enhance recording density. This improved sensitivity is particularly important for color development within a small halftone range where the heat energy applied to the thermal recording layer is limited. Furthermore, when the thermal recording layer is formed from an undercoat with excellent thermal insulation, heat diffusion to the thermal recording layer is prevented, resulting in excellent image uniformity and improved image quality. Therefore, in this embodiment, foamed hollow particles that excel in improving the thermal insulation of the undercoat are preferred.

[0096] Examples of resins that can be used in foamed hollow granules include thermoplastic resins, such as styrene-acrylic resins, polystyrene resins, acrylic resins, polyethylene resins, polypropylene resins, polyacetal resins, chlorinated polyether resins, polyvinyl chloride resins, polyvinylidene chloride resins, acrylic resins (e.g., acrylic resins containing acrylonitrile as a component), styrene resins, vinylidene chloride resins, and copolymer resins mainly formed from polyvinylidene chloride and acrylonitrile. Propane, butane, isobutane, air, etc., can typically be used as the gas contained in the foamed hollow granules. From the viewpoint of strength for maintaining the shape of the foamed granules, acrylonitrile resins and copolymer resins mainly formed from polyvinylidene chloride and acrylonitrile are preferred resins that can be used in hollow granules.

[0097] The maximum particle size of the hollow particles in this invention is preferably 10 to 30 μm, and more preferably 10 to 25 μm. The maximum particle size is also referred to as "D100". When the maximum particle size of the hollow particles is 10 μm or more, the buffering capacity of the undercoat is improved; therefore, the adhesion between the thermal recorder and the hothead is improved during printing, and a thermal recorder with high image quality is obtained. This high image quality can produce improved recording density in the halftone range at energy levels lower than those used to provide maximum recording density (Dmax). When the maximum particle size of the hollow particles is 30 μm or less, the smoothness of the undercoat is improved; therefore, the thermal recording layer disposed between the undercoat and the thermal recorder can be made uniform, and a thermal recorder in which white spots are less likely to form in the image can be obtained.

[0098] The average particle size of the hollow particles in this invention is preferably 3 to 15 μm, more preferably 5 to 15 μm, or preferably 4.0 to 15 μm, more preferably 4.5 to 15 μm. As used herein, the average particle size is the diameter at which the volume of the larger particle is equal to the volume of the smaller particle when the particles are divided into two types based on particle size; that is, the median diameter, which corresponds to a frequency of 50% by volume. The average particle size is also referred to as "D50". When the average particle size of the hollow particles is 3 μm or more, the buffering properties of the undercoat are improved; therefore, the adhesion between the thermal recorder and the hothead is improved during printing, and a thermal recorder with high image quality is obtained. This high image quality can produce improved recording density in the halftone range at energy levels lower than those used to provide maximum recording density (Dmax). When the average particle size of the hollow particles is 15 μm or less, the smoothness of the undercoat is improved; therefore, the thermal recording layer disposed between the undercoat and the thermal recorder can be made uniform, and a thermal recorder in which white spots are less likely to form in the image can be obtained.

[0099] The maximum particle size (D100) and average particle size (D50) of hollow particles can be measured using a laser diffraction particle size distribution analyzer. The average particle size (D50) can be shown as the average of the particle sizes of 10 particles, which are measured from images of individual particles using an electron microscope (SEM image).

[0100] The ratio of the maximum particle size (D100) to the average particle size (D50) of the hollow particles, i.e., D100 / D50, is an indicator of the degree of particle size distribution. The D100 / D50 ratio is preferably 1.8 to 3.0, and more preferably 2.0 to 2.8. When the D100 / D50 ratio of the hollow particles is 1.8 or higher, the hollow particles can be fully foamed, the maximum particle size will be large enough, the hollowness ratio will be high, and the thermal insulation of the undercoat can be improved. When the D100 / D50 ratio of the hollow particles is 3.0 or lower, the size of the hollow particles is uniform, which improves the smoothness of the undercoat and suppresses white spots in the image.

[0101] In the particle size distribution measured using a laser diffraction particle size distribution analyzer, the volume percentage of hollow particles with a diameter of 2.0 μm or less is preferably 1% or less. More preferably, the volume percentage of hollow particles with a diameter of 2.0 μm or less is 0.5% or less, and even more preferably, hollow particles with a diameter of 2.0 μm or less are not included. Hollow particles with a diameter of 2 μm or less are considered to contribute very little to thermal insulation because they are too small to have sufficient hollow space. When the volume percentage of hollow particles with a diameter of 2 μm or less in the undercoat is 1% or less, the recording density, image quality, etc., can be improved.

[0102] The hollowness of the hollow particles is preferably 80% to 98%, and more preferably 90% to 98%. When the hollowness of the hollow particles is 80% or more, the undercoating containing the hollow particles can be endowed with excellent thermal insulation properties. When the hollowness of the hollow particles is 98% or less, the strength of the film around the hollow portion is improved, and thus hollow particles that do not collapse even when the undercoating is formed can be obtained.

[0103] The hollowness of the hollow particles is determined by measuring the true specific gravity according to the IPA method, and the true specific gravity value is used as follows.

[0104] (1) Sample pretreatment

[0105] The sample was dried at 60°C for 24 hours.

[0106] (2) Reagents

[0107] Isopropanol (IPA: Ultrapure Reagent)

[0108] (3) Measurement method

[0109] - Weighing volumetric flask (W1).

[0110] Weigh approximately 0.5 g of the dried sample (W2) into a volumetric flask.

[0111] Add approximately 50 mg of IPA and shake the volumetric flask thoroughly to completely remove any air from the capsule.

[0112] - Add IPA to the mark line and weigh the volumetric flask (W3).

[0113] - As a blank, simply add IPA to the mark line of the volumetric flask and weigh the volumetric flask (W4).

[0114] (4) Calculation of true specific gravity

[0115] True specific gravity = {(W2-W1)×((W4-W1) / 100)} / {(W4-W1)-(W3-W2)}

[0116] (5) Calculation of hollow ratio

[0117] Hollow content (%) = {1 - 1 / (1.1 / true specific gravity)} × 100

[0118] The hollow ratio can also be calculated using the following formula: (d 3 / D 3 )×100. In the formula, d represents the inner diameter of the hollow particle, and D represents the outer diameter of the hollow particle.

[0119] Because the hollow particles in this invention have a relatively large particle size, the content of hollow particles in the primer coating can be reduced. The content of hollow particles is based on the total solid content of the primer coating, preferably 5 to 40% by mass, and more preferably 5 to 35% by mass. A hollow particle content of 5% by mass or more can improve the thermal insulation of the primer coating, while a hollow particle content of 40% by mass or less makes it less likely to cause problems such as coatability, and allows for easy formation of a uniform primer coating and improved recording concentration. Furthermore, the film strength of the primer coating can be improved.

[0120] adhesive

[0121] Examples of binders include water-soluble polymers such as polyvinyl alcohol and its derivatives, starch and its derivatives, cellulose derivatives such as hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose and ethyl cellulose, sodium polyacrylate, polyvinylpyrrolidone, acrylamide-acrylate copolymers, acrylamide-acrylate-methacrylate copolymers, styrene-maleic anhydride copolymers, isobutylene-maleic anhydride copolymers, casein, gelatin and its derivatives; emulsions such as polyvinyl acetate, polyurethane, polyacrylic acid, polyacrylate, vinyl chloride-vinyl acetate copolymers, polybutyl methacrylate and ethylene-vinyl acetate copolymers; and latexes of water-insoluble polymers such as styrene-butadiene copolymers and styrene-butadiene-acrylic copolymers; etc. Among these, binders containing latex are preferred. The content of the binder can be selected from a wide range, and is generally preferably from about 20% by mass to 70% by mass, and more preferably from about 25% by mass to 60% by mass, based on the total solid content of the base coat.

[0122] The adhesive preferably comprises an adhesive resin with a glass transition temperature (Tg) below -10°C. When the glass transition temperature is below -10°C, image quality can be improved even in the low energy range. A glass transition temperature below -30°C is more preferred because image quality can be further improved in the low energy range. A glass transition temperature below -50°C is undesirable because adhesion will occur. Therefore, a glass transition temperature above -40°C is preferred.

[0123] Inorganic Pigment I

[0124] The base coating of this invention comprises inorganic pigment I. From the viewpoint of increasing recording concentration and improving long-term preservation, the oil absorption of inorganic pigment I is preferably 130 mL / 100g or less, more preferably 125 mL / 100g or less, and even more preferably 110 mL / 100g or less. From the viewpoint of effectively reducing printing problems such as tip residue and adhesion, the oil absorption of inorganic pigment I is also preferably 40 mL / 100g or more, more preferably 80 mL / 100g or more. The oil absorption is a value obtained according to the method of JIS K 5101.

[0125] Various inorganic pigments can be used as inorganic pigment I, with preferred examples including calcined kaolin and clay. From the viewpoint of improving long-term preservation, the content of inorganic pigment I based on the total solids content of the undercoat is preferably 60% by mass or less, and more preferably 50% by mass or less. From the viewpoint of effectively reducing printing problems such as head residue and adhesion, the content of inorganic pigment I based on the total solids content of the undercoat is also preferably 20% by mass or more, and more preferably 25% by mass or more.

[0126] For example, a primer coating solution is prepared by mixing hollow particles, a binder, inorganic pigment I, and optional additives using water as a medium. The coating solution is then applied to a support and dried to form a primer coating on the support. There is no particular limitation on the amount of primer coating solution applied, but it is preferably about 2 to 20 g / m³ based on the dried mass. 2 More preferably about 2 to 12 g / m 2 .

[0127] thermal recording layer

[0128] Leuco dyes

[0129] The thermal recording layer of the thermal recorder of the present invention can contain any of a variety of known colorless or light-colored leuco dyes. Specific examples of such leuco dyes are described below.

[0130] Specific examples of leuco dyes include blue chromogenic dyes such as 3,3-bis(p-dimethylaminophenyl)-6-dimethylaminophthalide, 3-(4-diethylamino-2-methylphenyl)-3-(4-dimethylaminophenyl)-6-dimethylaminophthalide, and fluorane; green chromogenic dyes such as 3-(N-ethyl-N-p-tolyl)amino-7-N-methylaniline fluorane, 3-diethylamino-7-aniline fluorane, 3-diethylamino-7-dibenzylaminofluorane, and rhodamine B-aniline lactam; and red chromogenic dyes such as 3,6-bis(diethylamino)fluorane-γ-aniline lactam, 3-cyclohexylamino-6-chlorofluorane, 3-diethylamino-6-methyl-7-chlorofluorane, and 3-diethylamino-7-chlorofluorane.Black color-developing dyes, such as 3-(N-ethyl-N-isopentyl)amino-6-methyl-7-anilinofluorane, 3-(N-methyl-N-cyclohexyl)amino-6-methyl-7-anilinofluorane, 3-diethylamino-6-methyl-7-anilinofluorane, 3-di(n-butyl)amino-6-methyl-7-anilinofluorane, 3-di(n-pentyl)amino-6-methyl-7-anilinofluorane, 3-(N-ethyl-N-isopentylamino)-6-methyl-7-anilinofluorane, 3-diethylamino-7-(m-trifluoromethylanilino)fluorane, 3-(N-isopentyl-N-ethylamino)-7-(o-chloroanilino)fluorane, 3-(N-ethyl-N-2- Tetrahydrofurfurylamino)-6-methyl-7-aniline fluorane, 3-(N-hexyl-N-ethylamino)-6-methyl-7-aniline fluorane, 3-[N-(3-ethoxypropyl)-N-ethylamino]-6-methyl-7-aniline fluorane, 3-[N-(3-ethoxypropyl)-N-methylamino]-6-methyl-7-aniline fluorane, 3-diethylamino-7-(2-chloroaniline)fluorane, 3-di(n-butylamino)-7-(2-chloroaniline)fluorane, 4,4'-bis-dimethylaminobenzodihydroindene benzyl ether, N-2,4,5-trichlorophenylleucoauramine amine), 3-diethylamino-7-butylaminofluorane, 3-ethyl-tolylamino-6-methyl-7-aniline fluorane, 3-cyclohexyl-methylamino-6-methyl-7-aniline fluorane, 3-diethylamino-6-chloro-7-(β-ethoxyethyl)aminofluorane, 3-diethylamino-6-chloro-7-(γ-chloropropyl)aminofluorane, 3-diethylamino-6-methyl-7-aniline fluorane, 3-(N-isopentyl-N-ethylamino)-6-methyl-7-aniline fluorane, 3-dibutylamino-7-chloroaniline fluorane, 3-diethylamino-7-(o-chlorophenylamino)fluorane, 3-(N-ethyl-p-tolyl)-6-methyl-7-phenyl Aminofluorane, 3-(N-ethyl-p-toluidine)-6-methyl-7-(p-toluidine)fluorane, 3-(N-ethyl-N-tetrahydrofurfurylamino)-6-methyl-7-aniline fluorane, 3-diethylamino-6-chloro-7-aniline fluorane, 3-dimethylamino-6-methyl-7-aniline fluorane, 3-pyrrolidinyl-6-methyl-7-aniline fluorane, 3-piperidinyl-6-methyl-7-aniline fluorane, 2,2-bis{4-[6'-(N-cyclohexyl-N-methylamino)-3'-methylspiro[phthalide-3,9'-xanthonone-2'-ylamino]phenyl}propane and 3-diethylamino-7-(3'-trifluoromethylphenyl)aminofluorane;Dyes with absorption wavelengths in the near-infrared region include, for example, 3,3-bis[1-(4-methoxyphenyl)-1-(4-dimethylaminophenyl)ethylidene-2-yl]-4,5,6,7-tetrachlorophthalide, 3,3-bis[1-(4-methoxyphenyl)-1-(4-pyrrolidinephenyl)ethylidene-2-yl]-4,5,6,7-tetrachlorophthalide, 3-p-(p-dimethylaminoanilino)anilino-6-methyl-7-chlorofluorane, 3-p-(p-chloroanilino)anilino-6-methyl-7-chlorofluorane, and 3,6-bis(dimethylamino)fluorene-9-spiro-3'-(6'-dimethylamino)phthalide; etc. Of course, the available leuco dyes are not limited to these compounds, and two or more such compounds can be used in combination as needed.

[0131] There is no particular limitation on the content of the leuco dye, and the total solid content based on the thermal recording layer is preferably about 3 to 30% by mass, more preferably about 5 to 25% by mass, and even more preferably about 7 to 20% by mass. A leuco dye content of 3% by mass or more can improve the color development ability, thereby improving the recording concentration, while a leuco dye content of 30% by mass or less can improve the heat resistance.

[0132] color developer

[0133] In this invention, a compound represented by formula (1) is included as a first color developer. The combination of this compound with inorganic pigment II can achieve excellent long-term preservation of the printed material.

[0134] By R 1 To R 5 The halogen atom represented can be a fluorine atom, a chlorine atom, or a bromine atom, with fluorine and chlorine atoms being preferred.

[0135] Alkyl groups can be straight-chain, branched, or cyclic, and are preferably straight-chain or branched alkyl groups, and more preferably straight-chain alkyl groups. Typically, the alkyl group is C10. 1-12 Alkyl, preferably C 1-8 Alkyl, more preferably C 1-6 Alkyl, and even more preferably C 1-4 alkyl.

[0136] The alkoxy group can be straight-chain, branched, or cyclic, and is preferably straight-chain or branched, and more preferably straight-chain alkoxy. Typically, the alkoxy group is C10-32 ... 1-12 Alkoxy, preferably C 2-8 Alkoxy, more preferably C 2-6 Alkyl groups, and even more preferably C 2-4 Alkyl group.

[0137] The alkyl carbonyloxy group can be straight-chain, branched, or cyclic, and is preferably straight-chain or branched, and more preferably straight-chain alkyl carbonyloxy. The alkyl carbonyloxy group is also preferably C10. 1-10 Alkyl carbonyloxy group.

[0138] The alkyl carbonyl amino group can be straight-chain, branched, or cyclic, and is preferably straight-chain or branched, and more preferably straight-chain alkyl carbonyl amino group. The alkyl carbonyl amino group is also preferably C10. 1-10 Alkyl carbonyl amino.

[0139] The alkylsulfonylamino group can be straight-chain, branched, or cyclic, and is preferably straight-chain or branched, and more preferably straight-chain alkylsulfonylamino. The alkylsulfonylamino group is also preferably C10. 1-10 Alkylsulfonylamino.

[0140] An aryl group is a monocyclic or polycyclic aromatic hydrocarbon group formed by one or more 5- or 6-membered aromatic hydrocarbon rings. Examples of aryl groups include phenyl, naphthyl, and biphenyl.

[0141] The preferred aryloxy group is C. 6-12 Aryloxy group. The aryl carbonyloxy group is preferably C. 6-12 Arylcarbonyloxy group. The arylcarbonylamino group is preferably C10. 6-12 Aryl carbonyl amino. Aryl sulfonyl amino is preferably C. 6-12 Arylsulfonylamino.

[0142] Monoalkylamino groups can be straight-chain, branched, or cyclic, and are preferably straight-chain or branched monoalkylamino groups, more preferably straight-chain monoalkylamino groups. Monoalkylamino groups having 1 to 10 carbon atoms are also preferred.

[0143] Dialkylamino groups can be straight-chain, branched, or cyclic, and are preferably straight-chain or branched dialkylamino groups, and more preferably straight-chain dialkylamino groups. Dialkylamino groups having 1 to 10 carbon atoms are also preferred.

[0144] The arylamino group can be a monoarylamino or a diarylamino, and is preferably C10. 6-12 Monoarylamino.

[0145] Specific examples of compounds represented by equation (1) include those in which R 1 To R 5 Compounds in which each atom is an alkyl group or a hydrogen atom, preferably R. 1 To R 5 Each is C 1-8 Compounds with straight-chain alkyl groups or hydrogen atoms, more preferably R 1 To R 5 Each is C 1-4Compounds with straight-chain alkyl or hydrogen atoms, and even more preferably R 1 To R 5 Compounds consisting of either a methyl group or a hydrogen atom.

[0146] Other specific examples of compounds represented by equation (1) include those in which R 1 R 2 R 4 and R 5 Each is a hydrogen atom and R 3 It can be a hydrogen atom, halogen atom, nitro group, amino group, alkyl group, alkoxy group, aryloxy group, alkyl carbonyloxy group, alkyl carbonyl amino group, aryl carbonyl amino group, alkyl sulfonyl amino group, aryl sulfonyl amino group, monoalkyl amino group, dialkyl amino group or aryl amino group (preferably hydrogen atom or alkyl group, more preferably hydrogen atom or C group). 1-8 Alkyl groups, or even more preferably hydrogen atoms or C atoms 1-4 Compounds of alkyl groups, and particularly preferably methyl groups.

[0147] The substitution position of the substituent that is attached to a benzene ring in the diphenylurea structure of formula (1) can be ortho, meta, or para relative to the amino carbonyl group on the benzene ring, preferably ortho or meta, and more preferably meta.

[0148] The compound represented by formula (1) is not particularly limited, but is preferably at least one selected from the group consisting of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, 2-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate and 4-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate. 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate is preferred.

[0149] The content of the compound represented by formula (1) is not particularly limited and can be adjusted according to the leuco dye used. Generally, the content of the compound represented by formula (1) relative to 1 part by mass of leuco dye is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, even more preferably 1 part by mass or more, even more preferably 1.2 parts by mass or more, and particularly preferably 1.5 parts by mass or more. The content of the compound represented by formula (1) relative to 1 part by mass of leuco dye is also preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 4 parts by mass or less, and particularly preferably 3.5 parts by mass or less. A content of 0.5 parts by mass or more of the compound represented by formula (1) can improve recording performance. A content of 10 parts by mass or less of the compound represented by formula (1) can effectively reduce background fogging in high-temperature environments.

[0150] The thermal recording layer may contain other color-developing agents, as long as they do not impair the effectiveness of the invention. Specific examples of other color-developing agents include phenolic compounds, such as 4-tert-butylphenol, 4-acetylphenol, 4-tert-octylphenol, 4,4'-sec-butylidene diphenol, 4-phenylphenol, 4,4'-dihydroxydiphenylmethane, 4,4'-isopropylidene diphenol, 4,4'-cyclohexylidene biphenyl, 4,4'-cyclohexylidene diphenol, 1,1-bis(4-hydroxyphenyl)-ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 4,4'-bis(p-toluenesulfonylaminocarbonylamino)diphenylmethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2'-bis[4-(4-hydroxyphenyl)phenoxy]diethyl ether, 4 4'-Dihydroxydiphenyl sulfide, 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-dihydroxydiphenyl sulfone, 2,4'-dihydroxydiphenyl sulfone, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 2,4'-dihydroxydiphenyl sulfone, 4-hydroxy-4'-isopropoxydiphenyl sulfone, 4-hydroxy-4'-n-propoxydiphenyl sulfone, 4-hydroxy-4'-allyloxydiphenyl sulfone, 4-hydroxy-4'-benzyloxydiphenyl sulfone, 3,3'-diallyl-4,4'-dihydroxydiphenyl sulfone, bis(p-hydroxyphenyl)acetic acid butyl ester, bis(p-hydroxyphenyl)acetic acid methyl ester, hydroquinone monobenzyl ether, bis(3-allyl) 4-hydroxyphenyl sulfone, 4-hydroxy-4'-methyl diphenyl sulfone, 4-allyloxy-4'-hydroxy diphenyl sulfone, 3,4-dihydroxyphenyl-4'-methylphenyl sulfone, 4-hydroxybenzophenone, dimethyl 4-hydroxyphthalate, methyl 4-hydroxybenzoate, propyl 4-hydroxybenzoate, sec-butyl 4-hydroxybenzoate, phenyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, toluene 4-hydroxybenzoate, chlorophenyl 4-hydroxybenzoate, and 4,4'-dihydroxydiphenyl ether; aromatic carboxylic acids, such as benzoic acid, p-chlorobenzoic acid, p-tert-butylbenzoic acid, trichlorobenzoic acid, terephthalic acid, salicylic acid, 3-tert-butylsalicylic acid, 3-isopropylsalicylic acid, 3-benzylsalicylic acid, 3-(α-methylbenzyl)salicylic acid, 3,5-di-tert-butylsalicylic acid, 4-[2-(p-methoxyphenoxy)ethoxy]salicylic acid, 4-[3-(p-toluenesulfonyl)propoxy]salicylic acid, 5-[p-(2-p-methoxyphenoxyethoxy)cumyl]salicylic acid, and zinc 4-[3-(p-toluenesulfonyl)propoxy]salicylic acid; salts of these phenolic compounds or aromatic carboxylic acids with polyvalent metals such as zinc, magnesium, aluminum, calcium, titanium, manganese, tin, and nickel; antipyrine complexes of zinc thiocyanate; complex zinc salts of organic acids such as terephthalic acid and other aromatic carboxylic acids;Thiourea compounds, such as N-p-toluenesulfonyl-N'-3-(p-toluenesulfonyloxy)phenylurea, N-p-toluenesulfonyl-N'-p-butoxycarbonylphenylurea, N-p-toluenesulfonyl-N'-phenylurea, and N,N'-di-m-chlorophenylthiourea; organic compounds with -SO2NH- bonds in their molecules, such as N-(p-toluenesulfonyl)carbamate p-cumylphenyl ester, N-(p-toluenesulfonyl)carbamate p-benzyloxyphenyl ester, N-[2-(3-phenylureo)phenyl]benzenesulfonamide, and N-(o-toluyl)-p-toluenesulfonamide; inorganic acidic substances, such as activated clay, attapulgite, colloidal silica, and aluminum silicate; etc.

[0151] Examples of other color developers include urea carbamate compounds represented by formula (2), such as 4,4'-bis[(4-methyl-3-phenoxycarbonylaminophenyl)ureo]diphenyl sulfone, 4,4'-bis[(2-methyl-5-phenoxycarbonylaminophenyl)ureo]diphenyl sulfone and 4-(2-methyl-3-phenoxycarbonylaminophenyl)ureo-4'-(4-methyl-5-phenoxycarbonylaminophenyl)ureo diphenyl sulfone; cross-linked diphenyl sulfone compounds represented by formula (3); and 4,4'-bis(3-toluenesulfonylureo)diphenylmethane, etc.

[0152]

[0153] Where n = 1 to 6.

[0154] There is no particular limitation on the content of other color developers, and it is preferably 0.5 parts by mass or less, and more preferably 0.3 parts by mass or less, relative to 1 part by mass of the compound represented by formula (1).

[0155] Inorganic Pigment II

[0156] The thermal recording layer of the present invention comprises an inorganic pigment II with an oil absorption of 130 mL / 100 g or less. The oil absorption of the inorganic pigment II is preferably 125 mL / 100 g or less, more preferably 100 mL / 100 g or less, and most preferably 65 mL / 100 g or less. This significantly improves long-term preservation. From the viewpoint of effectively reducing printing problems such as printhead residue and adhesion, the oil absorption of the inorganic pigment II is preferably 30 mL / 100 g or more. The thermal recording layer of the present invention may contain pigment with an oil absorption greater than 130 mL / 100 g, as long as it does not impair the effect of the present invention. The content of pigment with an oil absorption greater than 130 mL / 100 g is preferably 0.5 parts by weight or less, more preferably 0.3 parts by weight or less, and even more preferably 0.1 parts by weight or less, relative to 1 part by weight of pigment with an oil absorption of 130 mL / 100 g or less. Particularly preferred is that the thermal recording layer does not contain pigment with an oil absorption greater than 130 mL / 100 g. The oil absorption rate was determined according to the method in JIS K 5101.

[0157] Various inorganic pigments can be used as inorganic pigment II. Specific examples include inorganic pigments such as calcium carbonate (e.g., light calcium carbonate), aluminum hydroxide, clay (e.g., kaolin), and talc. Inorganic pigment II is preferably at least one selected from the group consisting of calcium carbonate, aluminum hydroxide, and clay. The type of inorganic pigment II may be different from or the same as inorganic pigment I. The content of inorganic pigment II can be selected from a wide range, and is preferably 10–50% by mass, more preferably 10–40% by mass, and even more preferably 15–35% by mass, based on the total solid content of the thermal recording layer.

[0158] In this invention, the thermal recording layer may further comprise a preservation enhancer, primarily to further enhance the preservation of the developed color image. Such a preservation enhancer can be, for example, selected from phenolic compounds, such as 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,1-bis(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 4,4'-[1,4-phenylenebis(1-methylethylene)]bisphenol, and 4,4'-[1,3-phenylenebis(1-methylethylene)]bisphenol. At least one of the following groups: bis(1-methylethylidene)bisphenol; epoxy compounds, such as 4-benzyloxyphenyl-4'-(2-methyl-2,3-epoxypropoxy)phenyl sulfone, 4-(2-methyl-1,2-epoxyethyl)diphenyl sulfone, and 4-(2-ethyl-1,2-epoxyethyl)diphenyl sulfone; and isocyanuric acid compounds, such as 1,3,5-tris(2,6-dimethylbenzyl-3-hydroxy-4-tert-butyl)isocyanuric acid. Of course, the available preservation modifiers are not limited to these compounds, and two or more such compounds may be used in combination as needed.

[0159] When using a preservation enhancer, the amount used can be an effective amount for improving preservation. The preservation enhancer is generally preferably used in an amount of about 1 to 25% by mass, and more preferably about 5 to 20% by mass, based on the total solid content of the thermal recording layer.

[0160] In this invention, the thermal recording layer may further contain a sensitizer. The use of the sensitizer improves recording sensitivity. Examples of available sensitizers include stearamide, methoxycarbonyl-N-stearamide, N-benzoylstearamide, N-eicosanoamide, ethylene bis-stearamide, benzylamide, methylene bis-stearamide, N-hydroxymethylstearamide, dibenzyl terephthalate, dimethyl terephthalate, dioctyl terephthalate, diphenyl sulfone, benzyl p-benzyloxybenzoate, phenyl 1-hydroxy-2-naphthoic acid ester, 2-naphthyl benzyl ether, m-terphenyl, p-benzyl biphenyl, di-p-chlorobenzyl oxalate, di-p-methylbenzyl oxalate, dibenzyl oxalate, p-tolyl diphenyl ether, di(p-methoxyphenoxyethyl) ether, 1,2-di(3-methylphenoxy)ethane, 1,2-di(4-methylphenoxy) Ethane, 1,2-di(4-methoxyphenoxy)ethane, 1,2-di(4-chlorophenoxy)ethane, 1,2-diphenoxyethane, 1-(4-methoxyphenoxy)-2-(3-methylphenoxy)ethane, p-methylthiophenyl benzyl ether, 1,4-di(phenylthio)butane, p-acetyltoluidine, p-acetophenetidide, N-acetylacetyl-p-toluidine, 1,2-diphenoxytoluene, di(β-biphenylethoxy)benzene, p-di(ethyleneoxyethoxy)benzene, 1-isopropylphenyl-2-phenylethane, di-o-chlorobenzyl adipate, 1,2-bis(3,4-dimethylphenyl)ethane, 1,3-bis(2-naphthoxy)propane, biphenyl, and benzophenone, etc. Among these, 1,2-di(3-methylphenoxy)ethane is preferred from the viewpoint of achieving sensitization without compromising long-term shelf life. These sensitizers can be used in combination, as long as the combination does not impair the effectiveness of the present invention. The content of the sensitizer can be the effective amount for sensitization, and the total solid content based on the thermal recording layer is generally preferably 2 to 25% by mass, more preferably 5 to 20% by mass, and even more preferably 5 to 15% by mass.

[0161] As other components constituting the thermal recording layer, binders can be used. Additionally, depending on the requirements, additives such as crosslinking agents, waxes, metal soaps, water resistance improvers, dispersants, colored dyes, and fluorescent dyes can be used.

[0162] Examples of binders include water-soluble polymers such as polyvinyl alcohol and its derivatives, starch and its derivatives, cellulose derivatives such as hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose and ethyl cellulose, sodium polyacrylate, polyvinylpyrrolidone, acrylamide-acrylate copolymer, acrylamide-acrylate-methacrylate copolymer, styrene-maleic anhydride copolymer, isobutylene-maleic anhydride copolymer, casein, gelatin and its derivatives; emulsions such as polyvinyl acetate, polyurethane, polyacrylic acid, polyacrylate, vinyl chloride-vinyl acetate copolymer, polybutyl methacrylate and ethylene-vinyl acetate copolymer; and latexes of water-insoluble polymers such as styrene-butadiene copolymers and styrene-butadiene-acrylic copolymers; etc. Polyvinyl alcohol and latex are preferred. The content of the binder can be selected from a wide range, and is generally preferably about 5 to 30% by mass, and more preferably about 10 to 20% by mass, based on the total solid content of the thermal recording layer.

[0163] When the thermal recording layer contains a crosslinking agent, the water resistance of the thermal recording layer can be improved. Examples of crosslinking agents include aldehyde compounds, such as glyoxal; polyamine compounds, such as polyethyleneimine; epoxy compounds, polyamide resins, melamine resins, glyoxylates, dimethylolurea compounds, aziridine compounds, and capped isocyanate compounds; inorganic compounds, such as ammonium persulfate, ferric chloride, magnesium chloride, sodium tetraborate, and potassium tetraborate; boric acid, triborate, boron polymers, hydrazide compounds, and glyoxylates, etc. These can be used alone or in combination of two or more. The amount of crosslinking agent used is preferably about 1 to 5% by mass based on the total solid content of the thermal recording layer.

[0164] The thermal recording layer is formed on the base layer as follows: For example, using water as the dispersion medium and employing at least one of various agitators or wet mills, such as ball mills, co-ball mills, grinders, or vertical or horizontal sand mills, a leuco dye and a color developer, along with, as needed, a sensitizer or preservation modifier, either together or separately, a water-soluble synthetic polymer such as polyacrylamide, polyvinylpyrrolidone, polyvinyl alcohol, methylcellulose, or styrene-maleic anhydride copolymer salts, and other additives such as surfactants, to form a dispersion; then, the dispersion obtained by reducing the average particle size to less than 2 μm is mixed with inorganic pigment II, optionally further mixed with binders and additives, to prepare a coating liquid for the thermal recording layer; the coating liquid for the thermal recording layer is applied onto the base layer; and then dried. There is no particular limitation on the coating amount of the thermal recording layer, but for the amount of coating after drying, approximately 1 to 12 g / m² is preferred. 2 More preferably 2-10 g / m 2 Even more preferably, it is 2.5–8 g / m³.2 And particularly preferred is 3-5.5 g / m 2 Note that, as needed, the thermal recording layer can be formed as two or more separate layers, and the composition and coating amount of each layer can be the same or different.

[0165] protective layer

[0166] As needed, the thermal recorder may include a protective layer formed on the thermal recording layer. The protective layer preferably comprises pigments and binders. The protective layer preferably further comprises a lubricant, such as a polyolefin wax or zinc stearate, to prevent the protective layer from adhering to the hot head. The protective layer may also contain a UV absorber. When a glossy protective layer is formed, the resulting product can have increased added value.

[0167] There are no particular limitations on the pigments contained in the protective layer. Examples include inorganic pigments such as amorphous silica, kaolin, clay, light calcium carbonate, heavy calcium carbonate, calcined kaolin, titanium dioxide, magnesium carbonate, aluminum hydroxide, colloidal silica, and synthetic layered mica; and plastic pigments such as urea-formaldehyde resin fillers; etc.

[0168] There are no particular limitations on the adhesive contained in the protective layer, and an aqueous adhesive selected from water-soluble and water-dispersible adhesives can be used. The adhesive can be suitably selected from adhesives that can be used in thermal recording layers. Among these, various modified polyvinyl alcohols, such as acetoacetyl-modified polyvinyl alcohol, carboxyl-modified polyvinyl alcohol, and diacetone-modified polyvinyl alcohol, can be more preferably used.

[0169] For example, a protective coating solution is prepared by mixing pigments and binders, optionally with additives, using water as a dispersion medium. The coating solution is then applied to a thermal recording layer and dried to form a protective layer on the thermal recording layer. There are no particular limitations on the amount of the protective coating solution applied, but it is preferably about 0.3 to 15 g / m³ on a dry weight basis. 2 More preferably about 0.3 to 10 g / m 2 Even more preferred is approximately 0.5–8 g / m 2 A particularly preferred concentration is approximately 1–8 g / m³. 2 Furthermore, it is particularly preferred to have a concentration of approximately 1–5 g / m³. 2 Depending on the requirements, the protective layer can be formed into two or more separate layers, and the composition and coating amount of each layer can be the same or different.

[0170] Other layers

[0171] In this invention, the thermal recorder preferably has an adhesive layer on at least one surface of the support. This can increase the added value of the thermal recorder. For example, adhesive paper, rewet adhesive paper, or delayed adhesive paper can be formed as an adhesive layer by coating one surface of the support with an adhesive such as an adhesive, rewet adhesive, or delayed adhesive. Recording paper capable of double-sided recording can also be formed by giving the surface of the support opposite the thermal recording layer the function of thermal transfer paper, inkjet recording paper, carbonless paper, electrostatic recording paper, or electrostatic copying paper. Of course, the thermal recorder can be formed as a double-sided thermal recorder. A back layer can also be provided to inhibit the penetration of oil and plasticizers from the back of the thermal recorder, or for curl control and antistatic purposes. The thermal recorder can also be formed as a linerless label that does not require a release liner by forming a release layer containing silicone on a protective layer and applying an adhesive to one side.

[0172] thermal recording device

[0173] The thermal recorder can be manufactured by forming the aforementioned layers on a support. Any known coating method, such as air knife coating, doctor blade coating, gravure coating, roller coating, spray coating, dip coating, bar coating, curtain coating, groove coating, slip coating, and extrusion, can be used to form the aforementioned layers on the support. Each coating liquid can be applied in a manner that involves applying a first coating liquid and drying it, then applying a second coating liquid and drying it to form layer after layer, or the same coating liquid can be applied individually to form two or more layers. Furthermore, simultaneous multilayer coating can also be performed, in which all coating liquids are applied at once to simultaneously form two or more layers. After the formation of each layer or at any stage after the formation of all layers, the layers can be smoothed using known methods such as ultracalendering or soft calendering.

[0174] B. Thermal recording medium (B)

[0175] In this invention, the thermal recording body comprises at least a base coating layer and a thermal recording layer sequentially on the support.

[0176] The base coat consists of hollow particles and a binder.

[0177] The thermal recording layer contains leuco dye, developer, and binder.

[0178] The thermal recorder comprises a compound represented by formula (1) as the first chromogenic agent of the thermal recording layer and 5-(N-3-methylphenyl-sulfonamide)-N',N”-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureo)phenyl]benzenesulfonamide as the second chromogenic agent of the thermal recording layer.

[0179] The second colorimetric agent is contained in an amount of 0.4 to 2.5 parts by mass relative to 1 part by mass of the first colorimetric agent.

[0180] support body

[0181] The support used in this embodiment may be those described in the “Support” section of “A. Thermal Recorder (A)” above.

[0182] Primer

[0183] The thermal recorder of the present invention has an undercoat layer between a support and a thermal recording layer. The undercoat layer comprises hollow particles and a binder.

[0184] hollow particles

[0185] The hollow particles used can be those described in the "Undercoat" section of "A. Thermal Recorder (A)" above, and the content of hollow particles can be set as described in the "Undercoat" section of "A. Thermal Recorder (A)" above.

[0186] adhesive

[0187] The adhesive used may be those described in the "Undercoat" section of "A. Thermal Recorder (A)" above, and the content of the adhesive may be set as described in the "Undercoat" section of "A. Thermal Recorder (A)" above.

[0188] The base coat may contain oil-absorbing pigments with an oil absorption of 70 ml / 100g or more, and particularly about 80 to 150 ml / 100g. The oil absorption is a value determined according to the method in JIS K 5101.

[0189] Oil-absorbing pigments can be any of various types. Specific examples include inorganic pigments such as calcined kaolin, amorphous silica, light calcium carbonate, and talc. These oil-absorbing pigments preferably have an average primary particle size of about 0.01 to 5 μm, and particularly about 0.02 to 3 μm. The amount of oil-absorbing pigment used can be selected from a wide range, and is generally preferably about 20 to 60% by mass, and more preferably about 25 to 55% by mass, based on the total solids content of the undercoat.

[0190] For example, a primer coating liquid is prepared by mixing hollow particles and a binder with water as a medium, along with oil-absorbing pigments and additives as needed. The coating liquid is then applied to a support and dried to form a primer coating on the support. There is no particular limitation on the amount of primer coating liquid applied, but it is preferably about 2 to 20 g / m³ based on the dried mass. 2 More preferably about 2 to 12 g / m 2 .

[0191] Examples of additives that may be included in the coating liquid for the primer layer include dispersants such as sodium dioctyl sulfosuccinate, sodium dodecylbenzene sulfonate, sodium lauryl sulfate, and fatty acid metal salts; waxes such as zinc stearate, calcium stearate, polyethylene wax, carnauba wax, paraffin wax, and ester waxes; water-resistant agents such as hydrazide compounds, boric acid, dialdehyde starch, glyoxylate, and epoxy compounds; defoamers; coloring dyes; and fluorescent dyes; etc.

[0192] thermal recording layer

[0193] Leuco dyes

[0194] The thermal recording layer of the thermal recorder of the present invention may contain any of a variety of known colorless or light-colored leuco dyes. The leuco dyes used may be those described in the "thermal recording layer" section of "A. Thermal Recorder (A)" above. The content of the leuco dye may be set as described in the "thermal recording layer" section of "A. Thermal Recorder (A)" above.

[0195] color developer

[0196] In this invention, a first colorimetric agent and a second colorimetric agent are included as colorimetric agents, and a compound represented by the above formula (1) is included as the first colorimetric agent.

[0197] The content of the first color developer is not particularly limited and can be adjusted according to the leuco dye used. Generally, the content of the first color developer relative to 1 part by weight of leuco dye is preferably 0.5 parts by weight or more, more preferably 0.8 parts by weight or more, even more preferably 1 part by weight or more, even more preferably 1.2 parts by weight or more, and particularly preferably 1.5 parts by weight or more. The content of the first color developer relative to 1 part by weight of leuco dye is also preferably 10 parts by weight or less, more preferably 5 parts by weight or less, even more preferably 4 parts by weight or less, and particularly preferably 3.5 parts by weight or less. A content of 0.5 parts by weight or more can improve recording performance. A content of 10 parts by weight or less can effectively reduce background fogging under high-temperature environments.

[0198] The second colorimetric agent comprises 5-(N-3-methylphenyl-sulfonamide)-N',N”-bis-(3-methylphenyl)-isophthalic acid diamide or N-[2-(3-phenylureo)phenyl]benzenesulfonamide. This allows for high sensitivity, excellent resistance to heat background fogging at high temperatures (especially 100°C and 110°C), and resistance to plasticizers. The second colorimetric agent is preferably 5-(N-3-methylphenyl-sulfonamide)-N',N”-bis-(3-methylphenyl)-isophthalic acid diamide.

[0199] The content of the second colorimetric agent is not particularly limited, but is approximately 0.4 to 2.5 parts by weight relative to 1 part by weight of the first colorimetric agent, preferably approximately 0.7 to 2.5 parts by weight, more preferably approximately 0.9 to 2.5 parts by weight, and even more preferably approximately 1.7 to 2.3 parts by weight. A content of 0.4 parts by weight or more of the second colorimetric agent can improve plasticizer resistance. A content of 2.5 parts by weight or less of the second colorimetric agent can improve recording performance.

[0200] The thermal recording layer may contain other colorimetric agents, as long as they do not impair the effectiveness of the present invention. Specific examples of other colorimetric agents include phenolic compounds, such as 4-tert-butylphenol, 4-acetylphenol, 4-tert-octylphenol, 4,4'-sec-butylidene diphenol, 4-phenylphenol, 4,4'-dihydroxydiphenylmethane, 4,4'-isopropylidene diphenol, 4,4'-cyclohexylidene biphenyl, 4,4'-cyclohexylidene diphenol, 1,1-bis(4-hydroxyphenyl)-ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 4,4'-bis(p-toluenesulfonylaminocarbonylamino)diphenylmethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2'-bis[4-(4-hydroxyphenyl)phenoxy]diethyl ether, 4,4'-dihydroxydiphenylmethane, etc. Benzene sulfide, 4,4'-thiobis(3-methyl-6-tert-butylphenol), 4,4'-dihydroxydiphenyl sulfone, 2,4'-dihydroxydiphenyl sulfone, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 2,4'-dihydroxydiphenyl sulfone, 4-hydroxy-4'-isopropoxydiphenyl sulfone, 4-hydroxy-4'-n-propoxydiphenyl sulfone, 4-hydroxy-4'-allyloxydiphenyl sulfone, 4-hydroxy-4'-benzyloxydiphenyl sulfone, 3,3'-diallyl-4,4'-dihydroxydiphenyl sulfone, bis(p-hydroxyphenyl)acetic acid butyl ester, bis(p-hydroxyphenyl)acetic acid methyl ester, hydroquinone monobenzyl ether, bis(3-allyl-4-hydroxyphenyl) sulfone, 4-hydroxy- 4'-Methyl diphenyl sulfone, 4-allyloxy-4'-hydroxy diphenyl sulfone, 3,4-dihydroxyphenyl-4'-methylphenyl sulfone, 4-hydroxybenzophenone, dimethyl 4-hydroxyphthalate, methyl 4-hydroxybenzoate, propyl 4-hydroxybenzoate, sec-butyl 4-hydroxybenzoate, phenyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, toluene 4-hydroxybenzoate, chlorophenyl 4-hydroxybenzoate, and 4,4'-dihydroxydiphenyl ether; aromatic carboxylic acids, such as benzoic acid, p-chlorobenzoic acid, p-tert-butylbenzoic acid, trichlorobenzoic acid, terephthalic acid, salicylic acid, 3-tert-butylsalicylic acid, 3-isopropylsalicylic acid, 3-benzyl hydroxybenzoate. Salicylic acid, 3-(α-methylbenzyl)salicylic acid, 3,5-di-tert-butylsalicylic acid, 4-[2-(p-methoxyphenoxy)ethoxy]salicylic acid, 4-[3-(p-toluenesulfonyl)propoxy]salicylic acid, 5-[p-(2-p-methoxyphenoxyethoxy]cumyl]salicylic acid, and zinc 4-[3-(p-toluenesulfonyl)propoxy]salicylic acid; salts of these phenolic compounds or aromatic carboxylic acids with polyvalent metals such as zinc, magnesium, aluminum, calcium, titanium, manganese, tin, and nickel; antipyrine complexes of zinc thiocyanate; complex zinc salts of organic acids such as terephthalic acid and other aromatic carboxylic acids; diarylureas, such as N,N'-bis[3-(p-toluenesulfonyl)oxy]phenylurea;Thiourea compounds, such as N-p-toluenesulfonyl-N'-3-(p-toluenesulfonyloxy)phenylurea, N-p-toluenesulfonyl-N'-p-butoxycarbonylphenylurea, N-p-toluenesulfonyl-N'-phenylurea, and N,N'-di-m-chlorophenylthiourea; organic compounds with -SO2NH- bonds in their molecules, such as N-(p-toluenesulfonyl)carbamate p-cumylphenyl ester, N-(p-toluenesulfonyl)carbamate p-benzyloxyphenyl ester, and N-(o-toluyl)-p-toluenesulfonamide; inorganic acidic substances, such as activated clay, attapulgite, colloidal silica, and aluminum silicate; etc.

[0201] In this invention, the thermal recording layer may further include a preservation enhancer, primarily to further enhance the preservation of the color image. The preservation enhancer used may be those described in the "thermal recording layer" section of "A. Thermal Recorder (A)" above, and the content of the preservation enhancer may be set as described in the "thermal recording layer" section of "A. Thermal Recorder (A)" above.

[0202] In this invention, the thermal recording layer may further contain a sensitizer. The use of the sensitizer improves recording sensitivity. Examples of available sensitizers include stearamide, methoxycarbonyl-N-stearamide, N-benzoylstearamide, N-eicosanoamide, ethylene bis-stearamide, benzylamide, methylene bis-stearamide, N-hydroxymethylstearamide, dibenzyl terephthalate, dimethyl terephthalate, dioctyl terephthalate, diphenyl sulfone, benzyl p-benzyloxybenzoate, phenyl 1-hydroxy-2-naphthoic acid ester, 2-naphthyl benzyl ether, m-terphenyl, p-benzyl biphenyl, di-p-chlorobenzyl oxalate, di-p-methylbenzyl oxalate, dibenzyl oxalate, p-tolyl diphenyl ether, di(p-methoxyphenoxyethyl) ether, 1,2-di(3-methylphenoxy)ethane, 1,2-di(4-methylphenoxy)ethane Alkane, 1,2-di(4-methoxyphenoxy)ethane, 1,2-di(4-chlorophenoxy)ethane, 1,2-diphenoxyethane, 1-(4-methoxyphenoxy)-2-(3-methylphenoxy)ethane, p-methylthiophenyl benzyl ether, 1,4-di(phenylthio)butane, p-acetyltoluidine, p-acetophenetidide, N-acetylacetyl-p-toluidine, 1,2-diphenoxytoluene, di(β-biphenylethoxy)benzene, p-di(ethyleneoxyethoxy)benzene, 1-isopropylphenyl-2-phenylethane, di-o-chlorobenzyl adipic acid, 1,2-bis(3,4-dimethylphenyl)ethane, 1,3-bis(2-naphthoxy)propane, biphenyl, and benzophenone, etc. Dimethyl terephthalate, 1,2-di(3-methylphenoxy)ethane, stearamide, and diphenyl sulfone are preferred, and from the viewpoint of obtaining sensitization effect without reducing heat resistance to background fogging at high temperatures, dimethyl terephthalate and 1,2-di(3-methylphenoxy)ethane are more preferred. These sensitizers can be used in combination, as long as the combination does not impair the effect of the present invention. The content of the sensitizer can be the effective amount for sensitization, and the total solid content based on the thermal recording layer is generally preferably 2 to 25% by mass, more preferably 5 to 20% by mass, and even more preferably 5 to 15% by mass.

[0203] As other components constituting the thermal recording layer, a binder may be used. Additionally, additives may be used as needed, such as pigments, crosslinking agents, waxes, metal soaps, water resistance improvers, dispersants, colored dyes, and fluorescent dyes. The binders and crosslinking agents used may be those described in the "Thermal Recording Layer" section of "A. Thermal Recorder (A)" above. The content of the binder and the crosslinking agent may be set as described in the "Thermal Recording Layer" section of "A. Thermal Recorder (A)" above.

[0204] The thermal recording layer is formed on the base layer as follows: For example, using water as the dispersion medium and employing at least one of various agitators or wet mills, such as ball mills, co-ball mills, grinders, or vertical or horizontal sand mills, a leuco dye and a color developer, along with, as needed, a sensitizer or preservation modifier, either together or separately, a water-soluble synthetic polymer such as polyacrylamide, polyvinylpyrrolidone, polyvinyl alcohol, methylcellulose, or styrene-maleic anhydride copolymer salts, and other additives such as surfactants, to form a dispersion; then, the dispersion, obtained by reducing the average particle size to 2 μm or less, is optionally mixed with pigments, binders, and additives to prepare a coating liquid for the thermal recording layer; the coating liquid for the thermal recording layer is applied to the base layer; and then dried. There is no particular limitation on the coating amount of the thermal recording layer, but for the amount of coating after drying, approximately 1 to 12 g / m² is preferred. 2 More preferably 2-10 g / m 2 Even more preferably, it is 2.5–8 g / m³. 2 And particularly preferred is 3-5.5 g / m 2 Note that, as needed, the thermal recording layer can be formed as two or more separate layers, and the composition and coating amount of each layer can be the same or different.

[0205] protective layer

[0206] As needed, the thermal recorder may include a protective layer formed on the thermal recording layer. The protective layer used may be those described in the "Protective Layer" section of "A. Thermal Recorder (A)" above.

[0207] Other layers

[0208] In this embodiment, the thermal recorder can be further processed to give it higher functionality, thereby increasing its added value. The other layers used may be those described in the "Other Layers" section of "A. Thermal Recorder (A)" above.

[0209] thermal recording device

[0210] The thermal recorder can be manufactured by forming the aforementioned layers on a support. The method for forming each layer can be the method described in the "Thermal Recorder" section of "A. Thermal Recorder (A)" above.

[0211] Example

[0212] The invention is described in more detail with reference to the embodiments. However, the invention is not limited to these embodiments. In the embodiments, unless otherwise stated, “parts” and “%” mean “parts by mass” and “% by mass”. Particle size, such as average particle size and maximum particle size, was measured using a SALD2200 laser diffraction particle size distribution analyzer (manufactured by Shimadzu Corporation). As used herein, “average particle size” refers to the median diameter (D50).

[0213] The hollow particles used in the examples and comparative examples are as follows.

[0214] Hollow Particle A: Average particle size (D50): 5.0 μm; Maximum particle size (D100): 13.5 μm; Hollowness ratio: 90%; Proportion of particles smaller than 2 μm: 0.2% by volume; Solid content concentration: 15.0%.

[0215] Hollow Particles B: Average particle size (D50): 11 μm; Maximum particle size (D100): 23 μm; Hollowness ratio: 93%; Proportion of particles smaller than 2 μm: 0% by volume; Solid content concentration: 15.0%

[0216] Hollow Particles C: Ropaque SN-1055 (manufactured by Dow); Average Particle Size (D50): 1.0 μm; Maximum Particle Size (D100): 1.8 μm; Hollowness Ratio: 55%; Solid Content Concentration: 26.5%

[0217] The average particle size (D50) and maximum particle size (D100) of these hollow particles were measured using a SALD2200 laser diffraction particle size analyzer (manufactured by Shimadzu Corporation) at refractive indices of 1.70–0.01i.

[0218] The latex used in the examples and comparative examples is as follows.

[0219] Latex A: Styrene-butadiene copolymer latex development product (Tg: -35℃; Particle size: 300nm; Solid content concentration: 48%)

[0220] Latex B: Styrene-butadiene copolymer latex development product (Tg: -10℃; Particle size: 190nm; Solid content concentration: 48%)

[0221] Latex C: Styrene-butadiene copolymer latex (trade name: L-1571, produced by Asahi Kasei Corporation; Tg: -3℃; particle size: 190nm; solid content: 48%)

[0222] The inorganic pigment II used in the examples and comparative examples is as follows.

[0223] Calcium carbonate: Trade name: Brilliant-15, manufactured by Shiraishi Kogyo Kaisha, Ltd.; Oil absorption: 56ml / 100g

[0224] Calcium carbonate: Trade name: Cal-Light-KT, manufactured by Shiraishi Kogyo Kaisha, Ltd.; Oil absorption: 120ml / 100g

[0225] Aluminum hydroxide: Trade name: Higilite H-42, manufactured by Showa Denko KK; Oil absorption: 43ml / 100g

[0226] Clay: Product name: Hydragloss 90, manufactured by KaMin LLC: Oil absorption: 46ml / 100g

[0227] Amorphous silica: Trade name: Nipsil E743, manufactured by Tosoh Silica Corporation; Oil absorption: 160ml / 100g

[0228] A. Thermal recording medium (A)

[0229] Example A1

[0230] (1) Preparation of coating liquid for primer layer

[0231] A base coat coating was prepared by mixing and stirring 100 parts of hollow granules A, 38 parts of calcined kaolin (trade name: Ansilex 93, manufactured by BASF; oil absorption: 104 ml / 100 g), 79.2 parts of latex A, 32 parts of 25% oxidized starch solution, 1.1 parts of carboxymethyl cellulose (trade name: Cellogen AG gum, manufactured by DKS Co. Ltd.) and 100 parts of water.

[0232] (2) Preparation of leuco dye dispersion (dispersion A1)

[0233] 40 parts of 3-di-(n-butyl)amino-6-methyl-7-aniline fluorane, 40 parts of a 10% aqueous solution of polyvinyl alcohol (degree of polymerization: 500, degree of saponification: 88%), and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd., a sand grinder) to an average particle size of 0.5 μm to obtain a leuco dye dispersion (dispersion A1).

[0234] (3) Preparation of colorimetric reagent dispersion (dispersion B1)

[0235] 40 parts of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, 40 parts of a 10% aqueous solution of polyvinyl alcohol (degree of polymerization: 500, degree of saponification: 88%), and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd.) to an average particle size of 1.0 μm to obtain a colorimetric reagent dispersion (dispersion B1).

[0236] (4) Preparation of sensitizer dispersion (dispersion C1)

[0237] 40 parts of 1,2-bis(3-methylphenoxy)ethane (trade name: KS-232, manufactured by Sankosha Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (degree of polymerization: 500, degree of saponification: 88%), and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd.) to an average particle size of 1.0 μm to obtain a sensitizer dispersion (dispersion C1).

[0238] (5) Preparation of coating solution for thermal recording layer

[0239] A coating solution for thermal recording layers was prepared by mixing and stirring 29.5 parts of dispersion A1, 63.6 parts of dispersion B1, 45.5 parts of dispersion C1, 70 parts of 10% fully saponified polyvinyl alcohol (trade name: PVA117, degree of saponification: 99 mol%, average degree of polymerization: 1700, manufactured by Kuraray Co., Ltd.) aqueous solution, 20.8 parts of styrene-butadiene copolymer latex (trade name: L-1571, manufactured by Asahi Kasei Corporation, solid content concentration: 48%), 20 parts of calcium carbonate (trade name: Brilliant-15, manufactured by Shiraishi Kogyo Kaisha, Ltd., oil absorption: 56 ml / 100 g), 2 parts of adipic acid dihydrazide (manufactured by Otsuka Chemical Co., Ltd.).

[0240] (6) Preparation of coating liquid for protective layer

[0241] A protective coating solution was prepared by mixing and stirring a composition comprising 317 parts of an aqueous solution of 12% diacetone-modified polyvinyl alcohol (trade name: DF-10, manufactured by Japan Vam&Poval Co., Ltd.), 60 parts of kaolin (trade name: Hydragloss 90, manufactured by KaMin LLC), 0.5 parts of polyethylene wax (trade name: Chemipearl W-400, manufactured by Mitsui Chemicals, Inc., solid content concentration: 40%), 5 parts of zinc stearate (trade name: Hidorin Z-8-36, manufactured by Chukyo Yushi Co., Ltd., solid content concentration: 36%) and 300 parts of water.

[0242] (7) Manufacturing of thermal recording devices

[0243] The coating liquid for the base layer, the coating liquid for the thermal recording layer, and the coating liquid for the protective layer were applied at a dry coating weight of 4.5 g / m². 2 3.8g / m 2 and 2.3g / m 2 Coated to a basis weight of 60 g / m 2 A high-quality paper is applied to one surface and dried to sequentially form a base coating, a thermal recording layer, and a protective layer. The resulting product is then over-calendered to smooth the surface, thus obtaining a thermal recorder.

[0244] Example A2

[0245] Except that aluminum hydroxide (trade name: Higilite H-42, manufactured by Showa Keikinzoku, oil absorption: 43 ml / 100 g) was used instead of calcium carbonate in the preparation of the coating liquid for the thermal recording layer in Example A1, the thermal recorder was obtained in the same manner as in Example A1.

[0246] Example A3

[0247] Except that in the preparation of the coating liquid for the thermal recording layer in Example A1, clay (trade name: HG90, manufactured by KaMin LLC, oil absorption: 46ml / 100g) was used instead of calcium carbonate, the thermal recorder was obtained in the same manner as in Example A1.

[0248] Example A4

[0249] Except that in the preparation of the coating liquid for the thermal recording layer in Example A1, calcium carbonate (trade name: Cal-Light-KT, manufactured by Shiraishi Kogyo Kaisha, Ltd., oil absorption: 120ml / 100g) was used instead of calcium carbonate (trade name: Brilliant-15, manufactured by Shiraishi Kogyo Kaisha, Ltd., oil absorption: 56ml / 100g), the thermal recorder was obtained in the same manner as in Example A1.

[0250] Example A5

[0251] Except that in the preparation of the base coating liquid in Example A1, 79.2 parts of latex B were used instead of 79.2 parts of latex A, the thermal recorder was obtained in the same manner as in Example A1.

[0252] Example A6

[0253] Except that in the preparation of the base coating liquid in Example A1, 79.2 parts of latex C were used instead of 79.2 parts of latex A, the thermal recorder was obtained in the same manner as in Example A1.

[0254] Example A7

[0255] Except that in the preparation of the base coating liquid in Example A1, 100 parts of hollow particles B were used instead of 100 parts of hollow particles A, the thermal recorder was obtained in the same manner as in Example A1.

[0256] Example A8

[0257] Except that in the preparation of the coating liquid for the base coating in Example A1, the amount of calcined kaolin was changed from 38 parts to 66 parts, the amount of latex A was changed from 79.2 parts to 20.8 parts, and the amount of water was changed from 100 parts to 130 parts, the thermal recorder was obtained in the same manner as in Example A1.

[0258] Example A9

[0259] Except that in the preparation of the coating liquid for the base layer in Example A1, the amount of calcined kaolin was changed from 38 parts to 66 parts, 20.8 parts of latex C was used instead of 79.2 parts of latex A, 56.6 parts of hollow particles C was used instead of 100 parts of hollow particles A, and the amount of water was changed from 100 parts to 180 parts, the thermal recorder was obtained in the same manner as in Example A1.

[0260] Comparative Example A1

[0261] Except that in the preparation of the coating liquid for the thermal recording layer in Example A1, amorphous silica (trade name: Nipsil E743, manufactured by Tosoh Silica Corporation) was used instead of calcium carbonate, the thermal recorder was obtained in the same manner as in Example A1.

[0262] Comparative Example A2

[0263] (8) Preparation of colorimetric reagent dispersion (dispersion D1)

[0264] 40 parts of 4-hydroxy-4'-isopropoxydiphenyl sulfone (trade name: D-8, manufactured by Nippon Soda Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (degree of polymerization: 500, degree of saponification: 88%), and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd.) to an average particle size of 1.0 μm to obtain a colorimetric reagent dispersion (dispersion D1).

[0265] Except that in the preparation of the coating solution for the thermal recording layer in Comparative Example A1, the chromogenic recorder was obtained in the same manner as in Comparative Example A1, except that the chromogenic dispersion D1 was used instead of the chromogenic dispersion B1.

[0266] The embodiments and comparative examples were evaluated according to the following methods. Table 1 shows the results.

[0267] Record concentration

[0268] Images were recorded on each thermal recorder using a thermal recording evaluation machine (trade name: TH-PMD, manufactured by Ohkura Electric Co., Ltd.) with applied energy of 0.13 mJ / point (halftone color density) and 0.18 mJ / point (high grayscale color density). Print density was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite). Higher values ​​indicate higher print density.

[0269] The evaluation criteria for halftone color density are as follows.

[0270] Color density above 0.90: Excellent compatibility with high-speed printing.

[0271] Colorimetric concentration less than 0.90 and above 0.80: Practical requirement

[0272] A colorimetric concentration less than 0.80 indicates low sensitivity and numerous drawbacks, such as white spots, making it problematic in practical applications.

[0273] The evaluation criteria for high grayscale colorimetric concentration are as follows.

[0274] Colorimetric concentration above 1.30: Excellent

[0275] Colorimetric concentration less than 1.30 and above 1.20: Practical requirement

[0276] Color density less than 1.20: Low print density, which is undesirable for long-term print preservation in practical use.

[0277] Images were recorded on each thermal recorder using an applied energy of 0.13 mJ / point (halftone color density) and 0.18 mJ / point (high grayscale color density) using a thermal recording evaluation machine (trade name: TH-PMD, manufactured by Ohkura Electric Co., Ltd.). After each thermal recorder was left to stand in the dark at 23°C and 50% RH for 3 months, the optical density at halftone color density and high grayscale color density was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite). Furthermore, the retention rate of the recording section was obtained according to the following equation.

[0278] Residual rate (%) = (Concentration of records after treatment / Concentration of records before treatment) × 100

[0279] The evaluation criteria are as follows.

[0280] Survival rate above 95%: Very good

[0281] Residual rate less than 95% but above 85%: Good

[0282] Survival rate less than 85% but above 80%: No real problems.

[0283] Residual rate less than 80%: The recorded concentration after treatment is low, which is problematic in practical use. 90℃ heat resistance.

[0284] Samples of each thermal recorder, developed using a label printer (trade name: L-2000, manufactured by Ishida Co., Ltd.), were left to stand in a chamber at 90°C for 1 hour. After processing, the optical density of the white paper portion was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite).

[0285] The evaluation criteria are as follows.

[0286] The concentration of the treated white paper portion is below 0.10: Excellent.

[0287] The concentration of the treated white paper portion is greater than 0.10 and less than 0.20: No problems in actual use.

[0288] The concentration of the treated white paper portion is greater than 0.20: the background fogging is too strong, which is problematic in practical use.

[0289] Table 1

[0290]

[0291] As shown in Table 1, the recording density of each thermal recorder in Examples A1 to A8 is excellent, and there are no practical problems with the long-term preservation of the prints printed with each thermal recorder in Examples A1 to A8. Although the halftone density of the thermal recorder in Example A9 is low, there are no practical problems with the long-term preservation of the prints printed with the thermal recorder in Example A9. In contrast, the long-term preservation of the prints printed with Comparative Example A1 is significantly poor. Comparative Example A2 shows excellent recording density and long-term preservation of the prints by changing the developer; however, there is a density difference in the white paper portion during the 90°C heat resistance evaluation.

[0292] B. Thermal recording medium (B)

[0293] Example B1

[0294] (1) Preparation of coating liquid for primer layer

[0295] A base coat coating solution was obtained by mixing and stirring 56.6 parts of hollow particle C, 70 parts of calcined kaolin (trade name: Ansilex 93, produced by BASF, oil absorption: 105 ml / 100 g), 22.9 parts of latex C, 12 parts of 25% oxidized starch solution, 6.7 parts of 15% fully saponified polyvinyl alcohol (trade name: PVA105, degree of saponification: 99 mol%, average degree of polymerization: 500, produced by Kuraray Co., Ltd.) aqueous solution and 80 parts of water.

[0296] (2) Preparation of leuco dye dispersion (dispersion A2)

[0297] 40 parts of 3-di-(n-butyl)amino-6-methyl-7-aniline fluorane, 40 parts of 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.), and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd., sand mill) to an average particle size of 0.5 μm to obtain a leuco dye dispersion (dispersion A2).

[0298] (3) Preparation of colorimetric reagent dispersion (dispersion B2)

[0299] 40 parts of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, 40 parts of 10% aqueous polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd., sand mill) to an average particle size of 1.0 μm to obtain a color developer dispersion (dispersion B2).

[0300] (4) Preparation of colorimetric reagent dispersion (dispersion C2)

[0301] 40 parts of 5-(N-3-methylphenyl-sulfonamide)-N',N”-bis-(3-methylphenyl)-isophthalic acid diamide, 40 parts of 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd., sand mill) to an average particle size of 1.0 μm to obtain a color developer dispersion (dispersion C2).

[0302] (5) Preparation of sensitizer dispersion (dispersion D2)

[0303] 40 parts of dimethyl terephthalate (produced by Tokyo Chemical Industry Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, produced by Kuraray Co., Ltd.), and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (produced by Imex Co., Ltd.) to an average particle size of 1.0 μm to obtain a sensitizer dispersion (dispersion D2).

[0304] (6) Preparation of coating solution for thermal recording layer

[0305] A coating solution for thermal recording layers was obtained by mixing and stirring 34.1 parts of dispersion A2, 46.7 parts of dispersion B2, 22.7 parts of dispersion C2, 35 parts of dispersion D2, 63.7 parts of a 15% aqueous solution of fully saponified polyvinyl alcohol (trade name: PVA110, degree of saponification: 99 mol%, average degree of polymerization: 1000, manufactured by Kuraray Co., Ltd.), 12.8 parts of latex C (trade name: L-1571, manufactured by Asahi Kasei Corporation, solid content concentration: 48%), 21 parts of calcium carbonate (trade name: Brilliant-15, manufactured by Shiraishi Kogyo Kaisha, Ltd., oil absorption: 56 ml / 100 g), 1 part of adipic dihydrazide (manufactured by Otsuka Chemical Co., Ltd.).

[0306] (7) Preparation of coating liquid for protective layer

[0307] A coating solution for a protective layer was obtained by mixing and stirring a composition comprising 292 parts of an aqueous solution of 12% acetoacetyl-modified polyvinyl alcohol (trade name: Gohsenx Z-200, manufactured by Nippon Synthetic Chemical Industry Co., Ltd.), 62 parts of kaolin (trade name: Hydragloss 90, manufactured by KaMin LLC), 8.3 parts of zinc stearate (trade name: Hidorin Z-9-36, manufactured by ChukyoYushi Co., Ltd., solid content concentration: 36%) and 150 parts of water.

[0308] (8) Manufacturing of thermal recording devices

[0309] The base coating liquid, the thermal recording layer coating liquid, and the protective layer coating liquid were applied at a dry coating weight of 6.5 g / m². 2 3.5g / m 2 and 2.3g / m 2 Coated to a basis weight of 60 g / m 2 A high-quality paper is applied to one surface and dried to sequentially form a base coating, a thermal recording layer, and a protective layer. The resulting product is then over-calendered to smooth the surface, thus obtaining a thermal recorder.

[0310] Example B2

[0311] Except that in the preparation of the coating liquid for the thermal recording layer in Example B1, the amount of dispersion C2 was changed from 22.7 parts to 34.1 parts, and the amount of calcium carbonate was changed from 21 parts to 16 parts, the thermal recorder was obtained in the same manner as in Example B1.

[0312] Example B3

[0313] Except that in the preparation of the coating liquid for the thermal recording layer in Example B1, the amount of dispersion C2 was changed from 22.7 parts to 45.5 parts, and the amount of calcium carbonate was changed from 21 parts to 11 parts, the thermal recorder was obtained in the same manner as in Example B1.

[0314] Example B4

[0315] Except that in the preparation of the coating liquid for the thermal recording layer in Example B1, the amount of dispersion B2 was changed from 47.7 parts to 22.7 parts, and the amount of dispersion C2 was changed from 22.7 parts to 47.7 parts, the thermal recorder was obtained in the same manner as in Example B1.

[0316] Example B5

[0317] (9) Preparation of sensitizer dispersion (dispersion E2)

[0318] 40 parts of 1,2-bis(3-methylphenoxy)ethane (trade name: KS-232, manufactured by Sankosha Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.), and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd.) to an average particle size of 1.0 μm to obtain a sensitizer dispersion (dispersion E2).

[0319] Except that in the preparation of the coating liquid for the thermal recording layer in Example B1, dispersion E2 was used instead of dispersion D2, the thermal recorder was obtained in the same manner as in Example B1.

[0320] Example B6

[0321] Except that in the preparation of the coating solution for the thermal recording layer in Example B1, 64 parts of Hymicron L-271 (main component: stearamide, produced by Chukyo Yushi Co., Ltd., solid content concentration: 25%) were used instead of 36.4 parts of dispersion D2, the thermal recorder was obtained in the same manner as in Example B1.

[0322] Example B7

[0323] (10) Preparation of sensitizer dispersion (dispersion F2)

[0324] 40 parts of diphenyl sulfone (produced by Nicca Chemical Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, produced by Kuraray Co., Ltd.), and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (produced by Imex Co., Ltd., sand mill) to an average particle size of 1.0 μm to obtain a sensitizer dispersion (dispersion F2).

[0325] Except that in the preparation of the coating liquid for the thermal recording layer in Example B1, dispersion F2 was used instead of dispersion D2, the thermal recorder was obtained in the same manner as in Example B1.

[0326] Example B8

[0327] (11) Preparation of colorimetric reagent dispersion (dispersion G2)

[0328] 40 parts of N-[2-(3-phenylureo)phenyl]benzenesulfonamide (trade name: NKK-1304, manufactured by Nippon Soda Co., Ltd.), 40 parts of 10% aqueous polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd.) to an average particle size of 1.0 μm to obtain a colorimetric reagent dispersion (dispersion G2).

[0329] Except that in the preparation of the coating liquid for the thermal recording layer in Example B1, dispersion G2 was used instead of dispersion C2, the thermal recorder was obtained in the same manner as in Example B1.

[0330] Example B9

[0331] Except that in the preparation of the coating liquid for the thermal recording layer in Example B1, the amount of dispersion B2 was changed from 47.7 parts to 22.7 parts, and 47.7 parts of dispersion G2 was used instead of 22.7 parts of dispersion C2, the thermal recorder was obtained in the same manner as in Example B1.

[0332] Example B10

[0333] Except for the following changes in the preparation of the base coat coating liquid in Example B4: 66.7 parts of hollow particles B were used instead of 56.6 parts of hollow particles C; the amount of calcined kaolin (trade name: Ansilex 93, manufactured by BASF; oil absorption: 105 ml / 100 g) was changed from 70 parts to 30 parts; the amount of latex C was changed from 22.9 parts to 95.8 parts; the amount of 25% oxidized starch solution was changed from 12 parts to 40 parts; and the amount of water was changed from 80 parts to 0 parts, the thermal recorder was obtained in the same manner as in Example B4.

[0334] Example B11

[0335] Except that in the preparation of the base coat coating liquid in Example B10, 66.7 parts of hollow particles A were used instead of 66.7 parts of hollow particles B, the thermal recorder was obtained in the same manner as in Example B10.

[0336] Example B12

[0337] Except that in the preparation of the base coat coating liquid in Example B10, 95.8 parts of latex B were used instead of 95.8 parts of latex C, the thermal recorder was obtained in the same manner as in Example B10.

[0338] Example B13

[0339] Except that in the preparation of the base coat coating liquid in Example B10, 95.8 parts of latex A were used instead of 95.8 parts of latex C, the thermal recorder was obtained in the same manner as in Example B10.

[0340] Comparative Example B1

[0341] (12) Preparation of colorimetric reagent dispersion (dispersion H2)

[0342] 40 parts of 4-hydroxy-4'-isopropoxydiphenyl sulfone (trade name: D-8, manufactured by Nippon Soda Co., Ltd.), 40 parts of 10% aqueous polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.) and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd.) to an average particle size of 1.0 μm to obtain a colorimetric reagent dispersion (dispersion H2).

[0343] Except that in the preparation of the coating liquid for the thermal recording layer in Example B1, dispersion H2 was used instead of dispersion B2, the thermal recorder was obtained in the same manner as in Example B1.

[0344] Comparative Example B2

[0345] (13) Preparation of colorimetric reagent dispersion (dispersion J2)

[0346] 40 parts of N-p-toluenesulfonyl-N'-3-(p-toluenesulfonyloxy)phenylurea (trade name: PF201, manufactured by Solenis), 40 parts of a 10% aqueous solution of polyvinyl alcohol (trade name: PVA205, degree of polymerization: 500, degree of saponification: 88%, manufactured by Kuraray Co., Ltd.), and 20 parts of water were mixed. The resulting mixture was pulverized using a sand mill (manufactured by Imex Co., Ltd.) to an average particle size of 1.0 μm to obtain a colorimetric reagent dispersion (dispersion J2).

[0347] Except that in the preparation of the coating liquid for the thermal recording layer in Example B1, dispersion J2 was used instead of dispersion B2, the amount of dispersion C2 was changed from 22.7 parts to 0 parts, and the amount of calcium carbonate was changed from 21 parts to 31 parts, the thermal recorder was obtained in the same manner as in Example B1.

[0348] Comparative Example B3

[0349] Except for changing the amount of dispersion B2 from 47.7 parts to 0 parts, the amount of dispersion C2 from 22.7 parts to 44.7 parts, and the amount of calcium carbonate from 21 parts to 31 parts in the preparation of the coating liquid for the thermal recording layer in Example B1, the thermal recorder was obtained in the same manner as in Example B1.

[0350] The embodiments and comparative examples were evaluated according to the following methods. Table 4 shows the results.

[0351] Record concentration

[0352] Images were recorded on each thermal recorder using a thermal recording evaluation machine (trade name: TH-PMD, manufactured by Ohkura Electric Co., Ltd.) with an applied energy of 0.18 mJ / point (halftone color density). Print density was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite). Higher values ​​indicate higher print density.

[0353] The evaluation criteria for halftone color density are as follows.

[0354] Color density of 1.25 or higher: Excellent compatibility with high-speed printing.

[0355] Colorimetric concentration of 1.10 or higher and less than 1.25: Practical requirement

[0356] A colorimetric concentration less than 1.10 indicates low sensitivity and numerous drawbacks, such as white spots, making it problematic in practical applications.

[0357] Images were recorded on each thermal recorder using a thermal recording evaluation machine (trade name: TH-PMD, manufactured by Ohkura Electric Co., Ltd.) with an applied energy of 0.25 mJ / point (maximum color density). Print density was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite). Higher values ​​indicate higher print density.

[0358] The evaluation criteria for the highest colorimetric concentration are as follows.

[0359] Color density of 1.40 or higher: Excellent compatibility with high-speed printing.

[0360] Colorimetric concentration of 1.30 or higher but less than 1.40: Practical requirement

[0361] Colorimetric concentration less than 1.30: low sensitivity, many defects such as white spots, and problematic plasticizer resistance in practical use.

[0362] A wrapping film (trade name: Hi-S Soft, manufactured by Nippon Carbide Industries Co., Inc.) was wrapped three times around a polycarbonate tube (diameter: 40 mm), and a thermal recorder that had been developed using a label printer (trade name: L-2000, manufactured by Ishida Co., Ltd.) was placed on the film. The wrapping film was then wrapped three more times around the thermal recorder, and the wrapped thermal recorder was left to stand at 50°C for 24 hours. After this treatment, the optical density of the recording section was measured using a spectrophotometer (X-Rite504, manufactured by X-Rite), and the retention rate was calculated as follows: Retention rate = (print density after treatment) ÷ (print density before treatment).

[0363] The evaluation criteria for the survival rate are as follows.

[0364] The residual rate after processing is over 65%: barcodes are readable and in good condition.

[0365] Residual rate after processing: 40% or more but less than 65%: Visually readable, no actual problems. Residual rate after processing: less than 40%: Printing loss, which is problematic in practical use. 100℃ heat resistance.

[0366] Samples of each thermal recorder, developed using a label printer (trade name: L-2000, manufactured by Ishida Co., Ltd.), were left to stand in a chamber at 100°C for 1 hour. After processing, the optical density of the white paper portion was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite).

[0367] The evaluation criteria are as follows.

[0368] Table 2

[0369]

[0370] Heat resistance at 110℃

[0371] Samples of each thermal recorder, developed using a label printer (trade name: L-2000, manufactured by Ishida Co., Ltd.), were left to stand in a chamber at 110°C for 1 hour. After processing, the optical density of the white paper portion was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite).

[0372] The evaluation criteria are as follows.

[0373] Table 3

[0374]

[0375] Table 4

[0376]

Claims

1. A thermal recording medium, comprising at least a base coating layer and a thermal recording layer sequentially on a support. The base coating comprises hollow particles and a binder. The thermal recording layer contains a leuco dye and a color developer. The thermal recorder contains a compound represented by the following formula (1) as the first chromogenic agent of the thermal recording layer: Where R 1 To R 5 They may be the same or different, and each represents a hydrogen atom, halogen atom, nitro group, amino group, alkyl group, alkoxy group, aryloxy group, alkyl carbonyloxy group, aryl carbonyloxy group, alkyl carbonyl amino group, aryl carbonyl amino group, alkyl sulfonyl amino group, aryl sulfonyl amino group, monoalkyl amino group, dialkyl amino group, or aryl amino group. The thermal recorder meets the following requirements: The thermal recording layer contains 5-(N-3-methylphenyl-sulfonamide)-N',N”-bis-(3-methylphenyl)-isophthalic acid diamide as a second colorimetric agent, and contains the second colorimetric agent in an amount of 0.4 to 2.5 parts by mass relative to 1 part by mass of the first colorimetric agent.

2. The thermal recorder according to claim 1, wherein the compound represented by formula (1) is at least one selected from the group consisting of 3-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate, 2-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate and 4-[(phenylcarbamoyl)amino]phenyl-4-methylbenzenesulfonate.

3. The thermal recorder according to claim 1, wherein the second colorimetric agent is contained in an amount of 0.9 to 2.5 parts by mass relative to 1 part by mass of the first colorimetric agent.

4. The thermal recording device according to claim 1, wherein the thermal recording layer comprises at least one sensitizer selected from the group consisting of dimethyl terephthalate, 1,2-di(3-methylphenoxy)ethane, stearamide and diphenyl sulfone.

5. The thermal recorder according to claim 1, wherein the maximum particle size D100 of the hollow particles is 10~30 μm and the average particle size D50 is 4.0~15 μm, the ratio of the maximum particle size D100 to the average particle size D50 D100 / D50 is 1.8~3.0, and the volume percentage of hollow particles with a particle size of 2.0 μm or less is 1% or less.

6. The thermal recorder according to any one of claims 1 to 5, wherein the hollow particle has a hollowness of 80% to 98%.

7. The thermal recorder according to any one of claims 1 to 5, wherein the content of the hollow particles is from 5% to 40% by mass based on the total solid content of the undercoating layer.

8. The thermal recorder according to any one of claims 1 to 5, wherein the binder of the undercoat comprises a binder resin having a glass transition temperature of -10°C or less.

Citation Information

Patent Citations

  • Thermal recording medium

    JP7072130B1

  • Heat-sensitive recording material

    JP2021100798A

  • Thermosensitive recording medium

    JP2021171990A

  • Heat sensitive recording material with non-phenolic color developers