Mg3 (Sb / Bi) 2-based thermoelectric composite material with high-temperature stability and preparation method thereof

CN119072210APending Publication Date: 2024-12-03SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310633763.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

Smart Images

  • Figure CN119072210A_ABST
    Figure CN119072210A_ABST
Patent Text Reader

Abstract

The invention relates to an Mg3 (Sb / Bi) 2-based thermoelectric composite material with high-temperature stability and a preparation method thereof. The synthesis method of the Mg3 (Sb / Bi) 2-based thermoelectric composite material comprises the following steps: weighing an Mg elementary substance, an Sb elementary substance, a Bi elementary substance, a Q elementary substance and an M elementary substance as raw materials according to the stoichiometric ratio of a raw material chemical formula Mg < 3 + delta > SbyBi < 2-y-z > Qz + a wt% M, and preparing the Mg3 (Sb / Bi) 2-based thermoelectric composite material by adopting a melting method or a ball milling method, wherein 0.05 < = delta < = 0.4; 0 < = y < = 2; q is a chalcogenide element or / and a transition metal element, the chalcogenide element is at least one of S, Se and Te, the transition metal element is at least one of Y and Sc, and z is more than or equal to 0.01 and less than or equal to 0.1; m is Zr, Cu or Al, and a is more than 0 and less than or equal to 5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a Mg3(Sb / Bi)2-based thermoelectric composite material and a preparation method thereof, belonging to the field of material preparation. Background Art

[0002] Thermoelectric conversion technology is an environmentally friendly energy conversion technology based on the Seebeck effect and the Peltier effect, which can directly realize the mutual conversion between thermal energy and electrical energy. It has the characteristics of small system size, noiseless operation, no emissions, high reliability and long life. It plays an irreplaceable role in technical fields such as multi-stage utilization of industrial waste heat, environmental energy recovery, special power supplies, and local refrigeration.

[0003] Thermoelectric conversion efficiency is determined by the thermoelectric properties of the material, and the dimensionless thermoelectric figure of merit zT is usually used to characterize the thermoelectric performance of the material. 2 σT / κ, where σ, S, κ and T are the electrical conductivity, Seebeck coefficient, thermal conductivity and absolute temperature of the thermoelectric material, respectively. Among them, the three parameters σ, κ and S are coupled with each other and difficult to regulate individually, which brings challenges to the performance optimization of thermoelectric materials. With the development of disciplines and technologies related to thermoelectric materials, people's understanding of the microscopic mechanism of electrothermal transport properties in thermoelectric materials has continued to deepen. In recent years, new high-performance thermoelectric materials such as filled skutterudites, cage compounds, liquid-like materials, GeTe-based compounds, half-Heusler compounds, SnSe and Mg3(Sb / Bi)2-based compounds have emerged. Among them, Mg3(Sb / Bi)2-based thermoelectric materials have attracted widespread attention from industry and academia due to their excellent thermoelectric properties and good mechanical properties.

[0004] The crystal structure of Mg3(Sb / Bi)2-based compounds is anti-α-La2O3 type, the space group is P-3m1, and it is AB2X2 (where A is an alkaline earth or divalent rare earth element, and B is a d 0 , d 5 or 10 The transition metal (X is generally Sb or Bi) is a special case of Zintl phase compound, that is, Mg atoms occupy both A and B positions in AB2X2. In Mg3(Sb / Bi)2-based compounds, due to the different chemical environments at A and B positions, Mg atoms have two different properties, namely ionic Mg(Ⅰ) and covalent Mg(Ⅱ). Among them, Mg(Ⅰ) constitutes [Mg] 2+ The cation layer can strongly scatter phonons, making it have a lower lattice thermal conductivity; Mg(Ⅱ) and Sb / Bi [Mg2(Sb / Bi)2] 2+ The anion layer can provide a channel for electron transmission, ensuring good electrical properties of the material.

[0005] In recent years, the thermoelectric performance of Mg3(Sb / Bi)2-based materials has been significantly improved through methods such as carrier concentration optimization, point defect scattering, band structure modification, and grain boundary engineering. Pei et al. increased the carrier concentration to ~1×10 20 cm -3 , the zT value reaches ~1.8 at 725K (Adv. Mater., 2019, 31, 1903387.). Chen et al. achieved the synergistic optimization of electrical properties and thermal conductivity by doping Mn elements in the Mg position, and the zT value was close to 1.85 at 723K (Nano Energy, 2018, 52, 246-255.). Liu et al. achieved differential scattering of electrons and phonons by introducing a small amount of additional Cu elements to optimize the thermoelectric properties of the material, and the zT value reached ~1.9 at 773K (Joule, 2021, 5, 1196-1208.). In addition, compared with other typical thermoelectric materials, Mg3(Sb / Bi)2 material has excellent mechanical properties, and its fracture toughness is ~3MPam 1 / 2 (Adv. Funct. Mater., 2019, 29, 1807235.), which is conducive to material machining. Therefore, Mg3(Sb / Bi)2-based thermoelectric materials with both high thermoelectric properties and good mechanical properties are considered to be a new type of thermoelectric material with commercial potential.

[0006] However, the poor thermal stability of Mg3(Bi / Sb)2-based materials limits their device application process. It is generally believed that the high vapor pressure and high chemical activity of Mg at high temperatures lead to continuous volatilization and oxidation of Mg elements during sintering and service (ACS Appl. Mater. Interfaces 2022, 14, 27, 31024-31034.), causing serious deterioration of material performance or even failure. There are two main ways to improve the stability of Mg3(Bi / Sb)2-based materials reported so far: one is annealing in Mg vapor, in which Mg vapor infiltrates the sample to increase the Mg content at the grain boundaries and in the grains, thereby slowing down and compensating for the loss of Mg and improving the stability of the material (ACS Appl. Mater. Interfaces 2022, 14, 27, 31024-31034.), but this process requires long-term annealing at a high temperature, a long cycle, and high energy consumption; the second is to inhibit Mg loss and improve the stability of the material by preparing a surface coating. Shang et al. prepared BN coating on the surface of Mg3(Bi / Sb)2-based materials by chemical vapor deposition and successfully improved its stability above 673K ​​(Acta Materialia 2020, 201, 572-579.), but the thermal expansion coefficient of the BN coating material is quite different from that of the substrate. In actual use, there is a problem of coating cracking due to the mismatch of thermal expansion coefficients. Summary of the invention

[0007] In view of the above problems, the present invention aims to provide a Mg3(Sb / Bi)2-based thermoelectric composite material which has high temperature stability and a preparation method thereof.

[0008] In a first aspect, the present invention provides a method for synthesizing a Mg3(Sb / Bi)2-based thermoelectric composite material, comprising: According to the nominal composition of raw materials Mg 3+δ Sb y Bi 2-y-z Q z+a wt%M stoichiometric ratio of Mg, Sb, Bi, Q and M as raw materials, using melting method or ball milling method to prepare the Mg3(Sb / Bi)2-based thermoelectric composite material; wherein 0.05≤δ≤0.4; 0≤y≤2; Q is a chalcogen element or / and a transition metal element, the chalcogen element is at least one of S, Se, Te, the transition metal element is at least one of Y, Sc, 0.01≤z≤0.1; M is Zr, Cu or Al, 0<a≤5. Wherein, when the addition amount of M is controlled between 1 and 5wt%, high thermoelectric performance and stability can be maintained at the same time. When the compounding amount is greater than 5%, the thermal conductivity rises sharply and the thermoelectric performance deteriorates seriously. The uncompounded sample has poor stability at high temperature and the electrical performance decays rapidly.

[0009] Preferably, the melting method comprises: first heating to 1373K-1473K and keeping the temperature for 10-24h to carry out a melting reaction, then cooling to room temperature, and finally grinding in a protective atmosphere to obtain the Mg3(Sb / Bi)2-based thermoelectric composite material.

[0010] Preferably, the M element is mixed with the Mg element, the Sb element, the Bi element, and the Q element before the melting reaction; Alternatively, Mg, Sb, Bi and Q are first mixed and melted before adding M. There are two situations: M is added before melting, and when melting, M reacts with a certain component element in the matrix to generate the target second phase; M is added after melting, and during the sintering process, M reacts with a certain element in the matrix to generate the target second phase.

[0011] Preferably, the protective atmosphere is an inert gas.

[0012] Preferably, the ball milling method includes: a ball-to-material ratio of (5-10):1, mechanical alloying in a high-energy ball mill with a rotation speed of 1000-2000r / min (e.g., 1400r / min), controlling the total ball milling time to be 8-10h, and stopping for 20-30min after each ball milling for 1h to cool down.

[0013] Preferably, 1 to 3 wt % of stearic acid is added to the raw materials as an anti-caking agent.

[0014] Preferably, the Mg single substance, the Sb single substance, the Bi single substance, the Q single substance and the M single substance are mixed and then directly subjected to mechanical alloying to generate the target composite material; Alternatively, Mg, Sb, Bi, and Q are first mechanically alloyed, and then M powder is added to mix. As with the preparation of samples by the melting method, there are also two situations. One is to directly generate the target second phase during mechanical alloying. The other is to add M after synthesizing the main phase and generate the target second phase during the sintering process. The mechanical alloying product is a powder and does not require grinding.

[0015] In the second aspect, the present invention provides a Mg3(Sb / Bi)2-based thermoelectric composite material prepared according to the above-mentioned preparation method. In the present invention, the element M reacts with an element in the matrix component to generate a second phase, which is dispersed in the matrix in the form of a second phase. Zr reacts with Sb, while Cu or Al reacts with Mg. For Zr, the lattice constants of samples with different composite amounts are refined, and it can be seen that the lattice constants of the uncompounded sample and the samples with different composite amounts are almost unchanged, indicating that Zr has not entered the lattice. It can be seen from the impurity peaks at 35° to 40° in XRD that the second corresponding card is Sb 1-x The larger the composite amount of Zr, the stronger the second phase peak. At the same time, since Zr is very easy to oxidize, Sb 1-x At the same time as the Zr second phase, some oxides will also be introduced. The present invention generates the second phase in situ by adding the M element to optimize the grain boundary, thereby improving the stability of the material without affecting the thermoelectric performance.

[0016] Preferably, when M is Zr, the chemical composition of the Mg3(Sb / Bi)2-based thermoelectric composite material comprises: Mg 3+δ Sb y-b(1-x) Bi 2-y-z Q z +a wt% Sb 1-x Zr where 0.05≤δ≤0.4; 0≤y≤2; Q is a chalcogen element and / or a transition metal element, the chalcogen element is at least one of S, Se, and Te, the transition metal element is at least one of Y and Sc, 0.01≤z≤0.1, 0<b≤0.1, 0<a≤5, 0≤x≤0.3.

[0017] Preferably, when M is Al or / and Cu, the chemical composition of the Mg3(Sb / Bi)2-based thermoelectric composite material comprises: Mg 3+δ-b Sb y Bi 2-y-z Q z +a wt%Mg cM alloy, wherein 0.05≤δ≤0.4; 0≤y≤2; Q is a chalcogen element and / or a transition metal element, the chalcogen element is at least one of S, Se, and Te, the transition metal element is at least one of Y and Sc, 0.01≤z≤0.1, 0<b≤0.1, 0<a≤5, and 0.7≤c≤1.5.

[0018] In a third aspect, the present invention provides a dense block of Mg3(Sb / Bi)2-based thermoelectric composite material, characterized in that the dense block of Mg3(Sb / Bi)2-based thermoelectric composite material is obtained by densification using Mg3(Sb / Bi)2-based thermoelectric composite material as raw material; the densification method includes: hot pressing sintering, spark plasma sintering and cold pressing; The parameters of the hot pressing sintering include: sintering pressure of 50-80 MPa; sintering temperature of 500-800° C.; sintering time of 2-90 min; The parameters of the spark plasma sintering include: sintering pressure of 50-80 MPa; sintering temperature of 500-800° C.; sintering time of 2-90 min; The cold pressing parameters include: the cold pressing pressure is 10-80 MPa, and the pressure holding time is 10-60 min.

[0019] Preferably, the relative density of the dense block of the Mg3(Sb / Bi)2-based thermoelectric composite material is above 95%.

[0020] Beneficial effects: The method of the present invention has the characteristics of simple process and easy operation, and does not add additional steps, which is conducive to large-scale preparation. That is, while synthesizing the matrix or densifying, the in-situ generated micro-nano second phase is evenly distributed at the grain boundary, which can effectively hinder the migration of Mg at the grain boundary and slow down the loss of Mg in the matrix at high temperature, thereby improving its high temperature stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The relationship between the lattice constants of the uncompounded sample and the compounded 1-4wt% Zr sample obtained by refinement and the compounding amount; Figure 2 is the Mg synthesized in the embodiment 3.1 Sb 0.5 Bi 1.49 Te 0.01 And XRD patterns of composite 1-3wt% Zr sample powders; Figure 3 The scanning electron microscope and element distribution spectrum of the composite 2wt% Zr sample in the embodiment; Figure 4 Mg in the embodiment 3.1 Sb 0.5 Bi1.49 Te 0.01 The thermoelectric performance of +1-3wt% Zr samples varies with temperature, where (a) is the conductivity σ varies with temperature, (b) is the Seebeck coefficient S varies with temperature, (c) is the thermal conductivity κ varies with temperature, and (d) is the dimensionless thermoelectric figure of merit zT varies with temperature; Figure 5 For composite 1-3wt% Zr and uncomposite sample Mg 3.1 Sb 0.5 Bi 1.49 Te 0.01 Relative change of conductivity σ / σ0 with time at 750K; Figure 6 For composite 1-3wt% Zr and uncomposite sample Mg 3.1 Sb 0.5 Bi 1.49 Te 0.01 Relative change of Seebeck coefficient S / S0 with time at 750K; Figure 7 For composite 1-3wt% Zr and uncomposite sample Mg 3.1 Sb 0.5 Bi 1.49 Te 0.01 Relative change of power factor PF / PF0 over time at 750K. Figure 8 Mg synthesized in Example 4 3.1 Sb 0.5 Bi 1.49 Te 0.01 +0.4wt%Al sample powder XRD pattern; Fig. 9 The scanning electron microscope and element distribution spectrum of the composite 0.4wt% Al sample in Example 4; Fig.10 Mg in Example 4 3.1 Sb 0.5 Bi 1.49 Te 0.01 The thermoelectric performance of the +0.4wt%Al sample varies with temperature, where (a) is the conductivity σ versus temperature, (b) is the Seebeck coefficient S versus temperature, (c) is the thermal conductivity κ versus temperature, and (d) is the dimensionless thermoelectric figure of merit zT versus temperature; Fig.11 The composite sample of 0.4wt% Al and the uncomposite sample Mg in Example 4 3.1 Sb 0.5 Bi 1.49 Te 0.01 Repeated tests of thermal conductivity versus temperature. DETAILED DESCRIPTION

[0022] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.

[0023] In the present disclosure, by compounding the M metal element with the Mg3(Sb / Bi)2-based material, a micro-nano second phase is generated in situ during the melting reaction, mechanical alloying or sintering densification process and distributed inside the material, thereby hindering the diffusion and migration of Mg in the grain boundaries and effectively improving the high-temperature stability of the material. The chemical formula of the Mg3(Sb / Bi)2-based thermoelectric composite material is Mg 3+δ Sb y Bi 2-y-z Q z +a wt% M, wherein 0.05≤δ≤0.4; 0≤y≤2; Q is at least one of the chalcogen elements S, Se, Te, or transition metals Y, Sc, 0.01≤z≤0.1; 0≤a≤5, and M is Zr, Cu or Al.

[0024] In one embodiment of the present invention, the preparation process of the Mg3(Sb / Bi)2-based thermoelectric composite material is simple and easy to prepare on a large scale. The following is an exemplary description of the preparation process of the Mg3(Sb / Bi)2-based thermoelectric composite material provided by the present invention.

[0025] According to the raw material chemical formula Mg 3+ Sb y Bi 2-y-z Q z +a wt%M stoichiometric ratio of weighing single element raw materials such as Mg, Sb, Bi, Q and M.

[0026] For the metal element M, it can be optionally added before or after melting or before or after ball milling. The melting process is: heating to 1150°C at a heating rate of ~130°C / h, and quenching at this temperature for 10 to 15 hours to obtain a molten ingot. The ball milling process is: additionally adding 1 to 3wt% stearic acid as an anti-adhesive agent, the ball-to-material ratio is 5:1 to 10:1, mechanical alloying in a high-energy ball mill with a rotation speed of 1400r / min, stopping for 20 to 30 minutes to cool down after each hour of grinding, and the reaction is complete after 8 to 10 hours of ball milling.

[0027] Grinding treatment: For samples prepared by the melting method, the ingot needs to be manually ground into powder in a glove box with a protective atmosphere.

[0028] Sample densification. If metal M is added during melting, a dense block is obtained directly by spark plasma sintering, hot pressing or cold pressing. If metal M is not added during melting, the ingot is ground and then added with the M metal powder weighed during batching, or the pre-synthesized alloy powder of M and matrix elements, and mixed under a protective atmosphere. The mixing methods include but are not limited to mixing with a mixer, manual grinding and mixing, and ball milling. After mixing evenly, a dense block is obtained by spark plasma sintering, hot pressing or cold pressing.

[0029] In an optional embodiment, when densification is performed by spark plasma sintering or hot pressing sintering, the sintering process parameters are: sintering temperature is 500°C to 800°C, sintering pressure is 50MPa to 80MPa, and holding time is 2 to 90min; when densification is performed by cold pressing, the cold pressing process parameters are: pressure is 10 to 80Mpa, and holding time is 10 to 60min.

[0030] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0031] Example 1 (1) According to the chemical formula Mg 3.1 Sb 1.5 Bi 0.49 Te 0.01 +1wt% Zr, weigh 0.8333g of Mg particles (purity 99.95%), 2.0200g of Sb particles (purity 99.9999%), 1.1326g of Bi particles (purity 99.999%), and 0.0141g of Te particles (purity 99.999%), mix them for synthesizing the matrix material, and weigh 0.04g of Zr powder (purity 99.95%) for generating the second phase of ZrSb. Put all the raw materials into a Ta tube and seal it, then seal the Ta tube in a quartz tube; (2) placing all sealed quartz tubes into a vertical melting furnace to perform a melting reaction to synthesize the target product. The melting process is: heating to 1150°C at a rate of 130°C / h, keeping the temperature for 10-15h, and quenching after the end of the temperature keeping; (3) grinding the ingot into powder and then sintering it into a compact form by discharge plasma sintering. The sintering process is as follows: heating the temperature to 550°C at a rate of 50°C / min, keeping the temperature for 2 min, and then slowly cooling it to room temperature in the furnace. (4) Measure and calculate the sample density, characterize the thermoelectric properties of the bulk material, and characterize its stability using long-term in-situ electrical performance testing.

[0032] Example 2 (1) According to the chemical formula Mg 3.1 Sb 1.5 Bi 0.49 Te 0.01 +2wt% Zr, weigh 0.8333g of Mg particles (purity 99.95%), 2.0200g of Sb particles (purity 99.9999%), 1.1326g of Bi particles (purity 99.999%), and 0.0141g of Te particles (purity 99.999%), mix them for synthesizing the matrix material, and weigh 0.08g of Zr powder (purity 99.95%) for generating the second phase of ZrSb. Put all the raw materials into a Ta tube and seal it, then seal the Ta tube in a quartz tube; (2) placing all sealed quartz tubes into a vertical melting furnace to perform a melting reaction to synthesize the target product. The melting process is: heating to 1150°C at a rate of 130°C / h, keeping the temperature for 10-15h, and quenching after the end of the temperature keeping; (3) grinding the ingot into powder and then sintering it to densify it by spark plasma. The sintering process is as follows: heating the temperature to 550°C at a rate of 50°C / min, keeping the temperature for 2 min, and then slowly cooling it to room temperature in the furnace; (4) Measure and calculate the sample density, characterize the thermoelectric properties of the bulk material, and characterize its stability using long-term in-situ electrical performance testing.

[0033] Example 3 (1) According to the chemical formula Mg 3.1 Sb 1.5 Bi 0.49 Te 0.01 +3wt% Zr, weigh 0.8333g of Mg particles (purity 99.95%), 2.0200g of Sb particles (purity 99.9999%), 1.1326g of Bi particles (purity 99.999%), and 0.0141g of Te particles (purity 99.999%), mix them for synthesizing the matrix material, and weigh 0.12g of Zr powder (purity 99.95%) for generating the second phase of ZrSb. Put all the raw materials into a Ta tube and seal it, then seal the Ta tube in a quartz tube; (2) Put all the sealed quartz tubes into a vertical melting furnace to perform melting reaction to synthesize the target product. Melting process: heat up to 1150°C at a heating rate of ~130°C / h, keep warm for 10-15h, and quench after the end of the insulation; (3) grinding the ingot into powder and then sintering it to densify it by spark plasma. The sintering process is as follows: heating the temperature to 550°C at a rate of 50°C / min, keeping the temperature for 2 min, and then slowly cooling it to room temperature in the furnace; (4) Measure and calculate the sample density, characterize the thermoelectric properties of the bulk material, and characterize its stability through long-term in-situ electrical performance testing.

[0034] Example 4 (1) According to the chemical formula Mg 3.1 Sb 1.5 Bi 0.49 Te 0.01 +0.4wt%Al, weigh 0.8333g of Mg particles (purity 99.95%), 2.0200g of Sb particles (purity 99.9999%), 1.1326g of Bi particles (purity 99.999%), and 0.0141g of Te particles (purity 99.999%), and mix them for synthesizing the matrix material, and weigh 0.016g of Al powder (purity 99.95%) for generating the second phase of MgSb alloy. Put all the raw materials into a Ta tube and seal it, then seal the Ta tube in a quartz tube; (2) Put all the sealed quartz tubes into a vertical melting furnace to perform melting reaction to synthesize the target product. Melting process: heat up to 1150°C at a heating rate of ~130°C / h, keep warm for 10-15h, and quench after the end of the insulation; (3) grinding the ingot into powder and then sintering it to densify it by spark plasma. The sintering process is as follows: heating the temperature to 550°C at a rate of 50°C / min, keeping the temperature for 2 min, and then slowly cooling it to room temperature in the furnace; (4) Measure and calculate the sample density to characterize the thermoelectric properties of the bulk material, and characterize its stability by testing the thermal conductivity multiple times.

[0035] Comparative Example 1 (1) According to the chemical formula Mg 3.1 Sb 1.5 Bi 0.49 Te 0.01 +0wt% Zr, weigh 0.8333g of Mg particles (purity 99.95%), 2.0200g of Sb particles (purity 99.9999%), 1.1326g of Bi particles (purity 99.999%), and 0.0141g of Te particles (purity 99.999%) and mix them. Put all the raw materials into a Ta tube and seal it, then seal the Ta tube in a quartz tube; (2) Put all the sealed quartz tubes into a vertical melting furnace to perform melting reaction to synthesize the target product. Melting process: heat up to 1150°C at a heating rate of ~130°C / h, keep warm for 10-15h, and quench after the end of the insulation; (3) grinding the ingot into powder and then sintering it to densify it by spark plasma. The sintering process is as follows: heating the temperature to 550°C at a rate of 50°C / min, keeping the temperature for 2 min, and then slowly cooling it to room temperature in the furnace; (4) Measure and calculate the sample density, characterize the thermoelectric properties of the bulk material, and characterize its stability through long-term in-situ electrical performance testing.

[0036] Figure 1 The relationship between the lattice constant of the uncompounded sample and the compounded sample with 1-4wt% Zr and the compounding amount. It does not increase monotonically with the increase of the composite amount, indicating that Zr does not enter the lattice to cause lattice expansion, but is only dispersed at the grain boundary in the form of a second phase; Figure 2 is the Mg synthesized in the embodiment 3.1 Sb 0.5 Bi 1.49 Te 0.01 The XRD spectrum of the powder of the composite 1-3wt% Zr sample shows that the main phase is synthesized for the uncompounded sample and the samples with different composite amounts. The peak position of the main phase does not shift after the composite, indicating that the lattice constant has not changed, the composite elements have not entered the lattice, and only exist in the form of a second phase. The sample has a second phase peak at about 35° to 40°, and the peak intensity increases with the increase of the composite amount. The second phase peak corresponds to the compound Sb 1-x Zr, and some oxides introduced due to the more active compound elements; Figure 3 The scanning electron microscope and element distribution spectrum of the composite 2wt% Zr sample in the embodiment. It can be seen from the figure that the Mg, Bi, and Sb elements are evenly distributed, and the in-situ generated ZrSb exists in the matrix in the form of a micron-sized second phase; Figure 4 Mg in the embodiment 3.1 Sb 0.5 Bi 1.49 Te 0.01 The thermoelectric performance of +1-3wt% Zr samples varies with temperature. Among them, Figure (a) is the relationship between the conductivity σ and the temperature, Figure (b) is the relationship between the Seebeck coefficient S and the temperature, Figure (c) is the relationship between the thermal conductivity κ and the temperature, and Figure (d) is the dimensionless thermoelectric figure of merit zT and the temperature. It can be seen from the figure that the conductivity decreases with the increase of temperature, the Seebeck coefficient is negative, and increases with the increase of temperature, indicating that the sample is n-type conduction. The electrical transport behavior of the uncompounded sample and the samples with different composite amounts remains unchanged. The thermal conductivity of different samples decreases with the increase of temperature. For the composited samples, the thermal conductivity of the samples with different composite amounts remains the same, which is higher than that of the uncompounded samples, resulting in the thermoelectric figure of merit of the composited samples being slightly lower than that of the uncompounded samples; Figure 5 For composite 1-3wt% Zr and uncomposite sample Mg 3.1 Sb 0.5 Bi 1.49 Te 0.01 The relationship between the relative change of conductivity σ / σ0 and time at 750K. From the figure, we can see that the electrical performance of the uncompounded sample decays rapidly after 4 hours of testing, and is only ~50% of the initial value at 12 hours. The decay rate of samples with different compounding amounts slows down significantly, and remains above 90% of the initial value at 14 hours. Figure 6 For composite 1-3wt% Zr and uncomposite sample Mg 3.1 Sb 0.5 Bi 1.49 Te 0.01 The relationship between the relative change of Seebeck coefficient S / S0 and time at 750K. It can be seen from the figure that the change of Seebeck coefficient is more gentle than that of conductivity. The Seebeck coefficient of the uncompounded sample began to rise rapidly after 8 hours, indicating that a large amount of Mg volatilized, causing the carrier concentration to drop rapidly, and the material gradually transformed into an intrinsic semiconductor. The composite sample remained almost unchanged at 14 hours, indicating that the Mg content did not change significantly; Figure 7 For composite 1-3wt% Zr and uncomposite sample Mg 3.1 Sb 0.5 Bi 1.49 Te 0.01 The relative change of power factor PF / PF0 at 750K with time. The change of PF reflects the overall change of the electrical properties of the material. From the figure, it can be seen that the electrical properties of the uncompounded sample deteriorated rapidly due to the large amount of volatilization of Mg, while the composite sample remained almost unchanged after 14 hours. Figure 8 is the Mg synthesized in the embodiment 3.1 Sb 0.5 Bi 1.49 Te 0.01 +0.4wt%Al sample powder XRD spectrum. From the figure, we can see that the main phase is synthesized, and due to the small amount of composite, the second phase content is below the XRD detection limit, and no obvious second phase peak appears; Fig. 9 The scanning electron microscope and element distribution spectrum of the composite 0.4wt% Al sample in the embodiment. It can be seen from the figure that Mg is enriched at the Al element, indicating that the alloy particles generated by the reaction of Mg and Al are dispersed at the grain boundaries; Fig.10 Mg in the embodiment 3.1 Sb 0.5 Bi 1.49 Te 0.01The thermoelectric performance of the +0.4wt%Al sample varies with temperature. From the figure, we can see that the conductivity decreases with increasing temperature, the Seebeck coefficient is negative, and increases with increasing temperature, indicating that the sample is n-type conduction. The thermal conductivity decreases with increasing temperature; Fig.11 For composite 0.4wt% Al and uncomposite sample Mg 3.1 Sb 0.5 Bi 1.49 Te 0.01 Repeated test of thermal conductivity versus temperature. As can be seen from the figure, the thermal conductivity of the uncompounded sample dropped significantly in the second test, indicating that a large amount of Mg volatilized during the test, the number of electron carriers decreased, and the carrier thermal conductivity decreased, resulting in a decrease in the total thermal conductivity. Due to the loss of Mg, a large number of vacancies were excited at high temperatures, resulting in bipolar diffusion. Therefore, in the second test, the thermal conductivity began to rise at 700K. For the composite sample, the thermal conductivity was tested three times, and the performance was basically the same, indicating that the presence of the second phase inhibited the volatilization of Mg at high temperatures and had good thermal stability.

[0037] In the present invention, the micro-nano compound Sb is in situ generated by reacting the M element with the Sb, Bi or Mg element in the matrix. 1-x Zr or Mg x M alloy. Dispersed at the grain boundaries, it can effectively hinder the diffusion and migration of Mg in the grain boundaries, inhibit Mg loss, and significantly improve the high-temperature stability of the material. At the same time, the process is simple and has practical value. The present invention optimizes the grain boundary structure and element composition by introducing the second phase, reduces the driving force (concentration gradient) for Mg to diffuse to the grain boundaries, and hinders the diffusion of Mg in the grain boundaries, thereby achieving the purpose of improving stability, and provides a new idea for the stability optimization of MgSbBi-based alloys.

Claims

1. A method for synthesizing a Mg3(Sb / Bi)2-based thermoelectric composite material, characterized in that: include: According to the raw material chemical formula Mg 3+δ Sb y Bi 2-y-z Q z +a wt%M stoichiometric ratio of Mg, Sb, Bi, Q and M are weighed as raw materials, and the Mg3(Sb / Bi)2-based thermoelectric composite material is prepared by a melting method or a ball milling method; wherein 0.05≤δ≤0.4; 0≤y≤2; Q is a chalcogen element and / or a transition metal element, the chalcogen element is at least one of S, Se, and Te, the transition metal element is at least one of Y and Sc, 0.01≤z≤0.1; M is Zr, Cu or Al, 0<a≤5.

2. The preparation method according to claim 1, characterized in that: The melting method comprises: firstly heating to 1373K-1473K and keeping the temperature for 10-24h to carry out melting reaction, then cooling to room temperature, and finally grinding in a protective atmosphere to obtain the Mg3(Sb / Bi)2-based thermoelectric composite material.

3. The preparation method according to claim 2, characterized in that: The M element is mixed with the Mg element, the Sb element, the Bi element, and the Q element before the melting reaction; Alternatively, Mg single substance, Sb single substance, Bi single substance, and Q single substance are first mixed and melt-reacted, and then M single substance is added.

4. The preparation method according to claim 2 or 3, characterized in that: The protective atmosphere is an inert gas.

5. The preparation method according to claim 1, characterized in that: The ball milling method comprises: a ball-to-material ratio of (5-10):1, mechanical alloying in a high-energy ball mill with a rotation speed of 1000-2000 r / min, controlling the total ball milling time to be 8-10 hours, and stopping for 20-30 minutes after each ball milling for 1 hour for cooling treatment.

6. The preparation method according to claim 5, characterized in that: 1-3 wt % of stearic acid is added to the raw materials as an anti-caking agent.

7. The preparation method according to claim 5, characterized in that: Mg, Sb, Bi, Q and M are mixed and then directly subjected to mechanical alloying to generate a target composite material; Alternatively, Mg single substance, Sb single substance, Bi single substance, and Q single substance are first mechanically alloyed, and then M single substance powder is added and mixed.

8. A Mg3(Sb / Bi)2-based thermoelectric composite material prepared by the preparation method according to any one of claims 1 to 7.

9. The Mg3(Sb / Bi)2-based thermoelectric composite material according to claim 8, characterized in that: When M is Zr, the chemical composition of the Mg3(Sb / Bi)2-based thermoelectric composite material comprises: Mg 3+δ Sb y-b(1-x) Bi 2-y-z Q z +a wt% Sb 1-x Zr where 0.05≤δ≤0.4; 0≤y≤2; Q is a chalcogen element and / or a transition metal element, the chalcogen element is at least one of S, Se, and Te, the transition metal element is at least one of Y and Sc, 0.01≤z≤0.1, 0<b≤0.1, 0<a≤5, 0≤x≤0.

3.

10. The Mg3(Sb / Bi)2-based thermoelectric composite material according to claim 8, characterized in that: When M is Al or / and Cu, the chemical composition of the Mg3(Sb / Bi)2-based thermoelectric composite material comprises: Mg 3+δ-b Sb y Bi 2-y-z Q z +a wt%Mg c M alloy, wherein 0.05≤δ≤0.4; 0≤y≤2; Q is a chalcogen element and / or a transition metal element, the chalcogen element is at least one of S, Se, and Te, the transition metal element is at least one of Y and Sc, 0.01≤z≤0.1, 0<b≤0.1, 0<a≤5, and 0.7≤c≤1.

5.

11. A Mg3(Sb / Bi)2-based thermoelectric composite material dense block, characterized in that: Using the Mg3(Sb / Bi)2-based thermoelectric composite material as claimed in claim 8 as a raw material, a dense block of the Mg3(Sb / Bi)2-based thermoelectric composite material is obtained by densification; The densification methods include: hot pressing sintering, spark plasma sintering and cold pressing; The parameters of the hot pressing sintering include: sintering pressure of 50-80 MPa; sintering temperature of 500-800° C.; sintering time of 2-90 min; The parameters of the spark plasma sintering include: sintering pressure of 50-80 MPa; sintering temperature of 500-800° C.; sintering time of 2-90 min; The cold pressing parameters include: the cold pressing pressure is 10-80 MPa, and the pressure holding time is 10-60 min.

12. The Mg3(Sb / Bi)2-based thermoelectric composite material dense block according to claim 11, characterized in that: The relative density of the dense block of the Mg3(Sb / Bi)2-based thermoelectric composite material is above 95%.