Packaging material for battery cell, preparation method of packaging material, secondary battery and electric device
By using the interpenetrating polymer network coating coated with the substrate surface in the secondary battery, the problem of insufficient thermal conductivity of Mylar film is solved, the thermal dissipation and safety of the battery are improved, and the circulation and fast charging performance are improved.
Patent Information
- Application Number
- CN202310638236.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
In the existing secondary batteries, due to insufficient thermal conductivity of the Mylar film, poor heat dissipation is caused, which reduces battery life and has potential safety risks, limiting the development of battery technology.
The substrate surface is coated with an interpenetrating polymer network coating, and the coating material includes a first epoxy resin, a second epoxy resin, a curing agent and a modified thermal conductivity filler, with a thermal conductivity coefficient of ≥0.6W/(m·k). To improve the battery's heat dissipation performance and safety.
By improving the heat dissipation performance, the circulation performance, fast charging performance and safety of the secondary battery are improved, the battery life is extended, and the safety risks are reduced.
Smart Images

Figure CN119069900A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a packaging material for a battery cell and a preparation method thereof, a secondary battery and an electrical device. Background Art
[0002] Secondary batteries are widely used in various consumer electronic products and electric vehicles due to their outstanding features such as light weight, no pollution, and no memory effect. In related technologies, Mylar (polyester film) is usually used to wrap bare battery cells to prevent direct contact between the core and the aluminum shell, which plays an insulating role. Due to the poor thermal conductivity of Mylar film, heat dissipation is hindered, resulting in reduced battery life and potential safety issues, limiting the further development of battery technology. Summary of the invention
[0003] Based on this, it is necessary to provide a packaging material for a battery cell and a preparation method thereof, a secondary battery and an electrical device, so that the heat generated in the secondary battery can be discharged in time to improve the cycle performance and safety of the secondary battery.
[0004] In order to achieve the above-mentioned object, the first aspect of the present application provides a packaging material for a battery cell, comprising:
[0005] substrate; and
[0006] A coating layer is coated on at least one surface of the substrate, wherein the material of the coating layer comprises an interpenetrating polymer network, and the interpenetrating polymer network comprises a first epoxy resin, a second epoxy resin, a curing agent, and a modified thermally conductive filler containing an epoxy group;
[0007] The thermal conductivity of the coating is ≥0.6 W / (m·k).
[0008] The packaging material for the battery cell of the present application includes a substrate and a coating, and the material of the coating includes an interpenetrating polymer network, and the interpenetrating polymer network includes a first epoxy resin, a second epoxy resin, a curing agent and a modified thermally conductive filler containing an epoxy group, which can make the coating have excellent physical and chemical stability; because the interpenetrating polymer network has a high cross-linking density and a multi-ring structure, the coating can have good electrolyte resistance and insulation properties; and the modified thermally conductive filler can make the coating have thermal conductivity, and the thermal conductivity coefficient of the coating is ≥0.6W / (m·k), which can quickly conduct the heat generated during the charging and discharging of the bare battery cell through the coating, thereby improving the cycle performance, fast charging performance and safety of the battery; and the modified thermally conductive filler and the epoxy resin polymer system are firmly bonded by chemical bonds, the adhesion between the polymer and the modified thermally conductive filler is improved, and the interface scattering of phonons is reduced.
[0009] In some embodiments, the first epoxy resin includes one or more of a trifunctional epoxy resin, a bisphenol A epoxy resin, a bisphenol F epoxy resin, a bisphenol S epoxy resin, a hydantoin epoxy resin, an o-cresol epoxy resin, a phenol novolac epoxy resin, a BPA novolac epoxy resin, a phenoxy resin, a biphenyl phenol epoxy resin, and an anthracene epoxy resin;
[0010] Optionally, the first epoxy resin includes a trifunctional epoxy resin;
[0011] Further optionally, the first epoxy resin comprises a trifunctional epoxy resin having a number average molecular weight of 2000-2700 and an epoxy equivalent of 244 g / eq-314 g / eq;
[0012] More optionally, the first epoxy resin comprises a trifunctional epoxy resin having the following structural formula:
[0013]
[0014] Among them, 6≤X≤8.
[0015] In some embodiments, the second epoxy resin includes one or more of pyrogallol triglycidyl ether epoxy resin, glycidylamine epoxy resin, trisphenol methane triglycidyl ether epoxy resin and aliphatic epoxy resin;
[0016] Optionally, the second epoxy resin comprises an aliphatic epoxy resin;
[0017] Further optionally, the second epoxy resin comprises an aliphatic epoxy resin having an epoxy equivalent of 190 g / eq-273 g / eq;
[0018] More optionally, the second epoxy resin comprises an aliphatic epoxy resin having the following structural formula:
[0019]
[0020] Among them, 35≤m+n≤43, 8≤m≤11.
[0021] In some embodiments, the mass ratio of the second epoxy resin to the first epoxy resin is (0.12-0.4):1; optionally, (0.12-0.3):1.
[0022] In some embodiments, the modified thermally conductive filler has at least one of the following characteristics:
[0023] (1) The modified thermally conductive filler comprises one or more of aluminum nitride, boron nitride, silicon carbide, aluminum oxide, magnesium oxide and zinc oxide surface-modified by a first silane coupling agent, wherein the first silane coupling agent contains an epoxy group;
[0024] Optionally, the first silane coupling agent includes 3-glycidylpropyltrimethoxysilane coupling agent;
[0025] (2) The modified thermally conductive filler includes one or more of a nano-scale modified thermally conductive filler and a micro-scale modified thermally conductive filler;
[0026] Optionally, the volume particle size distribution Dv50 of the nano-scale modified thermally conductive filler is 100nm-400nm; the volume particle size distribution Dv50 of the micron-scale modified thermally conductive filler is 1μm-20μm;
[0027] Optionally, the modified thermally conductive filler comprises the nano-scale modified thermally conductive filler and the micro-scale modified thermally conductive filler in a mass ratio of 1:(0.125-0.8); further optionally, the modified thermally conductive filler comprises the nano-scale modified thermally conductive filler and the micro-scale modified thermally conductive filler in a mass ratio of 1:(0.28-0.5);
[0028] (3) The ratio of the mass of the modified thermally conductive filler to the total mass of the first epoxy resin and the second epoxy resin is (0.37-0.95):1; optionally, it is (0.47-0.85):1.
[0029] In some embodiments, the curing agent has at least one of the following characteristics:
[0030] (1) The curing agent includes one or more of diethylaminopropylamine, isophorone diamine, meta-xylylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, methylhexahydrophthalic anhydride, polyamide and xylylenediamine condensate;
[0031] Optionally, the curing agent includes m-xylylenediamine;
[0032] (2) The mass of the first epoxy resin is denoted as m1, the mass of the second epoxy resin is denoted as m2, and the mass of the curing agent is denoted as m3. The mass of the first epoxy resin, the mass of the second epoxy resin and the mass of the curing agent satisfy: m3 = active hydrogen equivalent of the curing agent × (m1 / epoxy equivalent of the first epoxy resin + m2 / epoxy equivalent of the second epoxy resin) × A, 1.1≤A≤1.2.
[0033] In some embodiments, the material of the coating further includes a second silane coupling agent;
[0034] Optionally, the second silane coupling agent has at least one of the following characteristics:
[0035] (1) the second silane coupling agent includes one or more of an amino-type silane coupling agent, an epoxy-type silane coupling agent, a vinyl-type silane coupling agent, an acyloxy-type silane coupling agent, an isocyanate-type silane coupling agent, a mercapto-type silane coupling agent, and a urea-type silane coupling agent;
[0036] (2) The ratio of the mass of the second silane coupling agent to the total mass of the first epoxy resin and the second epoxy resin is (0.5-3):53.
[0037] In some embodiments, the coating material further comprises a leveling agent;
[0038] Optionally, the leveling agent includes one or more of a polydimethylsiloxane leveling agent, a polyether-modified siloxane leveling agent, a polymethylalkylsiloxane leveling agent, a hydroxyl-reactive polysiloxane leveling agent, an epoxy-reactive polysiloxane leveling agent, an alkyl-reactive polysiloxane leveling agent, and a polyacrylate leveling agent;
[0039] Optionally, the mass ratio of the leveling agent to the second silane coupling agent is (0.05-0.5):(0.5-3).
[0040] In some embodiments, the coating material further comprises a defoaming agent;
[0041] Optionally, the defoamer includes one or more of a mineral oil defoamer, a polydimethylsiloxane defoamer, a polyether-modified polydimethylsiloxane defoamer, a polyurea defoamer and a polyamide defoamer;
[0042] Optionally, the mass ratio of the defoaming agent to the second silane coupling agent is (0.05-0.5):(0.5-3).
[0043] In some embodiments, the coating has a thickness of 20 μm-100 μm.
[0044] In some embodiments, the raw materials for preparing the coating include, by weight:
[0045] 38-47 parts of the first epoxy resin, 6-15 parts of the second epoxy resin, 7-9 parts of the curing agent, 20-50 parts of the modified thermal conductive filler, 0.5-3 parts of the second silane coupling agent, 0.05-0.5 parts of the leveling agent and 0.05-0.5 parts of the defoaming agent.
[0046] In some embodiments, the substrate includes one of a metal shell material, a hard plastic shell material, and an aluminum-plastic film.
[0047] In some embodiments, the coating further comprises at least one of the following features:
[0048] (1) The insulation resistance of the coating is ≥4 GΩ;
[0049] (2) The adhesion of the coating on the surface of the substrate is level 0 or level 1;
[0050] (3) The coating does not crack when bent 45° on a shaft with a curvature diameter of 32 mm;
[0051] (4) The coating is resistant to an electrolyte containing a carbonate solvent.
[0052] The second aspect of the present application provides a method for preparing the battery cell packaging material of the first aspect of the present application, comprising the following steps:
[0053] preparing a mixture including the first epoxy resin, the second epoxy resin, the modified thermally conductive filler, and a solvent;
[0054] The mixture and the curing agent are mixed and coated on one side surface of the substrate, and then baked to prepare the battery cell packaging material;
[0055] The elastic modulus of the first epoxy resin is 0.5 GPa-3 GPa, the dielectric constant is 2.5-4, and the elongation at break of the second epoxy resin is 150%-400%.
[0056] In some embodiments, the preparation method includes at least one of the following conditions:
[0057] (1) The fineness of the mixture is ≤20 μm;
[0058] (2) The baking temperature is 120°C-180°C, and the baking time is 10min-30min;
[0059] (3) The solvent includes one or more of an ester solvent, a ketone solvent, an alcohol solvent, an alcohol ether solvent, an ether solvent, an aromatic hydrocarbon solvent and an alkane solvent.
[0060] In some embodiments, the method for preparing the modified thermally conductive filler comprises the following steps:
[0061] In an acidic environment, mixing a thermally conductive filler and a first silane coupling agent and then performing a modification treatment to prepare the modified thermally conductive filler;
[0062] Optionally, the pH value of the acidic environment is 4-5;
[0063] Optionally, the temperature of the modification treatment is 20°C-30°C, and the time of the modification treatment is 30min-40min;
[0064] Optionally, the mass ratio of the thermally conductive filler to the first silane coupling agent is 50:(0.5-1).
[0065] A third aspect of the present application provides a secondary battery, comprising:
[0066] Battery cells; and
[0067] The packaging material for encapsulating the battery cell is selected from the battery cell packaging material of the first aspect of the present application, and the side of the battery cell packaging material having the coating is adjacent to the battery cell.
[0068] In some embodiments, the battery cell includes a heat dissipation tab, and the heat dissipation tab is inserted into the coating.
[0069] A fourth aspect of the present application provides an electrical device, comprising the secondary battery of the third aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Figure 1 is a schematic diagram of a secondary battery according to one embodiment of the present application.
[0071] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown.
[0072] Figure 3 Schematic diagram of an electrical device using a secondary battery according to an embodiment of the present application as a power source.
[0073] Description of reference numerals:
[0074] 1 secondary battery; 11 housing; 12 electrode assembly; 13 cover plate; 2 power-consuming device. DETAILED DESCRIPTION
[0075] In order to facilitate the understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0076] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0077] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0078] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0079] In this application, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left endpoint and the right endpoint are the same. For example, 10-1000nm means that the units of the left endpoint "10" and the right endpoint "1000" are both nm (nanometers).
[0080] In this application, "multiple", "multiple", "multiple times" and the like, unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "multiple" means greater than or equal to two. Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unambiguous range; and any lower limit can be combined with other lower limits to form an unambiguous range, and similarly any upper limit can be combined with any other upper limit to form an unambiguous range. In addition, each separately disclosed point or single value itself can be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unambiguous range.
[0081] The "range" disclosed in this application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values.
[0082] The temperature parameters in this application, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range of instrument control.
[0083] In the related art, Mylar film is used to wrap the bare battery cell. However, due to the poor thermal conductivity of the Mylar film, heat dissipation is hindered, resulting in reduced battery life and potential safety issues.
[0084] Based on the above problems, the present application prepares a coating including an interpenetrating polymer network on the surface of a substrate to replace the Mylar film in the related art. The interpenetrating polymer network can make the coating have excellent physical and chemical stability; the interpenetrating polymer network has a high cross-linking density and a polycyclic structure, which can make the coating have good electrolyte resistance and insulation properties; and the raw materials for preparing the interpenetrating polymer network include modified thermally conductive fillers, which can make the coating have thermal conductivity, and can quickly conduct the heat generated during the charging and discharging of the bare battery cell through the coating, thereby improving the battery's cycle performance, fast charging performance and safety.
[0085] A first aspect of the present application provides a packaging material for a battery cell, comprising a substrate and a coating coated on at least one surface of the substrate; the material of the coating comprises an interpenetrating polymer network, the interpenetrating polymer network comprises a first epoxy resin, a second epoxy resin, a curing agent and a modified thermally conductive filler containing epoxy groups; the thermal conductivity of the coating is ≥0.6W / (m·k).
[0086] It should be noted that the interpenetrating polymer network refers to a polymer blend composed of two or more polymer networks that are cross-linked and interpenetrate each other.
[0087] The coating can be located on one side of the substrate or on both sides of the substrate; when the coating is provided on both sides of the substrate, an insulating layer can also be provided on the outer side of the coating away from the battery cell in actual use. In this application, "battery cell packaging material" refers to the material used to encapsulate the electrode assembly formed by the positive electrode sheet, the negative electrode sheet and the separator. It can be used for lithium-ion batteries and sodium-ion batteries; it can be used for liquid batteries and solid-state batteries.
[0088] In this application, "first epoxy resin", "second epoxy resin", etc. are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features.
[0089] During the coating preparation process, under heating conditions, the active hydrogen contained in the curing agent can open the epoxy groups in the first epoxy resin, the second epoxy resin and the modified thermally conductive filler, causing an addition reaction to crosslink and cure the first epoxy resin, the second epoxy resin and the modified thermally conductive filler.
[0090] Understandably, the packaging material for the battery cell of the present application includes a substrate and a coating, the material of the coating includes an interpenetrating polymer network, the interpenetrating polymer network includes a first epoxy resin, a second epoxy resin, a curing agent and a modified thermally conductive filler containing an epoxy group, which can make the coating have excellent physical and chemical stability; since the interpenetrating polymer network has a high cross-linking density and a polycyclic structure, the coating can have good electrolyte resistance and insulation properties; and the modified thermally conductive filler can make the coating have thermal conductivity, and the thermal conductivity of the coating is ≥0.6W / (m·k), which can quickly conduct the heat generated during the charging and discharging of the bare battery cell through the coating, thereby improving the cycle performance, fast charging performance and safety of the battery; and the modified thermally conductive filler and the epoxy resin polymer system are firmly bonded by chemical bonds, the adhesion between the polymer and the modified thermally conductive filler is improved, and the interface scattering of phonons is reduced
[0091] As an example, the thermal conductivity of the coating mentioned above can be measured by the following method: using a thermal constant analyzer, testing according to ASTM D5470 standard, testing 5 pieces of packaging materials for the battery cells to be tested, and taking the average value.
[0092] In some embodiments, the first epoxy resin includes one or more of a trifunctional epoxy resin, a bisphenol A epoxy resin, a bisphenol F epoxy resin, a bisphenol S epoxy resin, a hydantoin epoxy resin, an o-cresol epoxy resin, a phenol novolac epoxy resin, a BPA novolac epoxy resin, a phenoxy resin, a biphenyl phenol epoxy resin, and an anthracene epoxy resin.
[0093] In some optional embodiments, the first epoxy resin includes a trifunctional epoxy resin. When a trifunctional epoxy resin is used as the first epoxy resin, the adhesion between the coating and the substrate can be improved, the crosslinking density of the coating after curing can be increased, and the electrolyte resistance and insulation performance of the coating can be improved.
[0094] In some optional embodiments, the first epoxy resin includes a trifunctional epoxy resin having a number average molecular weight of 2000-2700 and an epoxy equivalent of 244g / eq-314g / eq; for example, the number average molecular weight of the trifunctional epoxy resin can be but is not limited to 2000, 2030, 2050, 2080, 2100, 2130, 2150, 2180, 2200, 2230, 2250, 2270, 2300, 2330, 2350, 2380, 2400, 2430, 2450, 2480, 2500, 2530, 2550, 2570, 2600, 2630, 2650, 2680, 2700 or a range between any two of the above values. As an example, the epoxy equivalent of the trifunctional epoxy resin can be, but is not limited to, 244 g / eq, 250 g / eq, 260 g / eq, 270 g / eq, 280 g / eq, 290 g / eq, 300 g / eq, 310 g / eq, 314 g / eq, or a range between any two of the above values. When the number average molecular weight of the trifunctional epoxy resin is lower than the above range, the coating may have poor flexibility; when the number average molecular weight of the trifunctional epoxy resin is higher than the above range, the viscosity is high, which is not conducive to the leveling of the coating.
[0095] As a possible implementation, the first epoxy resin includes a trifunctional epoxy resin having the following structural formula:
[0096]
[0097] Among them, 6≤X≤8.
[0098] In some embodiments, the second epoxy resin includes one or more of pyrogallol triglycidyl ether epoxy resin, glycidyl amine epoxy resin, trisphenol methane triglycidyl ether epoxy resin, and aliphatic epoxy resin.
[0099] In some optional embodiments, the second epoxy resin includes an aliphatic epoxy resin. When an aliphatic epoxy resin is used as the second epoxy resin, the flexibility of the coating can be improved to meet the deformation requirements during battery charging and discharging.
[0100] In some optional embodiments, the second epoxy resin includes an aliphatic epoxy resin having an epoxy equivalent of 190 g / eq-273 g / eq; for example, the epoxy equivalent of the aliphatic epoxy resin may be, but is not limited to, 190 g / eq, 193 g / eq, 200 g / eq, 210 g / eq, 220 g / eq, 230 g / eq, 240 g / eq, 248 g / eq, 250 g / eq, 256 g / eq, 260 g / eq, 270 g / eq, 273 g / eq or a range between any two of the above values. If the epoxy equivalent of the aliphatic epoxy resin is higher than the above range, the crosslinking density of the interpenetrating polymer network may be too low, which is not conducive to improving the electrolyte resistance of the coating; if the epoxy equivalent of the aliphatic epoxy resin is lower than the above range, the crosslinking density of the interpenetrating polymer network may be too high, which is not conducive to meeting the flexibility requirements of the coating.
[0101] In some optional embodiments, the second epoxy resin includes an aliphatic epoxy resin having the following structural formula:
[0102]
[0103] Among them, 35≤m+n≤43, 8≤m≤11.
[0104] In some possible embodiments, the mass ratio of the second epoxy resin to the first epoxy resin is (0.12-0.4):1; for example, it can be but not limited to 0.12:1, 0.15:1, 0.18:1, 0.2:1, 0.23:1, 0.25:1, 0.28:1, 0.3:1, 0.33:1, 0.35:1, 0.38:1, 0.4:1 or a range between any two of the above ratios. When the mass ratio of the second epoxy resin to the first epoxy resin is lower than the above range, the flexibility of the coating will be insufficient, and the deformation during the battery charging and discharging process may cause the coating to crack, resulting in reduced battery performance and even safety problems; when the mass ratio of the second epoxy resin to the first epoxy resin is higher than the above range, the coating's resistance to electrolyte corrosion will be reduced, and the coating is easily corroded by the electrolyte, which may cause the bare battery to be in direct contact with the substrate, which may cause the battery to short-circuit and cause safety problems. Optionally, the mass ratio of the second epoxy resin to the first epoxy resin is (0.12-0.3):1.
[0105] As a possible implementation, the modified thermally conductive filler includes one or more of aluminum nitride, boron nitride, silicon carbide, aluminum oxide, magnesium oxide and zinc oxide surface-modified by a first silane coupling agent, wherein the first silane coupling agent contains an epoxy group. Optionally, the modified thermally conductive filler is modified silicon carbide.
[0106] It should be noted that the "first silane coupling agent" mentioned in the present application is only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can it be understood as implicitly indicating the importance or quantity of the indicated technical features.
[0107] After the first silane coupling agent is hydrolyzed, a silanol group (Si-OH) can be formed. The silanol group can condense with the hydroxyl group on the surface of the thermally conductive filler to form a permanent connection. The surface of the thermally conductive filler is modified by the first silane coupling agent containing an epoxy group, so that the thermally conductive filler can carry an epoxy group, so that the modified thermally conductive filler can participate in the ring-opening and chain extension reactions of the epoxy resin polymer system, and is convenient for participating in the formation of an interpenetrating polymer network. The strong bonding between the filler and the epoxy resin polymer system is ensured by chemical bonds, the adhesion between the polymer and the thermally conductive filler is improved, and the interface scattering of phonons is reduced; and the surface-modified thermally conductive filler can reduce the thermal contact resistance and improve the thermal conductivity of the thermally conductive filler.
[0108] In some optional embodiments, the first silane coupling agent includes 3-glycidylpropyltrimethoxysilane coupling agent.
[0109] In some embodiments, the modified thermally conductive filler includes one or more of a nano-scale modified thermally conductive filler and a micro-scale modified thermally conductive filler. The nano-scale modified thermally conductive filler and the micro-scale modified thermally conductive filler are compounded, and the nano-scale modified thermally conductive filler particles can be filled between the micro-scale modified thermally conductive filler particles and overlapped to form a thermally conductive path, thereby improving the thermal conductivity.
[0110] In some optional embodiments, the volume particle size distribution Dv50 of the nano-scale modified thermal conductive filler is 100nm-400nm; for example, it can be but not limited to 100nm, 130nm, 150nm, 170nm, 200nm, 230nm, 250nm, 270nm, 300nm, 330nm, 350nm, 380nm, 400nm or a range between any two of the above values. When the volume particle size distribution Dv50 of the nano-scale modified thermal conductive filler is within the above range, it is conducive to being dispersed in the gaps of the micron-scale modified thermal conductive filler particles. The volume particle size distribution Dv50 of the micron-sized modified thermally conductive filler is 1μm-20μm; for example, it can be but not limited to 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm or the range between any two of the above values. When the volume particle size distribution Dv50 of the micron-sized modified thermally conductive filler is higher than the above range, the coating surface may be uneven and the pole piece may be easily scratched; when the volume particle size distribution Dv50 of the micron-sized modified thermally conductive filler is lower than the above range, the thermal conductivity of the coating may be reduced.
[0111] It should be noted that Dv50 is the value at which 50% of the total volume of the modified thermally conductive filler has a diameter greater than this value, and 50% of the total volume of the particle modified thermally conductive filler has a diameter less than this value. Dv50 represents the median particle size of the modified thermally conductive filler.
[0112] Unless otherwise specified, the modified thermally conductive filler particle size distribution parameter Dv50 determined by the particle size distribution measurement value in this application is determined by a particle size analyzer-laser diffraction method. Specifically, reference can be made to the standard GB / T19077-2016, using a laser diffraction scattering particle size analyzer (such as the Mastersizer 2000E laser particle size analyzer of Malvern Instruments Ltd., UK), and the measurement is performed according to the manufacturer's instructions.
[0113] In some optional embodiments, the modified thermally conductive filler includes a nano-scale modified thermally conductive filler and a micro-scale modified thermally conductive filler in a mass ratio of 1:(0.125-0.8); for example, the mass ratio of the nano-scale modified thermally conductive filler and the micro-scale modified thermally conductive filler in the modified thermally conductive filler can be, but is not limited to, 1:0.125, 1:0.15, 1:0.18, 1:0.2, 1:0.23, 1:0.25, 1:0.28, 1:0. 3. 1:0.33, 1:0.35, 1:0.38, 1:0.4, 1:0.42, 1:0.45, 1:0.47, 1:0.5, 1:0.53, 1:0.55, 1:0.57, 1:0.6, 1:0.63, 1:0.65, 1:0.68, 1:0.7, 1:0.72, 1:0.75, 1:0.78, 1:0.8 or the range between any two of the above ratios. When the mass ratio of the nano-scale modified thermally conductive filler to the micron-scale modified thermally conductive filler in the modified thermally conductive filler is within the above range, the nano-scale silicon carbide particles have better filling and overlapping effects between the micron-scale silicon carbide particles, which is conducive to further improving the thermal conductivity of the coating. Optionally, the modified thermally conductive filler includes a nano-scale modified thermally conductive filler and a micro-scale modified thermally conductive filler in a mass ratio of 1:(0.28-0.5).
[0114] In some embodiments, the ratio of the mass of the modified thermally conductive filler to the total mass of the first epoxy resin and the second epoxy resin is (0.37-0.95):1; for example, it can be but is not limited to 0.37:1, 0.4:1, 0.43:1, 0.45:1, 0.47:1, 0.5:1, 0.52:1, 0.55:1, 0.57:1, 0.6:1, 0.63:1, 0.65:1, 0.67:1, 0.7:1, 0.73:1, 0.75:1, 0.77:1, 0.8:1, 0.83:1, 0.85:1, 0.87:1, 0.9:1, 0.93:1, 0.95:1 or a range between any two of the above ratios. When the ratio of the mass of the modified thermally conductive filler to the total mass of the first epoxy resin and the second epoxy resin is within the above range, it is conducive to forming a dense coating, so that the coating has good electrolyte corrosion resistance and insulation performance, and the modified thermally conductive filler can be fully overlapped inside the coating to form a thermally conductive path. When the amount of the modified thermally conductive filler is higher than the above range, it may cause the epoxy resin to be unable to completely wrap the modified thermally conductive filler, which may cause the gap around the thermally conductive filler to be too large to be eroded by the electrolyte, resulting in gaps, accelerating the destruction of the coating, and then causing the coating's electrolyte corrosion resistance, thermal conductivity and insulation performance to be reduced. When the amount of the modified thermally conductive filler is lower than the above range, it may cause the modified thermally conductive filler to be unable to form a thermally conductive path inside the coating, which may cause the thermal conductivity of the coating to be significantly reduced. Optionally, the ratio of the mass of the modified thermally conductive filler to the total mass of the first epoxy resin and the second epoxy resin is (0.47-0.85):1.
[0115] In some embodiments, the curing agent includes one or more of diethylaminopropylamine, isophorone diamine, meta-xylylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, methylhexahydrophthalic anhydride, polyamide and condensate of xylylenediamine. Optionally, the curing agent is meta-xylylenediamine.
[0116] The curing agent provides active hydrogen to open the epoxy group, causing an addition reaction, thereby causing the first epoxy resin, the second epoxy resin and the modified thermally conductive filler to crosslink and cure.
[0117] In some embodiments, the mass of the first epoxy resin is denoted as m1, the mass of the second epoxy resin is denoted as m2, and the mass of the curing agent is denoted as m3. The mass of the first epoxy resin, the mass of the second epoxy resin and the mass of the curing agent satisfy: m3 = active hydrogen equivalent of the curing agent × (m1 / epoxy equivalent of the first epoxy resin + m2 / epoxy equivalent of the second epoxy resin) × A, 1.1≤A≤1.2.
[0118] It should be noted that the mass of the curing agent is higher than the total amount of curing agent required for the first epoxy resin and the second epoxy resin, and the amount of the modified thermally conductive filler is small, so the amount of curing agent added can also meet the demand for the modified thermally conductive filler.
[0119] In some embodiments, the material of the coating further includes a second silane coupling agent; the second silane coupling agent facilitates the adhesion between the coating and the substrate.
[0120] In some possible embodiments, the second silane coupling agent includes one or more of an amino silane coupling agent, an epoxy silane coupling agent, a vinyl silane coupling agent, an acyloxy silane coupling agent, an isocyanate silane coupling agent, a mercapto silane coupling agent, and a urea silane coupling agent.
[0121] It should be noted that when the second silane coupling agent includes an epoxy silane coupling agent, the epoxy group in the epoxy silane coupling agent can participate in the formation of an interpenetrating polymer network; and after the epoxy silane coupling agent is hydrolyzed, a silanol group (Si-OH) can be formed, and the silanol group can form a hydrogen bond with the surface of the substrate, so that the adhesion between the coating and the substrate is higher.
[0122] In some possible embodiments, the ratio of the mass of the second silane coupling agent to the total mass of the first epoxy resin and the second epoxy resin is (0.5-3):53; for example, it can be but not limited to 0.5:53, 0.8:53, 1:53, 1.3:53, 1.5:53, 1.8:53, 2:53, 2.3:53, 2.5:53, 2.8:53, 3:53 or a range between any two of the above ratios. When the ratio of the mass of the second silane coupling agent to the total mass of the first epoxy resin and the second epoxy resin is lower than the above range, it may not be conducive to improving the adhesion between the coating and the substrate; when the ratio of the mass of the second silane coupling agent to the total mass of the first epoxy resin and the second epoxy resin is higher than the above range, too much second silane coupling agent may exist in the coating as a small molecule, which is not conducive to improving the overall performance of the coating, and is easy to cause material waste and increase costs.
[0123] In some embodiments, the coating material further includes a leveling agent; adding the leveling agent can make the coating more flat, smooth, and uniform.
[0124] As a possible implementation, the leveling agent includes one or more of a polydimethylsiloxane type leveling agent, a polyether modified siloxane type leveling agent, a polymethylalkylsiloxane type leveling agent, a hydroxyl reactive polysiloxane type leveling agent, an epoxy reactive polysiloxane type leveling agent, an alkyl reactive polysiloxane type leveling agent and a polyacrylate type leveling agent.
[0125] As a possible embodiment, the mass ratio of the leveling agent and the second silane coupling agent is (0.05-0.5): (0.5-3); for example, it can be but not limited to (0.05-0.45): (0.5-2.5), (0.1-0.4): (1-2.5), (0.15-0.35): (1-2), (0.2-0.3): (1.5-2), (0.25-0.3): (1-1.5), etc. When the mass ratio of the leveling agent and the second silane coupling agent is lower than the above range, it may be unfavorable for the leveling of the coating and the wetting and bonding of the substrate; when the mass ratio of the leveling agent and the second silane coupling agent is higher than the above range, it may be unfavorable for the defoaming of the coating. In some embodiments, the material of the coating also includes a defoaming agent; by adding a defoaming agent, the coating can be made flat and free of bubbles.
[0126] In some possible implementations, the defoamer includes one or more of a mineral oil defoamer, a polydimethylsiloxane defoamer, a polyether-modified polydimethylsiloxane defoamer, a polyurea defoamer, and a polyamide defoamer.
[0127] In some possible embodiments, the mass ratio of the defoamer to the second silane coupling agent is (0.05-0.5):(0.5-3); for example, it may be, but is not limited to, (0.05-0.45):(0.5-2.5), (0.1-0.4):(1-2.5), (0.15-0.35):(1-2), (0.2-0.3):(1.5-2), (0.25-0.3):(1-1.5), etc. When the mass ratio of the defoamer to the second silane coupling agent is higher than the above range, too much defoamer may exist in the coating as a small molecule, which is not conducive to improving the overall performance of the coating; when the mass ratio of the defoamer to the second silane coupling agent is lower than the above range, it is not conducive to defoaming of the coating.
[0128] In some embodiments, the thickness of the coating is 20 μm-100 μm; for example, it can be but not limited to 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm, 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm, 100 μm or the range between any two of the above values. When the thickness of the coating is within the above range, it can replace the mylar film, and at the same time, it can make the coating surface smooth and not easy to scratch the pole piece.
[0129] It should be noted that the thickness of the coating layer can be measured by the following method: CP slices are made on the cell packaging material, and the thickness of the coating layer is measured by a scanning electron microscope (SEM).
[0130] In some embodiments, the raw materials for preparing the coating include, by weight: 38-47 parts of a first epoxy resin, 6-15 parts of a second epoxy resin, 7-9 parts of a curing agent, 20-50 parts of a modified thermally conductive filler, 0.5-3 parts of a second silane coupling agent, 0.05-0.5 parts of a leveling agent, and 0.05-0.5 parts of a defoaming agent.
[0131] The weight proportion of the first epoxy resin contained in the coating preparation raw material is 38-47 parts; for example, it can be but not limited to 38 parts, 39 parts, 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, 45 parts, 46 parts, 47 parts or a range between any two of the above values.
[0132] The weight proportion of the second epoxy resin contained in the coating preparation raw material is 6-15 parts; for example, it can be but not limited to 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts or a range between any two of the above values.
[0133] The weight proportion of the curing agent contained in the coating preparation raw material is 7-9 parts; for example, it can be but not limited to 7 parts, 7.5 parts, 8 parts, 8.5 parts, 9 parts or a range between any two of the above values.
[0134] The weight proportion of the modified thermally conductive filler contained in the coating preparation raw material is 20-50 parts; for example, it can be but not limited to 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts or a range between any two of the above values.
[0135] The weight proportion of the second silane coupling agent contained in the coating preparation raw material is 0.5-3 parts; for example, it can be but not limited to 0.5 parts, 0.7 parts, 1 parts, 1.3 parts, 1.5 parts, 1.8 parts, 2 parts, 2.3 parts, 2.5 parts, 2.8 parts, 3 parts or a range between any two of the above values.
[0136] The weight proportion of the leveling agent contained in the coating preparation raw material is 0.05-0.5 parts; for example, it can be but not limited to 0.05 parts, 0.1 parts, 0.15 parts, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts or the range between any two of the above values.
[0137] The weight proportion of the defoaming agent contained in the coating preparation raw materials is 0.05-0.5 parts; for example, it can be but not limited to 0.05 parts, 0.1 parts, 0.15 parts, 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, 0.4 parts, 0.45 parts, 0.5 parts or the range between any two of the above values.
[0138] In some embodiments, the substrate includes one of a metal shell material, a hard plastic shell material, and an aluminum-plastic film. The coating can be used in square shell batteries or soft pack batteries.
[0139] In some embodiments, the insulation resistance of the coating is ≥ 4 GΩ; the insulation performance of the coating is excellent.
[0140] As an example, the insulation resistance of the coating mentioned above can be measured by the following method: use a Hioki DC withstand voltage insulation resistance tester, place the packaging material of the battery cell to be tested on an insulating table, place conductive cotton with an area smaller than the coating area in the middle of the coating, connect the negative electrode to the aluminum plate, and place the positive electrode on the conductive cotton. Set the resistance value module parameters to DC1000V, 60s, test 5 pieces of packaging materials for the battery cells to be tested, and take the average value.
[0141] In some embodiments, the adhesion of the coating on the substrate surface is level 0 or level 1; the bonding strength between the coating and the substrate is high.
[0142] By way of example, the adhesion of the above-mentioned coatings to the substrate surface can be determined in accordance with DIN EN ISO 2409.
[0143] In some embodiments, the coating does not crack when bent 45° on a mandrel with a curvature diameter of 32 mm; the coating has excellent flexibility.
[0144] As an example, the flexibility of the coating mentioned above can be tested according to GB / T 6742-86 standard, meeting the requirement of bending 45° on a 32 mm curvature diameter shaft.
[0145] In some embodiments, the coating is resistant to electrolytes containing carbonate-based solvents.
[0146] As an example, the tolerance of the above-mentioned coating to the electrolyte can be determined by the following method: prepare the electrolyte with ethylene carbonate (EC), dimethyl carbonate (DMC) and lithium hexafluorophosphate (LiPF6) in a mass ratio of 35:55:10; place the packaging material of the battery cell to be tested in the bottle containing the electrolyte until the sample is completely immersed, then seal it and place it in an oven at 85°C. After 7 days, take it out, wipe it clean with a paper towel, place it at room temperature for 4 hours, and observe it visually.
[0147] The second aspect of the present application provides a method for preparing the battery cell packaging material of the first aspect, comprising the following steps: preparing a mixture comprising a first epoxy resin, a second epoxy resin, a modified thermal conductive filler and a solvent; mixing the mixture with a curing agent and coating the mixture on one side surface of a substrate, and baking the mixture to prepare the battery cell packaging material;
[0148] The elastic modulus of the first epoxy resin is 0.5 GPa-3 GPa, the dielectric constant is 2.5-4, and the elongation at break of the second epoxy resin is 150%-400%.
[0149] The elastic modulus of the first epoxy resin at 25°C is 0.5GPa-3GPa; for example, it can be but not limited to 0.5GPa, 0.7GPa, 1GPa, 1.3GPa, 1.5GPa, 1.7GPa, 2GPa, 2.2GPa, 2.5GPa, 2.7GPa, 3GPa or a range between any two of the above values. The dielectric constant of the first epoxy resin at 25°C is 2.5-4; for example, it can be but not limited to 2.5, 2.6, 2.7, 2.8, 2.9, 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4 or a range between any two of the above values. When the elastic modulus and dielectric constant of the first epoxy resin are respectively within the above ranges, the obtained interpenetrating polymer network can have better strength and insulation.
[0150] The elongation at break of the second epoxy resin at 25° C. is 150%-400%; for example, it may be, but not limited to, 150%, 180%, 200%, 220%, 250%, 280%, 300%, 330%, 350%, 380%, 400%, or a range between any two of the above values. When the elongation at break of the second epoxy resin is within the above range, the interpenetrating polymer network prepared can have suitable flexibility to meet the requirement of deformation of the packaging material during battery charging and discharging.
[0151] It can be understood that by using raw materials including a first epoxy resin, a second epoxy resin, a curing agent and a modified thermally conductive filler containing an epoxy group to carry out epoxy ring-opening and chain extension reactions, chain-shaped, cyclic and other molecular chains are formed, and the molecular chains are interspersed with each other and tightly connected to each other through chemical crosslinking points to form an interpenetrating polymer network on the surface of the substrate, so that the coating has excellent physical and chemical stability; since the interpenetrating polymer network has a high crosslinking density and a multi-ring structure, the coating can have good electrolyte resistance and insulation properties; since the preparation raw materials include modified thermally conductive fillers, the coating can have thermal conductivity, and the heat generated during the charging and discharging of the bare battery cell can be quickly conducted away through the coating, thereby improving the battery's cycle performance, fast charging performance and safety. In addition, since the elastic modulus of the first epoxy resin is 0.5GPa-3GPa, the dielectric constant is 2.5-4, and the elongation at break of the second epoxy resin is 150%-400%, the coating can have better strength and insulation while having suitable flexibility, which can meet the deformation requirements of the packaging material during battery charging and discharging.
[0152] The method for preparing the battery cell packaging material provided in the present application has a simple process and is convenient for industrial application.
[0153] It can be understood that during the preparation process of the battery cell packaging material, the first epoxy resin, the second epoxy resin, the curing agent and the modified thermally conductive filler containing epoxy groups all participate in the chemical reaction. Therefore, the structures of the first epoxy resin, the second epoxy resin, the curing agent and the modified thermally conductive filler contained in the interpenetrating polymer network of the coating are partially changed from the structures of the first epoxy resin, the second epoxy resin, the curing agent and the modified thermally conductive filler added when preparing the battery cell packaging material.
[0154] It should be noted that after the mixture and the curing agent are mixed, they can be applied to one side surface of the substrate by spraying, screen printing, flow coating or dipping.
[0155] In some embodiments, the fineness of the mixture is ≤20 μm; for example, it can be, but not limited to, 1 μm, 3 μm, 5 μm, 8 μm, 10 μm, 13 μm, 15 μm, 18 μm, 20 μm, or a range between any two of the above values. The fineness of the mixture affects the thickness of the coating. When the fineness of the mixture is within the above range, it can be helpful to control the coating to have a suitable thickness.
[0156] In some embodiments, the baking temperature is 120°C-180°C; for example, it can be but not limited to 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C, 180°C or the range between any two of the above values. The baking time is 10min-30min; for example, it can be but not limited to 10min, 13min, 15min, 18min, 20min, 23min, 25min, 28min, 30min or the range between any two of the above values.
[0157] In some embodiments, the solvent includes one or more of an ester solvent, a ketone solvent, an alcohol solvent, an alcohol ether solvent, an ether solvent, an aromatic hydrocarbon solvent, and an alkane solvent.
[0158] In some embodiments, the method for preparing the modified thermally conductive filler comprises the following steps: in an acidic environment, mixing the thermally conductive filler and the first silane coupling agent and then performing a modification treatment to prepare the modified thermally conductive filler.
[0159] In some possible embodiments, the pH value of the acidic environment is 4-5; for example, it can be 4, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5 or a range between any two of the above values.
[0160] In some possible embodiments, the temperature of the modification treatment is 20°C-30°C; for example, it can be but not limited to 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C or the range between any two of the above values. The time of the modification treatment is 30min-40min; for example, it can be but not limited to 30min, 31min, 32min, 33min, 34min, 35min, 36min, 37min, 38min, 39min, 40min or the range between any two of the above values.
[0161] In some possible embodiments, the mass ratio of the thermally conductive filler to the first silane coupling agent is 50:(0.5-1); for example, it can be but not limited to 50:0.5, 50:0.6, 50:0.7, 50:0.8, 50:0.9, 50:1 or a range between any two of the above values.
[0162] The third aspect of the present application provides a secondary battery, comprising: a battery cell and a packaging material for encapsulating the battery cell, wherein the packaging material is selected from the battery cell packaging material of the first aspect of the present application, and the side of the battery cell packaging material having the coating is adjacent to the battery cell.
[0163] In some embodiments, the battery cell includes a heat dissipation tab, which is inserted into the coating. The contact area between the heat dissipation tab and the coating can be increased, and a solid heat conduction path is formed between the heat dissipation tab and the coating, thereby improving the heat conduction efficiency.
[0164] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0165] Positive electrode
[0166] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes the positive electrode active material of the first aspect of the present application.
[0167] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0168] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc. The polymer material substrate includes but is not limited to one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE).
[0169] In some embodiments, the lithium ion positive electrode active material may include positive electrode active materials for batteries that are well known in the art. As an example, the positive electrode active material may include at least one of the following materials: lithium phosphates containing olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries can also be used. These positive electrode active materials can be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05O2) and its modified compounds, etc. Examples of lithium-containing phosphates with olivine structure may include, but are not limited to, lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. The weight ratio of the positive electrode active material in the positive electrode film layer is 80-100% by weight, based on the total weight of the positive electrode film layer.
[0170] As an example, the sodium ion positive electrode active material may include at least one of the following materials: at least one of a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound. However, the present application is not limited to these materials, and other conventionally known materials that can be used as sodium ion battery positive electrode active materials may also be used.
[0171] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. The sodium transition metal oxide is, for example, Na x MO2, wherein M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.
[0172] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds with anionic units. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si; n represents (YO4) n- valence state.
[0173] Polyanionic compounds can also be those with sodium ions, transition metal ions, tetrahedral (YO4) n- A class of compounds containing anion units and halogen anions. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si, and n represents (YO4) n- valence state; the halogen may be at least one of F, Cl and Br.
[0174] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedral unit (ZO y ) m+ and an optional halogen anion. Y can be at least one of P, S and Si, and n represents (YO4)n- valence state; Z represents a transition metal, which may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; m represents (ZO y ) m+ valence state; the halogen may be at least one of F, Cl and Br.
[0175] Polyanionic compounds include NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2 (P2O7), NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VO y )2(PO4)2F 3-2y At least one of (0≤y≤1).
[0176] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ). The transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds are, for example, Na a Me b Me' c (CN)6, wherein Me and Me' are each independently at least one of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.
[0177] In some embodiments, the positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. The weight ratio of the binder in the positive electrode film layer is 0-20% by weight, based on the total weight of the positive electrode film layer.
[0178] In some embodiments, the positive electrode film layer may further include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. The weight ratio of the conductive agent in the positive electrode film layer is 0-20% by weight, based on the total weight of the positive electrode film layer.
[0179] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry, wherein the positive electrode slurry has a solid content of 40-80wt%, and the viscosity at room temperature is adjusted to 5000-25000mPa·s, and the positive electrode slurry is coated on both sides of the positive electrode collector, and after drying, the positive electrode sheet is formed by cold rolling; the unit surface density of the positive electrode powder coated on one side is 15-35mg / m 2 The compaction density of the positive electrode is 3.0-3.6g / cm 3 , optional: 3.3-3.5g / cm 3 The calculation formula of the compacted density is:
[0180] Compacted density = coating surface density / (thickness of the electrode after extrusion - thickness of the current collector).
[0181] Negative electrode
[0182] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.
[0183] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0184] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc., and the polymer material substrate includes but is not limited to polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE) and other substrates.
[0185] In some embodiments, the negative electrode active material may adopt the negative electrode active material for batteries known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more. The weight ratio of the negative electrode active material in the negative electrode film layer is 70-100% by weight, based on the total weight of the negative electrode film layer.
[0186] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS). The weight ratio of the binder in the negative electrode film layer is 0-30% by weight, based on the total weight of the negative electrode film layer.
[0187] In some embodiments, the negative electrode film layer may further include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. The weight ratio of the conductive agent in the negative electrode film layer is 0-20 weight %, based on the total weight of the negative electrode film layer.
[0188] In some embodiments, the negative electrode film layer may further include other additives, such as a thickener (such as sodium carboxymethyl cellulose (CMC-Na)), etc. The weight ratio of the other additives in the negative electrode film layer is 0-15% by weight, based on the total weight of the negative electrode film layer.
[0189] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry, wherein the solid content of the negative electrode slurry is 30-70wt%, and the viscosity at room temperature is adjusted to 2000-10000mPa·s; the obtained negative electrode slurry is coated on the surfaces of both sides of the negative electrode current collector, and after a drying process, cold pressing such as rolling, a negative electrode sheet is obtained. The unit surface density of the negative electrode powder coated on one side is 75-220mg / m 2 , the compaction density of negative electrode is 1.2-2.0g / m 3 .
[0190] Electrolytes
[0191] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.
[0192] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0193] In some embodiments, the electrolyte salt may be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP). The concentration of the electrolyte salt is generally 0.5-5 mol / L.
[0194] In some embodiments, the solvent can be selected from one or more of fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), cyclopentane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).
[0195] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0196] Isolation film
[0197] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0198] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0199] In some embodiments, the isolation film has a thickness of 6-40 μm, and optionally 12-20 μm.
[0200] In some embodiments, the positive electrode sheet, the negative electrode sheet and the separator can be made into an electrode assembly by a winding process or a lamination process; and the electrode assembly and the electrolyte are packaged using the battery cell packaging material of the first aspect of the present application.
[0201] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 1 is a square structure as an example.
[0202] In some embodiments, reference Figure 2 The outer package may include a shell 11 and a cover plate 13. The shell 11 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 11 has an opening connected to the receiving cavity, and the cover plate 13 can be covered on the opening to close the receiving cavity.
[0203] The positive electrode sheet, the negative electrode sheet and the separator can be wound or laminated to form an electrode assembly 12. The electrode assembly 12 is encapsulated in the housing cavity. The electrolyte is infiltrated in the electrode assembly 12. The number of electrode assemblies 12 contained in the lithium-ion battery 1 can be one or more, which can be adjusted according to demand.
[0204] In some embodiments, secondary batteries may be assembled into a battery module. The battery module may contain multiple secondary batteries, and the specific number may be adjusted according to the application and capacity of the battery module.
[0205] In the battery module, the plurality of secondary batteries may be arranged in sequence along the length direction of the battery module. Of course, they may also be arranged in any other manner. Further, the plurality of lithium-ion batteries may be fixed by fasteners.
[0206] Optionally, the battery module may further include a housing having an accommodation space, and the plurality of secondary batteries are accommodated in the accommodation space.
[0207] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0208] The battery pack may include a battery box and a plurality of battery modules disposed in the battery box. The battery box includes an upper box body and a lower box body, and the upper box body can be covered on the lower box body to form a closed space for accommodating the battery modules. The plurality of battery modules can be arranged in the battery box in any manner.
[0209] Electrical devices
[0210] In a fourth aspect, the present application provides an electrical device, which includes at least one of the secondary battery, battery module or battery pack of the third aspect of the present application. The secondary battery, battery module or battery pack can be used as a power source for the device, or as an energy storage unit for the device. The device may be, but is not limited to, a mobile device, an electric vehicle, an electric train, a ship and a satellite, an energy storage system, etc.; wherein the mobile device may include, but is not limited to, at least one of a mobile phone, a laptop computer, etc.; the electric vehicle may include, but is not limited to, at least one of a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.
[0211] The device can select a secondary battery, a battery module or a battery pack according to its usage requirements.
[0212] Figure 3 The power consumption device 2 is taken as an example. The power consumption device 2 is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the high power and high energy density requirements of the device for the secondary battery, a battery pack or a battery module can be used.
[0213] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a lithium-ion battery may be used as a power source.
[0214] The beneficial effects of the present application are further illustrated below with reference to the embodiments.
[0215] In order to make the technical problems, technical solutions and beneficial effects solved by the present application clearer, the following will be further described in detail with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work belong to the scope of protection of the present application.
[0216] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0217] 1. Preparation of packaging materials for battery cells
[0218] Example 1
[0219] Acetic acid was dripped into 100g pure water, and the pH value of the water was adjusted to 4.5 to obtain acidic water, and then 0.5g of 3-glycidylpropyltrimethoxysilane (as the first silane coupling agent) was added to the acidic water, and stirred for 15min until a transparent homogeneous solution was obtained. Then 50g of silicon carbide was added to the above homogeneous solution, stirred for 30min until a uniform dispersion state was obtained, filtered, and dried in an oven at 120°C for 2h to obtain modified silicon carbide (as a modified thermal conductive filler).
[0220] 3g of aliphatic epoxy resin (as the second epoxy resin), 50g of trifunctional epoxy resin (as the first epoxy resin), and 15g of isophorone (as the solvent) are mixed, placed in a sealed stainless steel heating container, heated to 50°C, and stirred for 2h until the solid is completely dissolved to obtain a mixed solution of aliphatic epoxy resin and trifunctional epoxy resin, and then the mixed solution, 30g of nano-modified silicon carbide, 0.1g of polyether-modified polydimethylsiloxane (as a leveling agent), 0.1g of dimethylpolysiloxane containing fumed silica (as a defoaming agent), and 1.8g of 3-glycidylpropyltrimethoxysilane (as the second silane coupling agent) are poured into a vacuum sand mill in sequence, fully ground and evacuated to a uniform bubble-free state, and the fineness is ≤20μm, to obtain an intermediate component;
[0221] The intermediate component was mixed with m-xylylenediamine (as a curing agent) in a weight ratio of 100:10, the mixture was sprayed onto the inner wall of the laser-treated aluminum shell, and then baked at 120° C. for 30 minutes to obtain a packaging material for a battery cell.
[0222] Among them, the structural formula of trifunctional epoxy resin is: x=7, epoxy equivalent is 275 g / eq, number average molecular weight is 2320, elastic modulus is 1.64 GPa, and dielectric constant is 3.2;
[0223] The structural formula of aliphatic epoxy resin is m=8, n=30; epoxy equivalent weight is 273g / eq, elongation at break is 312%;
[0224] The volume particle size distribution Dv50 of the nano-scale modified silicon carbide is 100 nm.
[0225] Example 2-24
[0226] The preparation method of the battery cell packaging material in Examples 2-24 is basically similar to the preparation method of the battery cell packaging material in Example 1, with the main differences being: at least one of the type and / or amount of the first epoxy resin, the type and / or amount of the second epoxy resin, the type and / or amount of the modifier, the type and / or amount of the curing agent, the type and / or amount of the second silane coupling agent, the type and / or amount of the leveling agent, the type and / or amount of the defoaming agent, the type of the substrate, and the coating thickness.
[0227] It should be noted that the structural formula of the trifunctional epoxy resin in Example 20 is: x=6, epoxy equivalent is 314 g / eq, number average molecular weight is 2630, elastic modulus is 1.72 GPa, and dielectric constant is 3.3;
[0228] The structural formula of aliphatic epoxy resin is m=11, n=25; epoxy equivalent is 193 g / eq, and elongation at break is 292%.
[0229] The structural formula of the trifunctional epoxy resin in Example 21 is: x=8, epoxy equivalent is 244 g / eq, number average molecular weight is 2010, elastic modulus is 1.60 GPa, and dielectric constant is 3.1;
[0230] The structural formula of aliphatic epoxy resin is m=10, n=33; epoxy equivalent is 248 g / eq, and elongation at break is 347%.
[0231] The structural formula of the trifunctional epoxy resin in Example 22 is: x=8, epoxy equivalent is 244 g / eq, number average molecular weight is 2010, elastic modulus is 1.60 GPa, and dielectric constant is 3.1;
[0232] The structural formula of aliphatic epoxy resin is m=9, n=31; epoxy equivalent is 256 g / eq, and elongation at break is 323%.
[0233] In Example 23, the elastic modulus of the o-cresol-formaldehyde epoxy resin is 1.65 GPa, and the dielectric constant is 3.0; the elongation at break of the pyrogallol triglycidyl ether epoxy resin is 156%.
[0234] In Example 24, the elastic modulus of the BPA novolac epoxy resin is 1.77 GPa, and the dielectric constant is 3.1; the elongation at break of the trisphenol methane triglycidyl ether epoxy resin is 153%.
[0235] Comparative Example 1
[0236] The preparation method of the battery cell packaging material in Comparative Example 1 is substantially similar to the preparation method of the battery cell packaging material in Example 1, with the main difference being that aliphatic epoxy resin of the same mass is used to replace the trifunctional epoxy resin, and the rest are the same.
[0237] Comparative Example 2
[0238] The preparation method of the battery cell packaging material in Comparative Example 2 is substantially similar to the preparation method of the battery cell packaging material in Example 1, with the main difference being that a trifunctional epoxy resin of the same mass is used to replace the aliphatic epoxy resin, and the rest are the same.
[0239] The parameter settings in Examples 1-13 are shown in Table 1-1, and the parameter settings in Examples 14-24 and Comparative Example 1-2 are shown in Table 1-2.
[0240]
[0241]
[0242] Among them, s1 represents the mass ratio of the first epoxy resin to the second epoxy resin; s2 represents the mass ratio of the nano-scale modified thermally conductive filler to the micron-scale modified thermally conductive filler; s3 represents the ratio of the mass of the modified thermally conductive filler to the total mass of the first epoxy resin and the second epoxy resin; the dimethyl polysiloxane contains fumed silica, purchased from Degussa, model number is Foamex N; the polyether modified polydimethylsiloxane is purchased from BYK Chemical, model number is BYK-346.
[0243] It should be noted that the thickness of the coating mentioned in Table 1 is measured by the following method: CP slices are made on the packaging material for the battery cell, and the thickness of the coating is measured by a scanning electron microscope (SEM).
[0244] 2. Performance test of packaging materials for battery cells
[0245] 1. Electrolyte resistance test
[0246] The electrolyte was prepared according to the mass ratio of ethylene carbonate (EC), dimethyl carbonate (DMC) and lithium hexafluorophosphate (LiPF6) of 35:55:10; the packaging material of the battery cell to be tested was placed in the bottle containing the electrolyte until the sample was completely immersed, and then sealed and placed in an oven at 85°C. After 7 days, it was taken out and wiped clean with a paper towel. After being placed at room temperature for 4 hours, it was visually observed. The results are shown in Table 2.
[0247] 2. Thermal conductivity test
[0248] The Hot Disk 520 thermal constant analyzer was used to test 5 pieces of packaging materials for the battery cells to be tested in accordance with the ASTM D5470 standard. The average value was taken and the results are shown in Table 2.
[0249] 3. Insulation impedance test
[0250] Using Hioki ST 5680 DC withstand voltage insulation resistance tester, take the packaging material of the battery cell to be tested and place it on the insulating table, place the conductive cotton with an area smaller than the coating area in the middle of the coating, connect the negative electrode to the aluminum plate, and place the positive electrode on the conductive cotton. Set the resistance value module parameters to DC 1000V, 60s, test 5 pieces of packaging materials for the battery cell to be tested, and take the average value. The results are shown in Table 2.
[0251] 4. Adhesion test
[0252] The test was carried out according to DIN EN ISO 2409 standard and the results are shown in Table 2.
[0253] 5. Flexibility test
[0254] The test was carried out according to GB / T 6742-86 standard, meeting the requirement of 32mm curvature diameter shaft bending 45°. The results are shown in Table 2.
[0255] Table 2
[0256]
[0257]
[0258] From the results of Examples 1-24 and Comparative Examples 1-2 in Table 2, it can be seen that by preparing an interpenetrating polymer network using raw materials including both a first epoxy resin and a second epoxy resin, the electrolyte resistance, insulation performance and flexibility of the coating can be improved simultaneously.
[0259] The difference between Examples 1-6 lies in the different mass ratios of the second epoxy resin and the first epoxy resin, with the mass ratio between the two being the smallest in Example 1 and the largest in Example 6; the coating cracked in Example 1, indicating that when the amount of the second epoxy resin is too small, the coating has poor flexibility; the coating swelled in Example 6, indicating that when the amount of the first epoxy resin is small, the coating has poor electrolyte resistance.
[0260] The difference between Example 4 and Examples 7-14 is that the amount of modified thermally conductive filler is different. The amount of modified thermally conductive filler in Example 7 is the least, and the amount of modified thermally conductive filler in Example 14 is the most. Compared with the results of Example 4 and Example 8-13, the thermal conductivity in Example 7 is too small, and the insulation resistance is the largest. The technicians analyzed that the reason may be that the amount of modified thermally conductive filler is too small, and a thermal conductive path cannot be formed inside the coating, which may cause the thermal conductivity of the coating to be significantly reduced. At the same time, due to the small amount of modified thermally conductive filler, when other components are set the same, the relative amount of epoxy resin in the coating may be large, thereby improving the insulation performance of the coating. The coating in Example 14 cracked. The technicians analyzed that the reason may be that the amount of modified thermally conductive filler is too large. When other components are set the same, the relative amounts of the two epoxy resins in the coating may be small, respectively, resulting in poor flexibility of the coating, which cannot meet the deformation requirements of battery charging and discharging.
[0261] The difference between Example 12 and Examples 15-19 is that the usage ratio of the nano-scale modified thermally conductive filler and the micron-scale modified thermally conductive filler is different. In Example 12, the nano-scale modified thermally conductive filler is completely used, and in Example 19, the usage of the micron-scale modified thermally conductive filler is the largest; compared with Examples 15-18, the thermal conductivity coefficients in Examples 12 and 19 are both reduced, indicating that when the mass ratio of the nano-scale modified thermally conductive filler and the micron-scale modified thermally conductive filler in the modified thermally conductive filler is in the range of 1:(0.125-0.8), the filling and overlapping effects of the nano-scale silicon carbide particles between the micron-scale silicon carbide particles are better, which is beneficial to further improve the thermal conductivity of the coating.
[0262] It should be noted that after the coating swells in contact with the electrolyte, it is easy to fall off, which may cause the positive and negative electrodes to directly contact the metal shell and cause a short circuit. When the filler in the coating precipitates, the filler particles may be embedded in the positive and negative active materials, resulting in a decrease in battery capacity; or the filler particles may pierce the diaphragm to cause direct contact between the positive and negative electrodes, causing a short circuit; or the filler particles may block the pores of the diaphragm, resulting in a decrease in the passage rate of lithium ions and a decrease in battery performance. After the coating cracks, the positive and negative electrodes may directly contact the metal shell and cause a short circuit. Therefore, the above-mentioned packaging materials for battery cells with swollen or cracked coatings cannot be used in battery production in actual processes.
[0263] 3. Preparation of secondary batteries
[0264] Preparation of lithium-ion batteries
[0265] 1. Preparation of positive electrode sheet
[0266] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1O2 (NCM811), binder polyvinylidene fluoride (PVDF), and conductive agent acetylene black are dissolved in solvent N-methylpyrrolidone (NMP) in a mass ratio of 97:1.5:1.5, and are fully stirred and mixed to prepare positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode collector aluminum foil, and then dried, cold pressed, and cut to obtain positive electrode sheets.
[0267] 2. Preparation of negative electrode sheet
[0268] Graphite, sodium carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), and conductive carbon are added to a certain amount of deionized water, with the mass ratio of graphite, sodium carboxymethyl cellulose, styrene butadiene rubber and conductive agent being 90:2:3:5. The mixture is stirred to form a uniform slurry with a viscosity controlled at 3000 mPa·S to 10000 mPa·S. The slurry is coated on copper foil and dried to form a negative electrode sheet.
[0269] 3. Isolation film
[0270] A polyethylene film (PE) with a thickness of 12 μm was used as the separator.
[0271] 4. Preparation of electrolyte
[0272] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte. In the electrolyte, the concentration of LiPF6 is 1 mol / L.
[0273] The positive electrode sheet, separator and negative electrode sheet are stacked in order, and the separator is placed between the positive and negative electrode sheets to play an isolating role. The above electrolyte is added, and the battery cells in Examples 1-24 and Comparative Examples 1-2 are respectively assembled into laminated lithium-ion batteries using packaging materials.
[0274] In Comparative Example 3, Mylar film was used to replace the coating, as follows:
[0275] 1. Preparation of positive electrode sheet
[0276] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2 (NCM811), binder polyvinylidene fluoride (PVDF), and conductive agent acetylene black are dissolved in solvent N-methylpyrrolidone (NMP) in a mass ratio of 97:1.5:1.5, and are fully stirred and mixed to prepare positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode collector aluminum foil, and then dried, cold pressed, and cut to obtain positive electrode sheets.
[0277] 2. Preparation of negative electrode sheet
[0278] Graphite, sodium carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR), and conductive carbon are added to a certain amount of deionized water, with the mass ratio of graphite, sodium carboxymethyl cellulose, styrene butadiene rubber and conductive agent being 90:2:3:5. The mixture is stirred to form a uniform slurry with a viscosity controlled at 3000 mPa·S to 10000 mPa·S. The slurry is coated on copper foil and dried to form a negative electrode sheet.
[0279] 3. Isolation film
[0280] A polyethylene film (PE) with a thickness of 12 μm was used as the separator.
[0281] 4. Preparation of electrolyte
[0282] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then LiPF6 is uniformly dissolved in the above solution to obtain an electrolyte. In the electrolyte, the concentration of LiPF6 is 1 mol / L.
[0283] 5. Preparation of battery cells
[0284] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, and the separator is placed between the positive and negative electrode sheets to play an isolating role. The positive electrode sheet, the separator, and the negative electrode sheet are packaged with a Mylar film, and the above-mentioned electrolyte is added into the Mylar film, and then assembled into a laminated lithium-ion battery in an aluminum shell.
[0285] 4. Secondary battery performance test
[0286] 1. Rate performance test
[0287] The battery cell was charged to 4.35V and then discharged to 2.0V at currents of 0.33, 1C, 3C, and 5C for 3 cycles. The same process was then used to perform rate tests at currents of 0.33, 1C, 3C, and 5C for 3 weeks each. The performance percentage at each current and 0.33C rate was recorded.
[0288] 2. Cycle performance
[0289] The battery cell is charged to 4.35V at 3C current, and then discharged to 2.0V at 3C current, and this cycle is repeated for 200 weeks; the capacity retention rate is the ratio of the discharge capacity in each week to the discharge capacity in the first week.
[0290] The performance test results of the secondary batteries in the above embodiments and comparative examples are shown in Table 3 below.
[0291] Table 3
[0292]
[0293]
[0294] From the comparison of the results of Examples 1-24 and Comparative Examples 1-3 in Table 3, it can be seen that the use of the battery cell packaging material of the present application can improve the cycle performance and fast charging performance of the secondary battery.
[0295] The difference between Examples 1-6 is that the mass ratio of the second epoxy resin to the first epoxy resin is different. From the comparison of the results of Examples 1-6, it can be seen that the battery cell packaging material prepared when the mass ratio of the second epoxy resin to the first epoxy resin is (0.12-0.4):1 can improve the cycle performance and fast charging performance of the secondary battery.
[0296] The difference between Example 4 and Example 7-14 is that the amount of modified thermally conductive filler used is different. By comparing the results of Example 4 and Example 7-14, it can be seen that when the ratio of the mass of the modified thermally conductive filler to the total mass of the first epoxy resin and the second epoxy resin is in the range of (0.37-0.95):1, the battery cell packaging material prepared can improve the cycle performance and fast charging performance of the secondary battery.
[0297] The difference between Example 12 and Examples 15-19 is that the usage ratio of the nano-scale modified thermally conductive filler and the micron-scale modified thermally conductive filler is different. From the comparison of the results of Examples 12 and Examples 15-19, it can be seen that the battery cell packaging material prepared when the mass ratio of the nano-scale modified thermally conductive filler and the micron-scale modified thermally conductive filler in the modified thermally conductive filler is in the range of 1:(0.125-0.8) can improve the cycle performance and fast charging performance of the secondary battery.
[0298] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0299] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.
Claims
1. A packaging material for a battery cell, It is characterized in that include: Base material; as well as A coating layer is coated on at least one surface of the substrate, wherein the material of the coating layer comprises an interpenetrating polymer network, and the interpenetrating polymer network comprises a first epoxy resin, a second epoxy resin, a curing agent, and a modified thermally conductive filler containing an epoxy group; The thermal conductivity of the coating is ≥0.6 W / (m·k).
2. The battery cell packaging material according to claim 1, It is characterized in that The first epoxy resin includes one or more of trifunctional epoxy resin, bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, hydantoin epoxy resin, o-cresol epoxy resin, phenol novolac epoxy resin, BPA novolac epoxy resin, phenoxy resin, biphenyl phenol epoxy resin and anthracene epoxy resin; Optionally, the first epoxy resin includes a trifunctional epoxy resin; Further optionally, the first epoxy resin comprises a trifunctional epoxy resin having a number average molecular weight of 2000-2700 and an epoxy equivalent of 244 g / eq-314 g / eq; More optionally, the first epoxy resin comprises a trifunctional epoxy resin having the following structural formula: Among them, 6≤X≤8.
3. The battery cell packaging material according to any one of claims 1 to 2, It is characterized in that The second epoxy resin comprises one or more of pyrogallol triglycidyl ether epoxy resin, glycidylamine epoxy resin, trisphenol methane triglycidyl ether epoxy resin and aliphatic epoxy resin; Optionally, the second epoxy resin comprises an aliphatic epoxy resin; Further optionally, the second epoxy resin comprises an aliphatic epoxy resin having an epoxy equivalent of 190 g / eq-273 g / eq; More optionally, the second epoxy resin comprises an aliphatic epoxy resin having the following structural formula: Among them, 35≤m+n≤43, 8≤m≤11.
4. The battery cell packaging material according to any one of claims 1 to 3, It is characterized in that The mass ratio of the second epoxy resin to the first epoxy resin is (0.12-0.4):1; optionally, it is (0.12-0.3):
1.
5. The battery cell packaging material according to any one of claims 1 to 4, It is characterized in that The modified thermally conductive filler has at least one of the following characteristics: (1) The modified thermally conductive filler comprises one or more of aluminum nitride, boron nitride, silicon carbide, aluminum oxide, magnesium oxide and zinc oxide surface-modified by a first silane coupling agent, wherein the first silane coupling agent contains an epoxy group; Optionally, the first silane coupling agent includes 3-glycidylpropyltrimethoxysilane coupling agent; (2) The modified thermally conductive filler includes one or more of a nano-scale modified thermally conductive filler and a micro-scale modified thermally conductive filler; Optionally, the volume particle size distribution Dv50 of the nano-scale modified thermally conductive filler is 100nm-400nm; the volume particle size distribution Dv50 of the micron-scale modified thermally conductive filler is 1μm-20μm; Optionally, the modified thermally conductive filler comprises the nano-scale modified thermally conductive filler and the micro-scale modified thermally conductive filler in a mass ratio of 1:(0.125-0.8); further optionally, the modified thermally conductive filler comprises the nano-scale modified thermally conductive filler and the micro-scale modified thermally conductive filler in a mass ratio of 1:(0.28-0.5); (3) The ratio of the mass of the modified thermally conductive filler to the total mass of the first epoxy resin and the second epoxy resin is (0.37-0.95):1; optionally, it is (0.47-0.85):
1.
6. The battery cell packaging material according to any one of claims 1 to 5, It is characterized in that The curing agent has at least one of the following characteristics: (1) The curing agent includes one or more of diethylaminopropylamine, isophorone diamine, meta-xylylenediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, methylhexahydrophthalic anhydride, polyamide and xylylenediamine condensate; Optionally, the curing agent includes m-xylylenediamine; (2) The mass of the first epoxy resin is denoted as m1, the mass of the second epoxy resin is denoted as m2, and the mass of the curing agent is denoted as m3. The mass of the first epoxy resin, the mass of the second epoxy resin and the mass of the curing agent satisfy: m3 = active hydrogen equivalent of the curing agent × (m1 / epoxy equivalent of the first epoxy resin + m2 / epoxy equivalent of the second epoxy resin) × A, 1.1≤A≤1.
2.
7. The battery cell packaging material according to any one of claims 1 to 6, It is characterized in that The material of the coating also includes a second silane coupling agent; Optionally, the second silane coupling agent has at least one of the following characteristics: (1) the second silane coupling agent includes one or more of an amino-type silane coupling agent, an epoxy-type silane coupling agent, a vinyl-type silane coupling agent, an acyloxy-type silane coupling agent, an isocyanate-type silane coupling agent, a mercapto-type silane coupling agent, and a urea-type silane coupling agent; (2) The ratio of the mass of the second silane coupling agent to the total mass of the first epoxy resin and the second epoxy resin is (0.5-3):
53.
8. The battery cell packaging material according to any one of claims 1 to 7, It is characterized in that The coating material also includes a leveling agent; Optionally, the leveling agent includes one or more of a polydimethylsiloxane leveling agent, a polyether-modified siloxane leveling agent, a polymethylalkylsiloxane leveling agent, a hydroxyl-reactive polysiloxane leveling agent, an epoxy-reactive polysiloxane leveling agent, an alkyl-reactive polysiloxane leveling agent, and a polyacrylate leveling agent; Optionally, the mass ratio of the leveling agent to the second silane coupling agent is (0.05-0.5):(0.5-3).
9. The battery cell packaging material according to any one of claims 1 to 8, It is characterized in that The coating material also includes a defoaming agent; Optionally, the defoamer includes one or more of a mineral oil defoamer, a polydimethylsiloxane defoamer, a polyether-modified polydimethylsiloxane defoamer, a polyurea defoamer and a polyamide defoamer; Optionally, the mass ratio of the defoaming agent to the second silane coupling agent is (0.05-0.5):(0.5-3).
10. The battery cell packaging material according to any one of claims 1 to 9, It is characterized in that The coating has a thickness of 20 μm-100 μm.
11. The battery cell packaging material according to any one of claims 1 to 9, It is characterized in that In parts by weight, the raw materials for preparing the coating include: 38-47 parts of the first epoxy resin, 6-15 parts of the second epoxy resin, 7-9 parts of the curing agent, 20-50 parts of the modified thermal conductive filler, 0.5-3 parts of the second silane coupling agent, 0.05-0.5 parts of the leveling agent and 0.05-0.5 parts of the defoaming agent.
12. The battery cell packaging material according to any one of claims 1 to 11, It is characterized in that The substrate comprises one of a metal shell material, a hard plastic shell material and an aluminum-plastic film.
13. The battery cell packaging material according to any one of claims 1 to 12, It is characterized in that The coating further comprises at least one of the following features: (1) The insulation resistance of the coating is ≥4 GΩ; (2) The adhesion of the coating on the surface of the substrate is level 0 or level 1; (3) The coating does not crack when bent 45° on a shaft with a curvature diameter of 32 mm; (4) The coating is resistant to an electrolyte containing a carbonate solvent.
14. A method for preparing a battery cell packaging material according to any one of claims 1 to 13, It is characterized in that The steps include: preparing a mixture including the first epoxy resin, the second epoxy resin, the modified thermally conductive filler, and a solvent; The mixture and the curing agent are mixed and coated on one side surface of the substrate, and then baked to prepare the battery cell packaging material; The elastic modulus of the first epoxy resin is 0.5 GPa-3 GPa, the dielectric constant is 2.5-4, and the elongation at break of the second epoxy resin is 150%-400%.
15. The method for preparing the battery cell packaging material according to claim 14, It is characterized in that The preparation method comprises at least one of the following conditions: (1) The fineness of the mixture is ≤20 μm; (2) The baking temperature is 120°C-180°C, and the baking time is 10min-30min; (3) The solvent includes one or more of an ester solvent, a ketone solvent, an alcohol solvent, an alcohol ether solvent, an ether solvent, an aromatic hydrocarbon solvent and an alkane solvent.
16. A method for preparing a battery cell packaging material according to any one of claims 14 to 15, It is characterized in that The preparation method of the modified thermally conductive filler comprises the following steps: In an acidic environment, mixing a thermally conductive filler and a first silane coupling agent and then performing a modification treatment to prepare the modified thermally conductive filler; Optionally, the pH value of the acidic environment is 4-5; Optionally, the temperature of the modification treatment is 20°C-30°C, and the time of the modification treatment is 30min-40min; Optionally, the mass ratio of the thermally conductive filler to the first silane coupling agent is 50:(0.5-1).
17. A secondary battery, It is characterized in that include: Battery cells; as well as A packaging material for encapsulating the battery cell, wherein the packaging material is selected from the battery cell packaging material according to any one of claims 1 to 13, and a side of the battery cell packaging material having the coating is adjacent to the battery cell.
18. The secondary battery according to claim 17, It is characterized in that The battery core comprises a heat dissipation tab, and the heat dissipation tab is inserted into the coating.
19. An electrical device, It is characterized in that Comprising the secondary battery as claimed in any one of claims 17 to 18.
Citation Information
Cited By
Secondary battery, electronic device, and manufacturing method for secondary battery
WO2026194553A1