Improved catalyst for selective nox reduction using hydrogen

By adding zeolite components and PGM components to the H2-SCR catalyst, the problems of low NOx conversion and high N2O by-products in the prior art are solved, and efficient NOx control over a wide temperature range is achieved.

CN119072349APending Publication Date: 2024-12-03BASF CORPORATON +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380035593.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-23
Filing Date
2023-05-22
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing H2-SCR catalysts effectively reduce NOx at low temperatures, but produce high levels of N2O by-products at high temperatures, and the NOx conversion efficiency is reduced below 250°C, making it difficult to meet the strict emission regulations requirements.

Method used

By adding the zeolite component to the PGM component on the oxide support, an improved H2-SCR catalyst composition is formed, and the synergistic effect of metal components such as platinum and palladium with the zeolite is used to improve the NOx conversion rate and reduce the formation of N2O.

Benefits of technology

It significantly improves NOx conversion rate and reduces the N2O formation rate, adapts to NOx control needs in various temperature ranges, and meets the strict emission regulations requirements in the future.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005095766370000281
    Figure BDA0005095766370000281
  • Figure HDA0005095766380000011
    Figure HDA0005095766380000011
  • Figure HDA0005095766380000012
    Figure HDA0005095766380000012
Patent Text Reader

Abstract

The present disclosure relates to a hydrogen selective catalytic reduction catalyst composition effective for reducing nitrogen oxides using hydrogen wherein the hydrogen selective catalytic reduction catalyst composition comprises a first component comprising a metal component supported by an oxide support and a second component comprising a zeolite; a selective catalytic reduction article effective for catalyzing reduction of nitrogen oxides using hydrogen, the selective catalytic reduction article comprising such a hydrogen selective catalytic reduction catalyst composition; and a method for treating an exhaust gas stream containing nitrogen oxides using an emissions treatment system comprising such a hydrogen selective catalytic reduction catalyst composition.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for reducing nitrogen oxides (NOx) from engine exhaust in the presence of a hydrogen reducing agent. x ) by selective catalytic reduction of hydrogen (H 2 -SCR) catalyst composition. For example, H 2 The SCR catalyst composition comprises a first component and a second component, wherein the first component comprises a metal component supported by an oxide support, and the second component comprises a zeolite. The present disclosure also relates to a selective catalytic reduction article for selectively reducing NO from an exhaust gas stream x Compound emission treatment system and system for treating NO x NOx describes the various chemical species of nitrogen oxides, including nitric oxide (NO) and nitrogen dioxide (NO 2 )etc.

[0002] By way of example, diesel engine exhaust is a heterogeneous mixture of gaseous, liquid and solid emissions such as carbon monoxide (CO), unburned or partially burned hydrocarbons or their oxygenates (HC), NOx and particulate matter. These emissions are subject to government legislation. Therefore, a catalyst composition and a substrate having the composition disposed thereon are provided in a diesel engine exhaust system to convert some or all of these exhaust components into harmless components and reduce the amount of emissions released into the atmosphere.

[0003] Two commercial technologies are currently used for diesel NOx control: (1) Selective Catalytic Reduction (SCR) using urea (or ammonia) and (2) Lean NOx Trap (LNT). SCR technology is used in both heavy-duty and light-duty applications. LNT technology is used exclusively in light-duty applications. The SCR process catalytically reduces nitrogen oxides with a reductant (e.g., urea or ammonia) in the presence of excess oxygen, resulting in the formation of primarily nitrogen and steam. Alternatively, H2O2, which relies on hydrogen rather than ammonia as the reductant, is used to reduce nitrogen oxides. 2 - The SCR catalyst composition can be used to reduce NOx from the engine exhaust. At low temperatures (e.g., below 200°C), hydrogen is a more reactive reducing agent than ammonia. In the case of a diesel engine, a hydrogen generator can be provided upstream of the catalyst composition as a source of hydrogen used as a reducing agent.

[0004] A diesel oxidation catalyst (DOC) is typically placed in the exhaust gas flow path from a diesel engine to treat the exhaust gas before it is discharged into the atmosphere for the conversion of gaseous HC and CO emissions. x The substance is mainly in the form of NO. As we all know, if NO / NO 2 The molar ratio is close to about 1, then NH 3(or urea) SCR catalysts will operate more efficiently at lower temperatures (such as below 250°C). 3 -Low temperature NO on SCR catalyst x performance, and also uses a diesel oxidation catalyst to convert a portion of the NO in the exhaust gas stream into NO 2 However, the NO conversion efficiency becomes very low below 250°C.

[0005] NOx emission levels are also a concern for the engine exhaust of hydrogen internal combustion engines burning hydrogen. With hydrogen fuel, there is no CO or unburned or partially burned hydrocarbons or their oxygenated compounds. However, when hydrogen is burned with air, NOx emissions are generated due to the presence of O in the combustion chamber. 2 / N 2 Unburned hydrogen and / or additional hydrogen injected into the exhaust gas stream can be used as H 2 - Reductant for the SCR catalyst composition.

[0006] However, the SCR catalysts of the prior art, especially H 2 - SCR catalyst compositions have known problems such as narrow operating temperature window for effective NOx conversion and high nitrous oxide (N 2 O) Undesirable side effects. 2 -SCR catalyst compositions are more effective at low temperatures, such as about 100 to 250°C, where hydrogen can selectively react with NOx on the catalyst surface. This allows H 2 -SCR catalyst compositions become excellent candidates for low temperature NOx control, especially compared to SCR catalyst compositions that rely on ammonia as a reductant. However, at higher temperatures, hydrogen preferentially reacts with oxygen, which is present in large quantities in the exhaust gas of most compression ignition engines. 2 During SCR, the process also generates high levels of N 2 O byproduct, N 2 O yields are in the range of 20% to 40%. 2 O is a powerful greenhouse gas that is highly regulated in most automotive markets around the world, so H 2 - Before the SCR catalyst composition is used for NOx control, it should be reduced by H 2 -Formation of SCR catalyst.

[0007] H 2 A theoretical mechanism of how the SCR catalyst composition reduces nitrogen oxides (NOx) from engine exhaust in the presence of a hydrogen reductant is given by the following elementary reaction steps.

[0008] H 2+→2H(a) (Equation 1)

[0009] NO+→NO(a) (Equation 2)

[0010] NO(a)→N(a)+O(a) (Equation 3)

[0011] O 2 +→2O(a) (Equation 4)

[0012] N(a)+N(a)→N 2 (Equation 5)

[0013] NO(a)+N(a)→N 2 O (Equation 6)

[0014] 2H(a)+O(a)→H 2 O (Equation 7)

[0015] Where (a) represents an active catalytic site on the metal surface, and (b) indicates an atom or molecule chemically adsorbed on the surface. It is inferred that hydrogen molecules adsorb on the surface of the supported metal component and dissociate into hydrogen atoms. NO molecules can be adsorbed on the surface both associatively and dissociatively. The combination of two adsorbed N atoms forms N 2 molecules, and the combination of a NO molecule and an O atom forms N 2 O. Surface H atoms scavenge surface O atoms to form water and thus keep the metal surface reduced or activated. Oxygen is not a necessary reactant for NO reduction, but is a competitor for hydrogen because oxygen increases the hydrogen required to keep the metal surface from being oxidized or deactivated.

[0016] EP 3 409 359 A2 discloses a four-way catalyst composition comprising a plurality of metal oxide nanoparticles hybridized with a metal zeolite, wherein the metal oxide nanoparticles have a maximum dimension of 0.1 nm to 50 nm.

[0017] WO 2018 / 073750 A1 relates to an emission treatment system comprising a hydrogen selective catalytic reduction article and a catalytic article for selectively reducing NOx compounds.

[0018] US2021 / 102486 A1 relates to an emission control system for treating an exhaust gas flow, comprising an oxidation catalyst composition disposed on a substrate fluidly connected to the exhaust gas flow; at least one selective catalytic reduction (SCR) composition disposed on a substrate downstream of the oxidation catalyst composition; and a hydrogen injection article configured to introduce hydrogen into the exhaust gas flow upstream of the oxidation catalyst composition or downstream of the oxidation catalyst composition and upstream of at least one SCR composition.

[0019] EP 2 313 196 A2 discloses a method suitable for using H 2 As a reducing agent to reduce NO x A binary mixed oxide catalyst comprising coprecipitated and mixed 2 O 3 A metal oxide of MnO 2 A type of B metal oxide.

[0020] As NOx regulations become more stringent worldwide and average engine exhaust temperatures continue to decrease, controlling NOx emissions with current SCR technology becomes increasingly challenging. Therefore, there is a need in the art to identify more effective NOx reduction H 2 -SCR technology, which can be sufficiently efficient over a wide temperature range without producing high yields of N 2 O gas in order to meet future stringent regulations.

[0021] The present disclosure provides advanced H 2 -SCR catalyst composition, which is relative to the standard reference H 2 -SCR catalyst composition, especially at low temperatures, significantly increases NOx conversion and reduces N 2 O is formed. In particular, it was found that by adding a zeolite component to a PGM component on an oxide support, 2 -SCR catalyst composition can significantly increase NOx conversion and reduce N 2 O formation. This simultaneous improvement in activity and selectivity appears to be related to a hitherto unrecognized synergistic effect between the two components. Fig.11 is the H of the present disclosure 2 - Schematic representation of an embodiment of an SCR catalyst composition, wherein a first component comprises a metal component (PGM, black dots) on an oxide support (white ovals), combined with a separate second component (yellow squares) comprising a zeolite.

[0022] Improved performance is achieved with various compositions including, but not limited to, those having a metal component selected from platinum (Pt) and / or palladium (Pd) and a zeolite having a zeolite structure on a (mixed) oxide support, such as *BEA, FER, MOR, CHA, FAU and MFI.

[0023] These and other features, aspects and advantages of the present disclosure will become apparent through a reading of the following detailed description and the accompanying drawings briefly described below. Other aspects and advantages of the disclosed subject matter will become apparent from the following. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to provide an understanding of the embodiments of the present disclosure, reference is made to the accompanying drawings. The accompanying drawings are exemplary only and should not be construed as limiting the present disclosure. The disclosure described herein is illustrated in the accompanying drawings by way of example and not limitation. For simplicity and clarity of illustration, the features illustrated in the accompanying drawings are not necessarily drawn to scale. For example, for clarity, the size of some features may be enlarged relative to other features.

[0025] Figure 1A H of the present disclosure 2 -SCR catalyst composition embodiment and standard Pt-SiO 2 / TiO 2 Comparison of NOx conversion of reference compositions.

[0026] Figure 1B Show Figure 1A The catalyst composition N 2 Comparison of O formation rates.

[0027] Figure 2A Show H 2 - Comparison of NOx conversion of SCR catalyst compositions with PGM (Pt) supported on oxide supports or zeolite supports.

[0028] Figure 2B Show Figure 2A Comparison of N2O formation rates of catalyst compositions.

[0029] Figure 3A The H of the present disclosure with different oxide / Y zeolite mixing ratios is shown. 2 -SCR catalyst composition embodiment and standard Pt-Si / TiO 2 Comparison of NOx conversion of reference compositions.

[0030] Figure 3B Show Figure 3A The catalyst composition N 2 Comparison of O formation rates.

[0031] Figure 4A The results show that H with different PGM (Pt) concentrations on oxide or zeolite supports 2 - NOx conversion of the SCR catalyst composition.

[0032] Figure 4B Show Figure 4A The catalyst composition N 2 Comparison of O formation rates.

[0033] Figure 5A The H of the present disclosure with different CHA zeolites was compared. 2-SCR catalyst composition embodiment and standard Pt-SiO 2 / TiO 2 NOx conversion of the reference composition.

[0034] Figure 5B Show Figure 5A The catalyst composition N 2 Comparison of O formation rates.

[0035] Fig. 6A Show H 2 - NOx conversion of SCR catalyst compositions, wherein the PGM is Pd or a mixture of Pt and Pd.

[0036] Figure 6B Show Fig. 6A The catalyst composition N 2 Comparison of O formation rates.

[0037] Fig. 7A The H of the present disclosure for zeolites with different iron loadings is shown. 2 -SCR catalyst composition embodiment and standard Pt-SiO 2 / TiO 2 NOx conversion of the reference composition.

[0038] Figure 7B Show Fig. 7A The catalyst composition N 2 Comparison of O formation rates.

[0039] Fig. 8A Compared with the H 2 -SCR catalyst composition embodiment and standard Pt / Al 2 O 3 NOx conversion of the reference composition.

[0040] Figure 8B Show Fig. 8A The catalyst composition N 2 Comparison of O formation rates.

[0041] Fig. 9A The H of the present disclosure with different oxide / β-zeolite mixing ratios is shown. 2 -SCR catalyst composition embodiment with Pt-SiO 2 / WO 3 / ZrO 2 Comparison of NOx conversion of reference compositions.

[0042] Fig. 9B Show Fig. 9A The catalyst composition N 2 Comparison of O formation rates.

[0043] Fig. 10A Compared with SiO 2 Oxide-supported H 2 - NOx conversion of the SCR catalyst composition.

[0044] Fig. 10B Show Fig. 10A The catalyst composition N 2 Comparison of O formation rates.

[0045] Fig.11 H of the present disclosure 2 - Schematic diagram of an embodiment of an SCR catalyst composition.

[0046] As used herein, unless otherwise specified, "a" or "an" entity refers to one or more of that entity, for example, "a vector" refers to one or more vectors or at least one vector. Therefore, the terms "a" (or "an"), "one or more" and "at least one" are used interchangeably herein.

[0047] As used herein, the term "about" means approximately, in the range of, roughly or around. When the term "about" is used in conjunction with a numerical range, it modifies the range by extending the boundaries above and below the listed values. Typically, the term "about" is used herein to modify the numerical values ​​above and below the stated values ​​by a variance of 5%. Whether or not explicitly indicated, all numerical values ​​are modified by the term "about". The numerical values ​​modified by the term "about" include specific identification values. For example, "about 100" means a number in the range of 95 to 105, including 95, 100 and 105. Unless otherwise indicated herein, the description of the value range herein is intended only to serve as a shorthand method of individually referring to each individual value falling within the range, and each individual value is incorporated into this specification as if individually described herein.

[0048] As used herein, "catalyst" or "catalyst material" or "catalytic material" refers to a material that promotes a reaction.

[0049] As used herein, the term "catalytic article" refers to an element used to promote a desired reaction. For example, a catalytic article may include a washcoat containing a catalyst material (eg, a catalyst composition) on a substrate (eg, a honeycomb substrate).

[0050] As used herein, the term "metal component" refers to any platinum group metal (PGM) (i.e., Ru, Rh, Ir, Pd, or Pt) other than osmium. Reference to a PGM allows the metal to exist in any valence state. For example, the PGM may be in the form of a metal having a zero valence, or the PGM may be in another form, such as an oxide form or a nitrate form. The terms "ruthenium (Ru)", "rhodium (Rh)", "iridium (Ir)", "palladium (Pd)", "platinum (Pt)", etc. refer to corresponding PGM compounds, complexes, etc., which decompose or otherwise convert to a catalytically active form, typically a metal or metal oxide, when calcined or using a catalyst.

[0051] As used herein, the term "nitrogen oxides" or "NOx" refers to oxides of nitrogen. Exemplary nitrogen oxides include oxide compounds such as NO and NO 2 .

[0052] As used herein, a "catalyst" or "catalyst material" or "support" of a "catalytic material" refers to a material that receives a "catalyst" or "catalyst material" or "catalytic material" by precipitation, association, dispersion, impregnation or other suitable means. The term "oxide support" refers to an oxide compound containing a transition metal or lanthanide element (e.g., aluminum (Al), vanadium (V), tungsten (W), titanium (Ti), copper (Cu), iron (Fe), nickel (Ni), manganese (Mn), cerium (Ce), lanthanum (La), praseodymium (Pr), zinc (Zn), niobium (Nb), zirconium (Zr), molybdenum (Mo), tin (Sn), silicon (Si), calcium (Ca), yttrium (Y) or a combination thereof) that has catalytic activity for the reduction of NOx, or promotes another catalytic component to be more active for the reduction of NOx. Oxide supports particularly include oxides of copper, iron, manganese, tin, aluminum, zirconium, silicon, titanium, tungsten, molybdenum, nickel and a combination thereof.

[0053] As used herein, the term "promoted" refers to a metal component ("promoter metal") that is intentionally added to, for example, a zeolite, typically by ion exchange, as opposed to an impurity inherent in the zeolite. In some embodiments, promoter metals that can be used to prepare the promoted zeolites of the disclosed catalyst compositions include, but are not limited to, iron (Fe) and copper (Cu). In some embodiments, both copper and iron may be present as promoter metals.

[0054] As used herein, the term "substrate" refers to a monolithic material upon which a catalyst composition is placed, typically in the form of a washcoat comprising a plurality of supports having catalytic materials thereon.

[0055] As used herein, the term "zeolite" refers to a specific example of a molecular sieve, comprising silicon and aluminum atoms. Zeolites are crystalline materials having fairly uniform pore sizes, ranging from about 3 angstroms in diameter to about 1 angstrom in diameter, depending on the type of zeolite and the type and amount of cations included in the zeolite lattice. To 10 Angstroms within the range.

[0056] The term "acidic zeolite" refers to a protonated zeolite (H-zeolite) or a zeolite that can be converted to H-zeolite, such as NH 4 - Zeolite. The term "H-zeolite" refers to a zeolite having more than 90% of the exchangeable sites as protons (H+).

[0057] H 2 -SCR catalyst composition

[0058] In the present disclosure, there is provided a hydrogen selective catalytic reduction (H 2 -SCR) catalyst composition which effectively catalyzes the reduction of NOx from engine exhaust in the presence of a hydrogen reductant. 2 The SCR catalyst comprises a first component comprising a metal component supported by an oxide support and a second component comprising a zeolite.

[0059] In some embodiments, the metal component is a PGM selected from platinum, palladium, rhodium, iridium, ruthenium and combinations thereof. For example, the metal component can be selected from platinum, palladium, rhodium, iridium and combinations thereof. In some embodiments, the metal component is platinum, or palladium, or a combination of platinum and palladium.

[0060] In some embodiments, two or more PGMs can be combined on the same oxide support. For example, both platinum and palladium can be present on the same oxide support. In other embodiments, the composition further comprises a third component comprising a second PGM supported on a separate second oxide support. For example, platinum and palladium can be present on different oxide supports; one from the first component and the other from the third component. Whether present on the same or different oxide supports, the weight ratio of platinum to palladium can be in the range of about 1:10 to about 10:1, about 1:5 to about 10:1, about 1:1 to about 10:1, about 2:1 to about 10:1, or about 3:1 to about 5:1.

[0061] Each supported PGM can be prepared separately or multiple PGMs can be impregnated on the same support in the same process.

[0062] The metal component can be dispersed on the oxide support by, for example, dispersing a soluble precursor (eg, palladium nitrate) thereon. Alternatively, the metal component is provided in the composition in particulate form, such as fine particles as small as 1 nm to 15 nm or less in diameter.

[0063] The amount of metal component deposited on the oxide support may vary. For example, for H 2 - An exemplary PGM loading of the SCR catalyst composition may be about 1 g / ft 3 About 200g / ft 3 , such as about 10g / ft 3 About 50g / ft 3 . By weight relative to the weight of the oxide support, H 2 - The first component of the SCR catalyst composition may comprise about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1.0%, about 1.1%, about 1.2%, about 1.3%, about 1.4%, about 1.5%, about 1.6%, about 1.7%, about 1.8%, about 1.9% %, about 2.0%, about 3.0%, about 4.0%, or about 5.0% to about 6.0%, about 7.0%, about 8.0%, about 9.0%, about 10.0%, about 11.0%, about 12.0%, about 13.0%, about 14.0%, about 15.0%, about 16.0%, about 17.0%, about 18.0%, about 19.0%, or about 20.0% PGM. In some embodiments, the metal component is present in an amount of about 0.1 wt % to about 10.0 wt % relative to the weight of the oxide support.

[0064] In some embodiments, the oxide support is an oxide of Al, V, W, Ti, Cu, Fe, Ni, Mn, Ce, La, Pr, Zn, Nb, Zr, Mo, Sn, Si, Ca, Y, or a combination thereof. Possible oxide supports include Al 2 O 3 、SiO 2 SnO 2 、CeO 2 、ZrO 2 、MgO、La 2 O 3 , CaO, Y 2 O 3 、TiO 2 、SiO 2 ,FeO x and MnO x In some embodiments, the oxide support is selected from TiO 2 、ZrO 2 、Al 2 O 3 and SiO 2 Oxides of Co, Cr, Ag and Au are not suitable oxide supports for the compositions of the present disclosure.

[0065] In other embodiments, the oxide support is a mixed oxide support. Possible mixed oxide supports include TiO 2 / ZrO 2 、CeO 2 / MgO、WO 3 / ZrO 2 , WO 3 / Al 2 O 3 , WO 3 / TiO 2 , WO 3 / SiO 2 、Al 2 O 3 / La 2 O 3 、TiO 2 / Al 2 O 3 、V 2 O 5 / TiO 2 -Al 2 O 3 , Nb 2 O 5 / SiO 2 、ZnO / Al 2 O 3 、SiO 2 / TiO 2 、SiO 2 / Al 2 O 3 、Mn / TiO 2 / Al 2 O 3 In another embodiment, the oxide support is selected from TiO 2 / ZrO 2 , WO 3 / ZrO 2 , WO 3 / Al 2 O 3 , WO 3 / TiO 2 , WO 3 / SiO 2 、SiO 2 / TiO 2 and SiO 2 / Al 2 O 3 .

[0066] In some embodiments, the metal component of the first component and / or the second PGM of the third component is supported by an oxide / zeolite support. The present disclosure does not relate to H having a first component comprising a zeolite support and no oxide support. 2 - SCR catalyst composition.

[0067] In some embodiments, H 2 -The first component and / or the third component of the SCR catalyst composition may also include an acidic oxide modifier (sometimes referred to as a promoter) on an oxide support. When an acidic oxide modifier is present, the mass ratio of the modifier to the PGM may be in the range of about 1:1 to about 1:30. For example, the mass ratio of the modifier to the PGM may be in the range of about 1:3 to about 1:10. The lower limit of the range may be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9. The upper limit of the range may be 1:10, 1:12, 1:14, 1:16, 1:18, 1:20, 1:22, 1:24, 1:26, 1:28 and 1:30. In certain embodiments, the acidic oxide modifier on the oxide support may be selected from SiO 2 、TiO 2 , Nb 2 O 5 、MoO 3 and combinations thereof. By way of example, SiO 2 Can be used as TiO 2 or Al 2 O 3 The presence of an acidic oxide modifier on the support, or SiO 2 and WO 3 Can be used as ZrO 2 The acidic oxide modifier of the support is present. For example, the acidic modifier may be added to the support as colloidal nanoparticles and is therefore not part of the support. When the oxide is part of a mixed oxide support, " / " is used to indicate the combination, such as Pt / SiO 2 / TiO 2 When an oxide is used as the acidic modifier, this is indicated by a "-", such as Pt-SiO 2 / TiO 2 .

[0068] H 2-SCR catalyst composition comprises a second component comprising zeolite. In some embodiments, the second component is substantially composed of zeolite or is composed of zeolite. The structure type of zeolite can be changed. In certain embodiments, the zeolite has a structure type selected from AEI, AFT, AFX, AVL, *BEA, CHA, DDR, EAB, EEI, ERI, FAU, FER, IFY, IRN, KFI, LEV, LTA, LIN, MOR, MER, MFI, MWF, NPT, PAU, RHO, RTE, RTH, SAS, SAT, SAV, SFW, TSC, UFI and combinations thereof.

[0069] In some embodiments, the zeolite is an acidic zeolite. For example, the zeolite may have a structure type selected from MOR (H-mordenite), *BEA (H-β), FER (H-ferrierite), CHA (H-chabazite), FAU (HY), MFI (H-ZSM-5), and combinations thereof.

[0070] Zeolite for H 2 -SCR catalyst composition has no practical activity. However, when zeolite, especially acidic zeolite, is included as H 2 -SCR catalyst composition, unexpectedly a synergistic effect was observed. The presence of zeolite as the second component increased the NOx conversion performance and reduced the N formed during the catalytic reaction relative to the first component alone. 2 This synergistic effect was not observed when the first component comprised zeolite.

[0071] In other embodiments, H 2 -The second component of the SCR catalyst composition is a metal-promoted zeolite. The metal that promotes the zeolite is generally a base metal (e.g., a transition metal or a lanthanide). In some embodiments, the metal that promotes the zeolite is one or more of Cu, Co, Ni, La, Mn, Fe, V, Ag, Ce, Nd, Mo, Hf, Y, or W. In certain embodiments, the metal that promotes the zeolite is one or more of Cu and Fe. In certain embodiments, the metal that promotes the zeolite is Fe. Mentioning "metal" in this context allows the metal to exist in any valence state. For example, the metal that promotes the zeolite can be in the form of a metal with zero valence, or the metal can be in the form of an oxide. Typically, the metal that promotes the zeolite will exist in the form of an oxide.

[0072] Zeolites typically have a silica to alumina (Si / Al) molar ratio of 2 or greater. 2The zeolite of the SCR catalyst composition has a Si / Al molar ratio in the range of 2:1 to 100:1. In other embodiments, the zeolite has a Si / Al molar ratio in the range of 10:1 to 15:1. Within the Si / Al molar ratio of 10:1 to 15:1, it has been observed that the H of the present disclosure having a FAU or FER structure type 2 -SCR catalyst compositions provide better activity and a wider reaction temperature window at lower temperatures than other structure types. It is theorized that the increased NOx conversion is related to the Bronsted acidity of the zeolite. The lower the Si / Al molar ratio in the zeolite, the higher the acid density the zeolite will provide. However, lower Si / Al molar ratios generally result in zeolites with poorer hydrothermal stability.

[0073] In some embodiments, the catalyst composition has a ratio of the first component to the second component in a range from 95:5 to 10:90.

[0074] H 2 - Preparation of SCR catalyst composition

[0075] According to the present disclosure, H 2 -SCR catalyst compositions are generally prepared by providing a first component comprising a metal component supported by an oxide support, and providing a second component comprising a zeolite. The first component and the second component are initially separate components. If present, the third component may be separate or previously combined with the first component.

[0076] The components can be combined in various ways to form H 2 -SCR catalyst composition. In one embodiment, the components may be physically mixed, such as dry powder mixing. In another embodiment, the components may be combined by dispersing the components in a solvent (such as water) to form a slurry. In yet another embodiment, the components may be co-milled, such as ball milling or wet milling.

[0077] Typically, the catalyst composition is prepared so as to be coated on a substrate. Typical additional components of the catalyst composition include, but are not limited to, additives that control, for example, the pH and viscosity of the catalyst composition to be coated. Additional components may include associative thickeners and / or surfactants (including anionic, cationic, nonionic or amphoteric surfactants). The typical pH range of the catalyst composition to be coated is from about 3 to about 6. Adding an acidic or alkaline substance to the catalyst composition to be coated may be performed to adjust the pH accordingly. For example, in some embodiments, the pH is adjusted downward by adding aqueous acetic acid or nitric acid, or the pH is adjusted upward by adding monoethanolamine.

[0078] The present invention 2-SCR catalyst compositions may also be prepared using a binder, for example, ZrO derived from a suitable precursor such as zirconyl acetate or any other suitable zirconium precursor such as zirconyl nitrate. 2 Binders. Zirconium acetate binders provide coatings that remain uniform and intact after heat aging, for example, when the catalyst is exposed to elevated temperatures of at least about 600°C to about 800°C and higher. Other potentially suitable binders include, but are not limited to, alumina and silica. Alumina binders include aluminum oxide, aluminum hydroxide, and aluminum oxyhydroxide. Aluminum salts and colloidal forms of alumina may also be used. Silica binders include various forms of SiO 2 , including silicates and colloidal silica. The binder composition may include any combination of zirconia, alumina and silica.

[0079] After the components are mixed, the catalyst composition to be coated can be ground to a reduced particle size and enhance the mixing of the particles and the formation of a uniform material. Grinding can be done in a ball mill, a continuous grinder or other similar equipment, and the solid content of the slurry can be, for example, about 20% to 60% by weight, more specifically about 20% to 40% by weight. In one embodiment, the slurry after grinding is characterized in that the D90 particle size is about 1 micron to about 40 microns, preferably 2 microns to about 20 microns, and more preferably about 4 microns to about 15 microns.

[0080] In order to simulate real-world usage, the NOx conversion rate and N 2 Prior to increasing the O formation rate, the catalytic composition may be hydrothermally aged, such as with 10% steam in air at 650°C for 50 hours.

[0081] Catalytic products

[0082] In another aspect of the present disclosure, a selective catalytic reduction (SCR) article effective to catalyze the reduction of nitrogen oxides (NOx) from exhaust gas in the presence of a hydrogen reductant comprises a hydrogen reductant having disposed thereon a hydrogen reductant of the present disclosure. 2 - A substrate for the SCR catalyst composition.

[0083] Base

[0084] In one or more embodiments, the present invention H 2 -SCR catalyst composition is disposed on a substrate to form a catalytic article. Catalytic articles comprising a substrate are generally used as part of an exhaust gas treatment system (e.g., catalyst articles, including but not limited to articles comprising the SCR composition disclosed herein). Useful substrates are three-dimensional, having a length, diameter, and volume similar to a cylinder. The shape does not necessarily have to conform to a cylinder. The length is the axial length defined by the inlet end and the outlet end.

[0085] According to one or more embodiments, the substrate for the disclosed composition can be composed of any material commonly used to prepare automotive catalysts, and will typically include a metal or ceramic honeycomb structure. The substrate typically provides a plurality of wall surfaces to which the washcoat composition is applied and adhered, thereby serving as a substrate for the catalyst composition.

[0086] The ceramic substrate can be made of any suitable refractory material, such as cordierite, cordierite-α-alumina, aluminum titanate, silicon titanate, silicon carbide, silicon nitride, zircon mullite, spodumene, alumina-silica-magnesium, zirconium silicate, sillimanite, magnesium silicate, zircon, petalite, α-alumina, aluminosilicates, etc.

[0087] The substrate may also be metallic, including one or more metals or metal alloys. The metal substrate may include any metal substrate, such as those with openings or "punching holes" in the channel wall. These metal substrates can be used in various shapes, such as pellets, compressed metal fibers, corrugated sheets or monolithic foams. Specific examples of metal substrates include heat-resistant alkali metal alloys, particularly those metal substrates in which iron is a basic or main component. Such alloys may contain one or more of nickel, chromium and aluminum, and the total amount of these metals may advantageously account for at least about 15% by weight (weight percentage) of the alloy based on the weight of the substrate in each case, such as about 10% by weight to about 25% by weight of chromium, about 1% by weight to about 8% by weight of aluminum, and 0% by weight to about 20% by weight of nickel. Examples of metal substrates include those with straight channels; those with protruding blades along the axial channel to interrupt gas flow and open the gas flow between channels; and those metal substrates with blades and holes to enhance gas transmission between channels to allow radial gas transmission throughout the entire body.

[0088] Any suitable substrate for the catalytic articles disclosed herein may be employed, such as a monolithic substrate of the type having thin, parallel gas flow channels extending therethrough from the inlet or outlet face of the substrate, such that the channels are open to fluid flow therethrough (a "flow-through substrate"). Another suitable substrate is of the type having a plurality of thin, substantially parallel gas flow channels extending along the longitudinal axis of the substrate, wherein typically each channel is blocked at one end of the body of the substrate, while alternating channels are blocked at the opposite end face (a "wall flow filter").

[0089] In some embodiments, the catalyst substrate comprises a honeycomb substrate or a flow-through substrate in the form of a wall-flow filter. In some embodiments, the substrate is a wall-flow filter. In some embodiments, the substrate is a flow-through substrate. For example, flow-through and wall-flow substrates are also taught in International Application Publication No. WO 2016 / 070090 and U.S. Patent Application Publication No. 2012 / 0178380A1, which are incorporated herein by reference in their entirety.

[0090] Substrate coating process

[0091] To produce the SCR articles of the present disclosure, H as disclosed herein is used. 2 - SCR catalyst composition coated substrate.

[0092] The present invention 2 -SCR catalyst compositions may typically be prepared in the form of H 2 The washcoat is applied in the form of one or more washcoats of the H-SCR catalyst composition. The washcoat is formed by preparing a slurry of the catalyst composition containing a specified solid content (e.g., about 10% to about 60% by weight) in a liquid carrier, which is then applied to the substrate using any washcoat technique known in the art and dried and calcined to provide a coating. If multiple washcoats are applied, the substrate is dried and / or calcined after each washcoat is applied and / or after the desired number of washcoats are applied. In one embodiment, H 2 - The SCR catalyst composition is applied to the substrate as a single washcoat.

[0093] After calcination, the catalyst loading obtained by the above-described washcoat technique can be determined by calculating the difference between the coated and uncoated weights of the substrate. As will be apparent to one skilled in the art, the catalyst loading can be modified by altering the slurry rheology. In addition, the coating / drying / calcining process to generate the washcoat (coating) can be repeated as needed to build up the coating to the desired loading level or thickness, meaning that more than one washcoat may be applied.

[0094] The catalytic coating of the present invention may comprise one or more coatings, at least one of which comprises the H 2 - SCR catalyst composition or one or more components of a catalyst composition. The catalytic coating may include one or more thin adherent coatings disposed on and adhered to at least a portion of the substrate. The entire coating comprises a single "coat layer".

[0095] In some embodiments, the catalytic articles of the present invention may include the use of one or more catalyst layers and combinations of one or more catalyst layers. The catalytic material may be present alone on the inlet side of the substrate wall, alone on the outlet side, on both the inlet side and the outlet side, or the wall itself may be composed entirely or partially of the catalytic material. The catalytic coating may be on the surface of the substrate wall and / or in the pores of the substrate wall, i.e., "in the substrate wall" and / or "on the substrate wall". Therefore, the phrase "a repair substrate coating disposed on a substrate" means on any surface, such as on the wall surface and / or on the pore surface.

[0096] A washcoat may be applied so that the different coatings are in direct contact with the substrate. Alternatively, there may be one or more "undercoats" so that at least a portion of the one or more catalytic coatings is not in direct contact with the substrate (but is in contact with the undercoat). There may also be one or more "overcoats" so that at least a portion of the one or more coatings is not directly exposed to the gas stream or atmosphere (but is in contact with the overcoat).

[0097] Alternatively, the present invention H 2 - The SCR catalyst composition may be in a top coating over a bottom coating. 2 - The SCR catalyst composition may be present in a top layer and a bottom layer. Any one layer may extend the entire axial length of the substrate, for example the bottom layer may extend the entire axial length of the substrate, and the top layer may also extend the entire axial length of the substrate above the bottom layer. Each of the top layer and the bottom layer may extend from either the inlet end or the outlet end.

[0098] For example, the bottom coating and the top coating can extend from the same substrate end, wherein the top layer partially or completely covers the bottom layer, and wherein the bottom layer extends part or all of the length of the substrate, and wherein the top layer extends part or all of the length of the substrate. Alternatively, the top layer can cover a portion of the bottom layer. For example, the bottom layer can extend the entire length of the substrate, and the top layer can extend about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80% or about 90% of the length of the substrate from either the inlet end or the outlet end.

[0099] Alternatively, the bottom layer may extend about 10%, about 15%, about 25%, about 30%, about 40%, about 45%, about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, or about 95% of the length of the substrate from either the inlet end or the outlet end, and the top layer may extend about 10%, about 15%, about 25%, about 30%, about 40%, about 45%, about 50%, about 55%, about 60%, about 65%, about 70%, about 75%, about 80%, about 85%, or about 95% of the length of the substrate from either the inlet end or the outlet end, wherein at least a portion of the top layer covers the bottom layer. This "coverage" zone may, for example, extend from about 5% to about 80% of the length of the substrate, such as about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60% or about 70% of the length of the substrate.

[0100] In some embodiments, a H as disclosed herein disposed on a substrate as disclosed herein 2 The SCR catalyst composition comprises a first washcoat layer comprising H 2 - An SCR catalyst composition wherein a first washcoat layer is disposed over at least a portion of the length of the catalyst substrate; and a second washcoat layer having the same or a different composition is disposed over at least a portion of the length of the catalyst substrate.

[0101] In some embodiments, the first washcoat layer is disposed directly on the catalyst substrate, and the second washcoat layer is disposed on at least a portion of the first washcoat layer. In some embodiments, the second washcoat layer is disposed directly on the catalyst substrate, and the first washcoat layer is disposed on at least a portion of the second washcoat layer. In some embodiments, the first washcoat layer is disposed directly on the catalyst substrate from the inlet end to a length of about 10% to about 50% of the total length; and the second washcoat layer is disposed on at least a portion of the first washcoat layer. In some embodiments, the second washcoat layer is disposed directly on the catalyst substrate from the inlet end to a length of about 50% to about 100% of the total length; and the first washcoat layer is disposed on at least a portion of the second washcoat layer. In some embodiments, the first washcoat layer is disposed directly on the catalyst substrate from the inlet end to a length of about 20% to about 40% of the total length, and the second washcoat layer extends from the inlet end to the outlet end. In some embodiments, the first washcoat layer is disposed directly on the catalyst substrate from the outlet end to a length of about 10% to about 50% of the total length, and the second washcoat layer is disposed on at least a portion of the first washcoat layer. In some embodiments, the first washcoat layer is disposed directly on the catalyst substrate from the outlet end to a length of about 20% to about 40% of the total length, and the second washcoat layer extends from the inlet end to the outlet end. In some embodiments, the second washcoat layer is disposed directly on the catalyst substrate from the outlet end to a length of about 50% to about 100% of the total length, and the first washcoat layer is disposed on at least a portion of the second washcoat layer. In some embodiments, the first washcoat layer is disposed directly on the catalyst substrate, covering 100% of the total length, and the second washcoat layer is disposed on the first washcoat layer, covering 100% of the total length. In some embodiments, the second washcoat layer is disposed directly on the catalyst substrate, covering 100% of the total length, and the first washcoat layer is disposed on the second washcoat layer, covering 100% of the total length.

[0102] The catalytic coating can advantageously be "partitioned", comprising a partitioned catalytic layer, that is, wherein the catalytic coating comprises different compositions on the axial length of the substrate. This can also be described as "lateral partitioning". For example, a layer can extend from the inlet end toward the outlet end, extending about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80% or about 90% of the length of the substrate. Another layer can extend from the outlet end toward the inlet end, extending about 10%, about 20%, about 30%, about 40%, about 50%, about 60%, about 70%, about 80% or about 90% of the length of the substrate. Different coatings can be adjacent to each other and do not cover each other. Alternatively, different layers can cover a portion of each other, thereby providing a third "middle" zone. The intermediate zone may, for example, extend from about 5% to about 80% of the length of the substrate, such as about 5%, about 10%, about 20%, about 30%, about 40%, about 50%, about 60% or about 70% of the length of the substrate.

[0103] The zones of the present disclosure are defined by the relationship of the coatings. There are several possible zone configurations with respect to the different coatings. For example, there can be an upstream zone and a downstream zone, there can be an upstream zone, an intermediate zone, and a downstream zone, there can be four different zones, etc. In the case where the two layers are adjacent and do not overlap, there are upstream zones and downstream zones. In the case where the two layers overlap to a certain extent, there are upstream zones, downstream zones, and intermediate zones. For example, when the coatings extend the entire length of the substrate and the different coatings extend a certain length from the outlet end and cover a portion of the first coating, there are upstream zones and downstream zones.

[0104] For example, the article may include an upstream region comprising a 2 - a first washcoat layer of an SCR catalyst composition; and a downstream zone comprising a second washcoat layer of the same or different composition.

[0105] Alternatively, the upstream zone may include the second washcoat layer and the downstream zone may include the first washcoat layer.

[0106] In some embodiments, the first washcoat layer is disposed on the catalyst substrate from the inlet end to a length of about 10% to about 50% of the total length; and the second washcoat layer is disposed on the catalyst substrate from the outlet end to a length of about 50% to about 90% of the total length. In some embodiments, the first washcoat layer is disposed on the catalyst substrate from the outlet end to a length of about 10% to about 50% of the total length; and wherein the second washcoat layer is disposed on the catalyst substrate from the inlet end to a length of about 50% to about 90% of the total length.

[0107] In some embodiments, the catalytic article may also include a diesel oxidation catalyst (DOC) composition, which may be 2- In the zone downstream of the SCR catalyst composition, the upper layer contains H 2 - in the bottom layer of the SCR catalyst article, or in which the DOC composition is mixed with H 2 -SCR catalyst composition. In other embodiments, the catalytic article may also include a low temperature NOx adsorbent (LTNA). The LTNA functional group may be part of the DOC composition, H 2 - a portion of the SCR catalytic composition, the DOC composition and H 2 - a portion of both the SCR catalytic composition and the DOC composition and the H 2 - SCR catalytic composition separately, or a combination thereof.

[0108] Exhaust gas treatment system

[0109] In another aspect of the present disclosure, an emission treatment system for selectively reducing NOx compounds from an exhaust gas stream includes a H 2 Another embodiment may be characterized in that it comprises H 2 -SCR catalyst composition and NH 3 - System of SCR catalyst composition.

[0110] In other embodiments, the exhaust treatment system may further include a hydrogen generator or a hydrogen injector. The hydrogen generator or the hydrogen may be fluidly connected and in the H 2 - Upstream of the SCR catalytic article. Such a system may also include pumps, reservoirs, etc. The hydrogen generator may vary and may be selected from onboard hydrogen, hydrogen produced by alcohol reforming, hydrogen produced by ammonia decomposition, hydrogen produced by hydrocarbon reforming, and mixtures thereof.

[0111] In some embodiments, the emission treatment system may further include a lean NOx trap (LNT) catalytic article including a substrate and an LNT catalyst composition, the LNT catalytic article being in fluid communication with and in contact with the H 2 - Downstream of the SCR catalytic product.

[0112] The relative placement of the various components present in the emission treatment system can be varied. In the exhaust treatment systems and methods of the present invention, the exhaust gas flow is received into the SCR article or treatment system by entering the upstream end and exiting the downstream end. The inlet end of the substrate of the article is synonymous with the "upstream" end or "front" end. The outlet end is synonymous with the "downstream" end or "rear" end. Generally speaking, the treatment system is downstream of an internal combustion engine (such as a diesel engine or a hydrogen internal combustion engine) and is in fluid communication with it.

[0113] Method for treating engine exhaust gas

[0114] Another aspect of the present invention relates to a method for treating an exhaust gas stream containing NOx compounds. In some embodiments, the method includes treating the exhaust gas stream during a cold phase or cold start phase, i.e., wherein the exhaust gas temperature is about 200°C or less, about 175°C or less, about 150°C or less, about 125°C or less, or about 100°C or less. In some embodiments, the method includes treating the exhaust gas stream, wherein the exhaust gas temperature is about 100°C to about 250°C.

[0115] The method may include treating H according to the present disclosure 2 - The SCR catalyst article is placed downstream of the engine and the engine exhaust stream is directed through the catalyst. In one or more embodiments, the method further comprises placing an additional catalyst component downstream of the engine as described above.

[0116] The present invention 2 -SCR catalyst compositions, articles, systems and methods are suitable for treating exhaust gas streams from diesel engines and hydrogen internal combustion engines. 2 The SCR catalyst composition is also suitable for treating NOx emissions from stationary industrial processes, from indoor air, or for catalysis in chemical reaction processes.

[0117] It will be readily apparent to those skilled in the art that suitable modifications and changes may be made to the compositions, methods, and applications described herein without departing from the scope of any embodiment or aspect thereof. The compositions and methods provided are exemplary and are not intended to limit the scope of the claimed embodiments. All various embodiments, aspects, and options disclosed herein may be combined in all variations. The scope of the compositions, methods, and applications described herein includes all actual or potential combinations of the embodiments, aspects, options, examples, and preferences herein. All patents and publications cited herein are incorporated herein by reference for their specific teachings as described, unless other specific incorporation statements are specifically provided.

[0118] Before describing exemplary embodiments of the present disclosure, it should be understood that the present disclosure is not limited to the details of construction or process steps set forth in the following examples and is capable of other embodiments and of being practiced or carried out in various ways.

[0119] Implementation plan:

[0120] The invention is further illustrated by the following set of embodiments and combinations of embodiments resulting from the indicated dependencies and back-references. In particular, it should be noted that in each case where a scope of embodiments is mentioned, for example in the context of a term such as "a method according to any one of embodiments 1 to 4", each embodiment within the scope is meant to be explicitly disclosed to the skilled person, i.e. the wording of the term should be understood by the skilled person as being synonymous with "a method according to any one of embodiments 1, 2, 3 and 4". Furthermore, it is explicitly noted that the following set of embodiments is not a set of claims determining the degree of protection, but rather represents a properly structured part of the description of general and preferred aspects of the invention.

[0121] Embodiment 1. A hydrogen selective catalytic reduction (H2-SCR) catalyst composition effectively used to reduce nitrogen oxides (NOx) from engine exhaust in the presence of a hydrogen reductant, the H2-SCR catalyst composition comprising: (i) a first component, the first component comprising a platinum group metal (PGM) supported by an oxide carrier; and (ii) a second component, the second component comprising a zeolite.

[0122] Embodiment 2. H according to embodiment 1 2 -SCR catalyst composition, wherein the metal component is a PGM selected from platinum (Pt), palladium (Pd), rhodium (Rh), iridium (Ir), and combinations thereof. When coated on a substrate, an exemplary PGM loading may be about 1 g / ft 3 About 200g / ft 3 , such as about 10g / ft 3 About 50g / ft 3 In addition, the composition may include about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1.0%, about 1.1%, about 1.2%, about 1.3%, about 1.4%, about 1.5%, about 1.6%, about 1.7%, about 1.8%, about 1.9%, about 2.0%, about 3.0%, about 4.0%, or about 5.0% to about 6.0%, about 7.0%, about 8.0%, about 9.0%, about 10.0%, about 11.0%, about 12.0%, about 13.0%, about 14.0%, about 15.0%, about 16.0%, about 17.0%, about 18.0%, about 19.0% or about 20.0% PGM.

[0123] Embodiment 3. H according to embodiment 2 2 - An SCR catalyst composition, wherein the PGM is Pt.

[0124] Embodiment 4. H according to embodiment 2 2 - An SCR catalyst composition, wherein the PGM is Pd.

[0125] Embodiment 5. H according to any one of embodiments 1 to 4 2 - An SCR catalyst composition further comprising a second PGM supported on the oxide support.

[0126] Embodiment 6. H according to embodiment 5 2 -SCR catalyst composition, wherein the second PGM is Pd. For example, when the metal component is Pt, the Pt to Pd weight ratio may be in the range of about 1:10 to about 10:1, about 1:5 to about 10:1, about 1:1 to about 10:1, about 2:1 to about 10:1, or about 3:1 to about 5:1.

[0127] Embodiment 7. H according to any one of embodiments 1 to 6 2 - An SCR catalyst composition further comprising a third component comprising a second PGM supported on a second oxide support.

[0128] Embodiment 8. H according to embodiment 7 2 -SCR catalyst composition, wherein the metal component is Pt and the second PGM is Pd. For example, the Pt to Pd weight ratio can be in the range of about 1:10 to about 10:1, about 1:5 to about 10:1, about 1:1 to about 10:1, about 2:1 to about 10:1, or about 3:1 to about 5:1.

[0129] Embodiment 9. H according to any one of embodiments 1 to 8 2 - An SCR catalyst composition, wherein the metal component is present in an amount of about 0.1 wt. % to about 10 wt. % by weight relative to the weight of the oxide support.

[0130] Embodiment 10. H according to any one of embodiments 1 to 9 2 -SCR catalyst composition, wherein the oxide support is an oxide of aluminum (Al), vanadium (V), tungsten (W), titanium (Ti), copper (Cu), iron (Fe), nickel (Ni), manganese (Mn), cerium (Ce), lanthanum (La), praseodymium (Pr), zinc (Zn), niobium (Nb), zirconium (Zr), molybdenum (Mo), tin (Sn), silicon (Si), calcium (Ca), yttrium (Y) or a combination thereof. For example, the oxide support is an oxide of copper, iron, manganese, tin, aluminum, zirconium, silicon, titanium, tungsten, molybdenum, nickel or a combination thereof.

[0131] Embodiment 11. H according to embodiment 10 2-SCR catalyst composition, wherein the oxide support is selected from Al 2 O 3 、SiO 2 SnO 2 、CeO 2 、ZrO 2 、MgO、La 2 O 3 , CaO, Y 2 O 3 、TiO 2 、SiO 2 ,FeO x and MnO x , such as selected from TiO 2 、ZrO 2 、Al 2 O 3 and SiO 2 .

[0132] Embodiment 12. H according to any one of embodiments 1 to 10 2 - An SCR catalyst composition, wherein the oxide support is a mixed oxide support.

[0133] Embodiment 13. H according to embodiment 12 2 -SCR catalyst composition, wherein the mixed oxide is selected from TiO 2 / ZrO 2 、CeO 2 / MgO、WO 3 / ZrO 2 , WO 3 / Al 2 O 3 , WO 3 / TiO 2 , WO 3 / SiO 2 、Al 2 O 3 / La 2 O 3 、TiO 2 / Al 2 O 3 、V 2 O 5 / TiO 2 -Al 2 O 3 , Nb 2 O 5 / SiO 2 、ZnO / Al 2 O 3 、SiO 2 / TiO2 、SiO 2 / Al 2 O 3 、Mn / TiO 2 / Al 2 O 3 and perovskites. For example, the mixed oxide is selected from TiO 2 / ZrO 2 , WO 3 / Al 2 O 3 , WO 3 / TiO 2 , WO 3 / SiO 2 , WO 3 / ZrO 2 and SiO 2 / TiO 2 , and SiO 2 / Al 2 O 3 .

[0134] Embodiment 14. H according to any one of embodiments 1 to 13. 2 - An SCR catalyst composition further comprising an acidic oxide modifier on the oxide support.

[0135] Embodiment 15. The H according to embodiment 14 2 -SCR catalyst composition, wherein the acidic oxide modifier is selected from SiO 2 , WO 3 , Nb 2 O 5 、MoO 3 and TiO 2 .

[0136] Embodiment 16. H according to any one of embodiments 1 to 15 2 - An SCR catalyst composition wherein the mass ratio of the metal component to the acidic oxide modifier is in the range of about 1:1 to about 1:30.

[0137] Embodiment 17. H according to any one of embodiments 1 to 16 2 - An SCR catalyst composition wherein the mass ratio of the metal component to the acidic oxide modifier is in the range of about 1:3 to about 1:10.

[0138] Embodiment 18. H according to any one of embodiments 1 to 17 2 - An SCR catalyst composition, wherein the zeolite is an acidic zeolite.

[0139] Embodiment 19. H according to any one of embodiments 1 to 18 2 - An SCR catalyst composition, wherein the second component consists essentially of an acidic zeolite.

[0140] Embodiment 20. H according to any one of embodiments 1 to 19. 2 -SCR catalyst composition, wherein the zeolite is a metal-promoted zeolite. For example, the metal promoting the zeolite is one or more of Cu, Co, Ni, La, Mn, Fe, V, Ag, Ce, Nd, Mo, Hf, Y and W.

[0141] Embodiment 21. The H according to embodiment 20 2 - An SCR catalyst composition, wherein the metal promoted zeolite is selected from the group consisting of Fe / zeolite, Cu / zeolite and Fe / Cu / zeolite.

[0142] Embodiment 22. H according to any one of embodiments 1 to 21 2 - An SCR catalyst composition, wherein the zeolite comprises more than one structure type.

[0143] Embodiment 23. H according to any one of embodiments 1 to 22 2 -SCR catalyst composition, wherein the zeolite has a structure type selected from the group consisting of AEI, AFT, AFX, AVL, *BEA, CHA, DDR, EAB, EEI, ERI, FAU, FER, IFY, IRN, KFI, LEV, LTA, LIN, MOR, MER, MFI, MWF, NPT, PAU, RHO, RTE, RTH, SAS, SAT, SAV, SFW, TSC, UFI and combinations thereof.

[0144] Embodiment 24. The H according to embodiment 23 2 - An SCR catalyst composition, wherein the zeolite is selected from the group consisting of FAU, *BEA, MOR, MFI, CHA, FER and combinations thereof.

[0145] Embodiment 25. The catalyst composition of any one of Embodiments 1 to 24, wherein the zeolite has a Si / Al molar ratio in the range of 2:1 to 100:1, such as in the range of 10:1 to 15:1.

[0146] Embodiment 26. The catalyst composition according to any one of Embodiments 1 to 25, wherein the first component and the second component are added in a mass ratio ranging from 95:5 to 10:90.

[0147] Embodiment 27. H according to any one of embodiments 1 to 26 2-SCR catalyst composition, wherein the first component and the second component are combined into a composite material by: (1) physically mixing the first component and the second component; (2) dispersing the first component and the second component in water to form a slurry; (3) co-grinding the first component and the second component; or (4) a combination thereof.

[0148] Embodiment 28. A method for effectively catalyzing the reduction of nitrogen oxides (NO x ) is a selective catalytic reduction (SCR) product for reduction, the SCR product comprising a H according to any one of embodiments 1 to 27 disposed thereon 2 - A substrate for the SCR catalyst composition.

[0149] Embodiment 29. A method for selectively reducing NO from an exhaust gas stream x An emission treatment system for a compound, the system comprising the SCR article according to embodiment 28. Embodiment 30. The emission treatment system according to embodiment 29, further comprising a hydrogen generator or a hydrogen injector.

[0150] Embodiment 31. A method for treating an exhaust gas stream containing NOx compounds, the method comprising passing the exhaust gas stream through an emission treatment system according to any one of Embodiments 29 to 30.

[0151] Embodiment 32. A method for treating an exhaust gas stream according to Embodiment 31, wherein the exhaust gas stream is an exhaust gas stream of a hydrogen internal combustion engine or an exhaust gas stream of a diesel engine treated with hydrogen.

[0152] Claims or specific embodiments that include "or" or "and / or" between at least one member of the group are considered satisfied if one, more than one, or all of the group members are present in, used in, or otherwise related to a given product or method, unless indicated to the contrary or otherwise obvious from the context. The present disclosure includes embodiments in which exactly one member of the group is present in, used in, or otherwise related to a given product or method. The present disclosure includes embodiments in which more than one or all of the group members are present in, used in, or otherwise related to a given product or method.

[0153] In addition, the present disclosure encompasses all variations, combinations and arrangements, wherein at least one limitation, element, clause and descriptive term from at least one of the listed claims is introduced into another claim. For example, any embodiment / claim subordinate to another embodiment / claim can be modified to be included in at least one limitation found in any other embodiment / claim subordinate to the same basic embodiment / claim. In the case where an element exists in a list (such as, for example, in Markush (Markush) group format), each subgroup of the element is also disclosed, and any element can be removed from the group. It should be understood that, generally speaking, in the case where the present disclosure or the various aspects of the present disclosure are referred to as including specific elements and / or features, the embodiments of the present disclosure or the various aspects of the present disclosure are made up of or substantially made up of such elements and / or features. For simplicity, these embodiments are not specifically described herein. In the case where a range (such as, for example, from [X] to [Y]) is given, endpoints (such as, for example, [X] and [Y] in the phrase "from [X] to [Y]") are included, unless otherwise indicated. In addition, unless otherwise indicated or apparent from the context and understanding of one of ordinary skill in the art, values ​​expressed in ranges may assume any specific value or sub-range within the stated range in the various embodiments of the present disclosure, to the tenth of the lower limit of the range, unless the context clearly indicates otherwise.

[0154] Using only routine experimentation, those skilled in the art will recognize or be able to ascertain many equivalents to the specific embodiments of the disclosure described herein. Such equivalents are intended to be encompassed by the following non-limiting examples. Example

[0155] The following examples are intended to be illustrative, and are not meant to limit the scope of the present disclosure in any way.

[0156] Unless otherwise stated, the evaluation of the catalytic activity of the samples listed below was conducted on a continuous flow fixed bed quartz tube reactor with an inner diameter of 4 mm. 26 mg (40 mesh-60 mesh) of the catalyst sample was diluted with 0.25 g of inert SiC powder (40 mesh-60 mesh) to minimize any hot spots. For the zeolite-containing catalyst (PGM / oxide + zeolite), the samples contained the same amount of metal as the PGM / oxide sample. The feed gas mixture contained 500 ppm NO, 1% H 2 , 10% O 2 , 5% CO 2 and 5% H 2 O and the balance Ar, flow rate is 200 cm 3 / min, which results in a weight hourly space velocity (WHSV) of 461,500 mLg -1 h -1The reactants and products were analyzed online using a MultiGas 2030CEMcert FTIR spectrometer coupled to a mass spectrometer (MS, Hiden Analytical). The m / z ratios of 32 and 2 were used for O 2 and H 2 Detection. NO x The conversion rate is defined as (C NOx-inlet -C NOx-outlet ) / C NOx-inlet × 100%, where C NOx-inlet and C NOx-outlet are the NO at the catalyst inlet and outlet, respectively. x (NO+NO 2 ) concentration. 2 The O yield is defined as C N2O-outlet ×2 / C NOx-inlet × 100%, where C N2O-outlet It is exit N 2 O concentration.

[0157] Example 1: 1Pt-8Si / TiO 2 + Preparation and evaluation of zeolite catalysts

[0158] Table 1 lists the dual-component catalysts of the present disclosure and the single-component reference catalyst. Sample 1 is a reference catalyst, and colloidal Pt nanoparticles and colloidal SiO 2 The mixed solution of nanoparticles (acidic oxide modifier) ​​was impregnated on TiO 2 The colloidal Pt particle size is between 1nm and 4nm. 2 The average particle size of the Pt and SiO2 was about 12 nm. After impregnation, the resulting material was calcined at 550 °C for 2 h in air. 2 The concentrations were 1 wt% and 8 wt%, respectively. Samples 2 to 7 were prepared by mechanically mixing the reference catalyst with the zeolite component in a 1:1 weight ratio. The zeolites in samples 2 to 7 were β (Si / Al=12.5:1), ferrierite (Si / Al=10:1), chabazite (Si / Al=14.5:1), Y (Si / Al=15:1), ZSM-5 (Si / Al=15:1) and H-type of mordenite (Si / Al=10:1), respectively. All samples (including the reference sample) were hydrothermally aged at 650°C with 10% steam in air for 50 hours. All samples in Table 1 contained the same amount of Pt.

[0159] Table 1

[0160] Sample No. Sample name PGM / Oxide Zeolite Mixing ratio 1 <![CDATA[1Pt-8SiO 2 / TiO 2 (Reference)]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> N / A NA 2 <![CDATA[1Pt-8SiO 2 / Ten 2 +BEA]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> H-β 1:1 3 <![CDATA[1Pt-8SiO 2 / TiO 2 +FER]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> H-Ferrierite 1:1 4 <![CDATA[1Pt-8SiO 2 / Uncle 2 +CHA]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> H-chabazite 1:1 5 <![CDATA[1Pt-8SiO 2 / Uncle 2 +Y]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> HY(FAU) 1:1 6 <![CDATA[1Pt-8SiO 2 / TiO 2 +ZSM5]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> H-ZSM-5(MFI) 1:1 7 <![CDATA[1Pt-8SiO 2 / TiO 2 +MOTHER]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> H-Mordenite 1:1

[0161] like Figure 1A and Figure 1B As shown, they compare the NO x Conversion rate and N 2 O formation rate, samples 2-7 showed higher NO formation rates than reference sample 1 (reference sample) at most of the tested temperatures. x Conversion rate and lower N 2 O formation. Sample 5 (zeolite Y) promotes NO x The most active in terms of conversion, while sample 2 (catalyst containing zeolite*β) has the lowest N 2 O is formed.

[0162] Example 2: 1Pt-8SiO 2 / TiO 2 +Y catalyst preparation and evaluation

[0163] Table 2 lists the samples prepared from two different types of component combinations and their corresponding references. Samples 1 and 5 were prepared as described in Example 1.

[0164] Sample 8 is a reference catalyst and was prepared by impregnating colloidal Pt nanoparticles on zeolite HY (Si / Al=15:1) using the incipient wetness technique. 8% SiO 2 / TiO 2 By adding colloidal SiO 2 Nanoparticles (acidic oxide modifiers) are impregnated in TiO 2 The prepared substrate was prepared by mechanically mixing 1Pt / Y and 8% SiO in a 1:1 weight ratio. 2 / TiO 2 Comparative Sample 9 was prepared. All samples were hydrothermally aged at 650°C with 10% steam in air for 50 hours.

[0165] Table 2

[0166] Sample No. Sample name Oxide Zeolite Mixing ratio 1 <![CDATA[1Pt-8SiO 2 / TiO 2 (Reference)]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> N / A NA 5 <![CDATA[1Pt-8SiO 2 / Uncle 2 +Y]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> HY 1:1 8 1Pt / Y(reference) NA 1%Pt / HY NA 9 <![CDATA[1Pt / Y+8SiO 2 / TiO 2 ]]> <![CDATA[8%SiO 2 / TiO 2 ]]> 1%Pt / HY 1:1

[0167] like Figure 2A and Figure 2B As shown, they compare the NO x Conversion rate and N 2 O formation rate, compared with the reference sample 1(1Pt-8SiO 2 / TiO 2 Compared with the reference sample 8 (directly loaded with Pt on zeolite HY), the reference sample 8 (directly loaded with Pt on zeolite HY) resulted in a lower NOx conversion. 2 / TiO 2 ) improves NOx conversion but increases N 2O formation. Overall, the highest NOx conversion across the entire temperature window was observed on Sample 5. Although Sample 5 and Comparative Sample 9 contained Pt, SiO 2 , TiO2 and HY zeolite, but significantly different NOx conversion and N 2 O formation rate.

[0168] Example 3: 1Pt-8SiO with different oxide to zeolite ratios 2 / TiO 2 +Y catalyst preparation and evaluation

[0169] Table 3 lists the reference sample 1 and the 1Pt-8SiO 2 / TiO 2 1Pt-8SiO with Y 2 / TiO 2 +Y catalyst. The catalyst was prepared in the same manner as in Example 1 and aged under the same conditions. All samples were hydrothermally aged at 650°C with 10% steam in air for 50 hours. All samples in Table 3 contained the same amount of Pt.

[0170] Table 3

[0171] Sample No. Sample name PGM / Oxide Zeolite Mixing ratio 1 <![CDATA[1Pt-8 SiO 2 / TiO 2 (Reference)]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> N / A NA 10 <![CDATA[1Pt-8 SiO 2 / Uncle 2 +Y_2:1]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> HY 2:1 5 <![CDATA[1Pt-8 SiO 2 / Uncle 2 +Y_1:1]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> HY 1:1 11 <![CDATA[1Pt-8 SiO 2 / Uncle 2 +Y_1:2]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> HY 1:2

[0172] like Figure 3A and Figure 3B As shown, they compare the NO x Conversion rate and N 2 O formation rate, all zeolite-containing samples showed higher NO x Conversion rate and lower N 2 O is formed regardless of the mixing ratio.

[0173] Example 4: 0.5Pt-4SiO 2 / TiO 2 Preparation and evaluation of 0.5Pt / Y catalysts

[0174] Table 4 lists the four catalyst samples. Sample 5 and Comparative Sample 9 were prepared as described in Examples 1 and 2, respectively. Reference Sample 12 was prepared in the same manner as Reference Sample 1 described in Example 1, but with 50% Pt and SiO 2 (acidic oxide modifier) ​​concentration. Similarly, reference sample 13 was prepared in the same manner as reference sample 8 described in Example 2, but with a Pt concentration of 50%. All four samples in Table 4 contained the same amount of Pt in the final catalyst, i.e., 0.5 wt. % relative to the catalyst weight. All samples were hydrothermally aged at 650° C. with 10% steam in air for 50 hours.

[0175] Table 4

[0176] Sample No. Sample name Oxide Zeolite Mixing ratio 12 <![CDATA[0.5Pt-4SiO 2 / TiO 2 (Reference)]]> <![CDATA[0.5% Pt-4%SiO 2 / TiO 2 ]]> NA NA 13 0.5Pt / Y(reference) NA 0.5%Pt / HY NA 5 <![CDATA[1Pt-8SiO 2 / Uncle 2 +Y]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> HY 1:1 9 <![CDATA[1Pt / Y+8SiO 2 / TiO 2 ]]> <![CDATA[8%SiO 2 / TiO 2 ]]> 1%Pt / HY 1:1

[0177] like Figure 4A and Figure 4B As shown, they compare the NO x Conversion rate and N 2 O formation rate, lower concentrations of Pt and SiO 2 Affects NOx conversion rate and N 2 O formation rate. For example, reference sample 13 shows the lowest NO formation rate at low temperatures. x conversion rate, while sample 5 showed the highest NO x Conversion rate.

[0178] Example 5: 1Pt-8SiO 2 / TiO 2 +1CuCHA catalyst preparation and evaluation

[0179] Table 5 lists reference sample 1, two-component sample 4 (where the zeolite is H-chabazite), and two-component sample 14 (where the H-chabazite of sample 4 is replaced by Cu-chabazite). Reference sample 1 and sample 4 were prepared as described in Example 1. Sample 14 was prepared similarly to sample 4, but with Cu-chabazite (1% CuO) replacing the H-chabazite (Si / Al=14.5:1) of sample 4. All samples were hydrothermally aged at 650°C with 10% steam in air for 50 hours.

[0180] Table 5

[0181] Sample No. Sample name PGM / Oxide Zeolite Mixing ratio 1 <![CDATA[1Pt-8SiO 2 / TiO 2 (Reference)]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> N / A NA 4 <![CDATA[1Pt-8SiO 2 / Uncle 2 +CHA]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> H-chabazite 1:1 14 <![CDATA[1Pt-8SiO 2 / TiO 2 +1CuCHA]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> Cu-Chabazite (1%CuO) 1:1

[0182] like Figure 5A and Figure 5B As shown, they compare the NO x Conversion rate and N 2 O formation rate, sample 14 shows similar NO formation rate to sample 4 at lower temperature x However, at higher temperatures, Sample 14 showed lower NO conversion than either Reference Sample 1 or Sample 4. x Conversion rate.

[0183] Example 6: Catalyst preparation and evaluation of Pt / Pd and Pd catalysts

[0184] Table 6 lists the TiO 2 Catalysts containing Pt / Pd or Pd on a support. Colloidal Pt, Pd nitrate and colloidal SiO in appropriate composition ratios are prepared by using the incipient wetness technique. 2 The solution mixture of (acidic oxide modifier) ​​was impregnated on TiO 2 Reference samples 15 and 17 were prepared as above (Pt / Pd weight ratio was 8 / 1 for reference sample 15 and 4 / 1 for reference sample 17, both with 8 wt% SiO 2). Reference sample 19 was prepared in the same manner as reference sample 1 in Example 1, but with Pd nitrate instead of colloidal Pt of reference sample 1. Samples 16, 18 and 20 were prepared by mechanically mixing the corresponding reference catalysts of reference samples 15, 17 and 19 with the HY zeolite component in a 1:1 weight ratio. For all samples, the PGM concentration on the support after calcination was 1 wt%. All samples (including the reference sample) were hydrothermally aged at 650°C with 10% steam in air for 50 hours.

[0185] Table 6

[0186] Sample No. Sample name PGM / Oxide Zeolite Mixing ratio 15 <![CDATA[Pt 8 Pd 1 -8SiO 2 / TiO 2 (Reference)]]> <![CDATA[1%PGM(Pt / Pd=8:1)-8%SiO 2 / TiO 2 ]]> N / A NA 16 <![CDATA[Pt 8 P.S 1 -8SiO 2 / Uncle 2 +Y]]> <![CDATA[1%PGM(Pt / Pd=8:1)-8%SiO 2 / TiO 2 ]]> HY 1:1 17 <![CDATA[Pt 4 Pd 1 -8SiO 2 / TiO 2 (Reference)]]> <![CDATA[1%PGM(Pt / Pd=4:1)-8%SiO 2 / TiO 2 ]]> N / A NA 18 <![CDATA[Pt 4 P.S 1 -8SiO 2 / Uncle 2 +Y]]> <![CDATA[1%PGM(Pt / Pd=4:1)-8%SiO 2 / TiO 2 ]]> HY 1:1 19 <![CDATA[1Pd-8SiO 2 / TiO 2 (Reference)]]> <![CDATA[1%Pd-8%SiO 2 / TiO 2 ]]> N / A NA 20 <![CDATA[1Pd-8SiO 2 / Uncle 2 +Y]]> <![CDATA[1%Pd-8%SiO 2 / TiO 2 ]]> HY 1:1

[0187] like Fig. 6A and Figure 6B As shown, they compare the NO x Conversion rate and N 2 O formation rate, sample 20 (Pd catalyst with HY-zeolite added) relative to that with equivalent N 2 O formed in reference sample 19 in NO x Samples 16 and 18 (PtPd catalysts) show that the addition of HY-zeolite improves NO conversion relative to reference samples 15 and 17. x conversion rate and significantly reduced N 2 O is formed.

[0188] Example 7: 1Pt-8SiO 2 / TiO 2 Preparation and evaluation of +xFeY catalysts

[0189] Table 7 lists reference sample 1 and catalysts in which zeolite Y of sample 5 was replaced by xFeY (Si / Al=15:1). Reference sample 1 was prepared as described in Example 1. Samples 21 to 24 were prepared in the same manner as sample 5 in Example 1, except that zeolite HY was replaced by xFeY with various Fe 2 O 3 The loading of xFeY (Si / Al=15:1) was substituted (x=0.25 wt%, 0.5 wt%, 1 wt% and 3 wt% respectively relative to the weight of zeolite). All samples were hydrothermally aged at 650°C with 10% steam in air for 50 hours.

[0190] Table 7

[0191] Sample No. Sample name PGM / Oxide Zeolite Mixing ratio 1 <![CDATA[1Pt-8 SiO 2 / TiO 2 (Reference)]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> N / A NA 21 <![CDATA[1Pt-8 SiO 2 / Ten 2 +0.25FeY]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> <![CDATA[Fe-Y(0.25%Fe 2 THE 3 )]]> 1:1 22 <![CDATA[1Pt-8 SiO 2 / TiO 2 +0.5FeY]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> <![CDATA[Fe-Y(0.5%Fe 2 THE 3 )]]> 1:1 23 <![CDATA[1Pt-8 SiO 2 / Ten 2 +1FeY]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> <![CDATA[Fe-Y(1%Fe 2 THE 3 )]]> 1:1 24 <![CDATA[1Pt-8 SiO 2 / TiO 2 +3FeY]]> <![CDATA[1% Pt-8%SiO 2 / TiO 2 ]]> <![CDATA[Fe-Y(3%Fe 2 THE 3 )]]> 1:1

[0192] like Fig. 7A and Figure 7B As shown, they compare the NO x Conversion rate and N 2O formation rate, compared with reference sample 1, the addition of FeY increased the NO x conversion rate and reduced N 2 O is formed. The best performance is observed with Sample 22.

[0193] Example 8: 1Pt / Al 2 O 3 + Preparation and evaluation of zeolite catalysts

[0194] Table 8 lists a series of 1Pt / Al 2 O 3 The colloidal Pt nanoparticle solution was impregnated into Al 2 O 3 1Pt / Al 2 O 3 After impregnation, the resulting material was calcined in air at 550° C. for 2 hours. The Pt concentration on the support was 1 wt % relative to the weight of the support after calcination.

[0195] Samples 26 to 31 were prepared by mechanically mixing sample 25 with zeolite components in a 1:1 weight ratio. The zeolites in samples 26 to 31 were β (Si / Al=12.5:1), ferrierite (Si / Al=10:1), chabazite (Si / Al=14.5:1), Y (Si / Al=15:1), ZSM-5 (Si / Al=15:1), and mordenite (Si / Al=10:1) in H form, respectively. All samples (including the reference sample) were hydrothermally aged at 650°C with 10% steam in air for 50 hours.

[0196] Table 8

[0197] Sample No. Sample name PGM / Oxide Zeolite Mixing ratio 25 <![CDATA[1Pt / Al 2 O 3 (Reference)]]> <![CDATA[1%Pt / Al 2 THE 3 ]]> N / A NA 26 <![CDATA[1Pt / Al 2 A 3 +BEA]]> <![CDATA[1%Pt / Al 2 THE 3 ]]> H-β 1:1 27 <![CDATA[1Pt / Al 2 EITHER 3 +FER]]> <![CDATA[1%Pt / Al 2 THE 3 ]]> H-Ferrierite 1:1 28 <![CDATA[1Pt / Al 2 Oh 3 +NO]]> <![CDATA[1%Pt / Al 2 THE 3 ]]> H-chabazite 1:1 29 <![CDATA[1Pt / Al 2 EITHER 3 +Y]]> <![CDATA[1%Pt / Al 2 THE 3 ]]> HY 1:1 30 <![CDATA[1Pt / Al 2 About 3 +ZSM5]]> <![CDATA[1%Pt / Al 2 THE 3 ]]> H-ZSM-5 1:1 31 <![CDATA[1Pt / Al 2 O 3 +MOTHER]]> <![CDATA[1%Pt / TiO 2 ]]> H-Mordenite 1:1

[0198] like Fig. 8A and Figure 8B As shown, they compare the NO x Conversion rate and N 2 O formation rate, all zeolite-containing catalysts (samples 26-31) showed higher NO formation rates than the reference sample (sample 25) over the entire temperature range. x Samples 27 and 29 showed the highest NO conversion x Samples 26, 30, and 31 showed the lowest N 2 O is formed.

[0199] Example 9: WO as Pt Support 3 / ZrO 2 Catalyst preparation and evaluation

[0200] Table 9 lists the use of WO 3 / ZrO 2 Catalyst prepared as support. Sample 32 is a reference sample. 5% WO 3 / ZrO 2 The mixed oxide support was prepared by 4 ) 6 W 12 O 39 Solution immersed in Zr(OH) 4 , followed by calcination at 550 °C for 2 h in air, which yielded 5% WO 3 / ZrO2. Then, the colloidal Pt nanoparticles and colloidal SiO 2 The mixed solution of nanoparticles (acidic oxide modifier) ​​was added to WO 3 / ZrO 2 The obtained material was calcined in air at 550°C for 2 hours. After calcination, the sample contained 1% Pt and 8% SiO by weight relative to the weight of the support. 2 It was further aged at 650°C in 10% steam / air for 50 hours.

[0201] By using the aged 1Pt-8Si / 5WO 3 / ZrO 2 The powders were mechanically mixed with fresh H-β (Si / Al=12.5:1) powder at oxide to zeolite ratios of 2:1, 1:1 and 1:2, respectively, to prepare samples 33 to 35.

[0202] All samples in Table 9 contain the same amount of Pt.

[0203] Table 9

[0204]

[0205] like Fig. 9A and Fig. 9B As shown, they compare the NO x Conversion rate and N 2 O formation rate, all zeolite-containing samples (samples 33-35) show higher NO x The conversion rate is independent of the mixing ratio. 2 O formation is mixed, depending on the temperature range and the oxide / zeolite mixing ratio.

[0206] Example 10: 1Pt / SiO 2 +Y catalyst preparation and evaluation

[0207] Table 10 lists the SiO 2 The colloidal Pt nanoparticle solution was impregnated on SiO 2Reference sample 36 was prepared by mechanically mixing reference sample 36 with zeolite HY in a 1:1 weight ratio. Both samples were hydrothermally aged at 650°C with 10% steam in air for 50 hours.

[0208] Table 10

[0209] Sample No. Sample name PGM / Oxide Zeolite Mixing ratio 36 <![CDATA[1Pt / SiO 2 (Reference) <![CDATA[1Pt / SiO 2 ]]> N / A NA 37 <![CDATA[1Pt / SiO 2 +Y]]> <![CDATA[1Pt / SiO 2 ]]> HY 1:1

[0210] like Fig. 10A and Fig. 10B As shown, they compare the NO x Conversion rate and N 2 O formation rate, sample 37 shows similar NO to reference sample 36 x However, N 2 O formation is low.

[0211] Prior art documents cited:

[0212] -EP 3 409 359 A2

[0213] -WO 2018 / 073750 A1

[0214] -US 2021 / 102486 A1

[0215] -EP 2 313 196 A2

Claims

1. A method for effectively reducing nitrogen oxides (NO) from engine exhaust in the presence of a hydrogen reducing agent x ) of a hydrogen selective catalytic reduction (H2-SCR) catalyst composition, the H2-SCR catalyst composition comprising: (i) a first component comprising a metal component of a platinum group metal (PGM) supported by an oxide support; and (ii) a second component, the second component comprising a zeolite. 2 . The H 2 -SCR catalyst composition according to claim 1 , wherein the first component further comprises a second PGM component supported on the oxide support. 3 . The H 2 -SCR catalyst composition according to claim 1 , further comprising a third component comprising a second PGM supported on a second oxide support.

4. The H2-SCR catalyst composition of claim 1, wherein the oxide support is a mixed oxide support.

5. The H2-SCR catalyst composition according to claim 4, wherein the mixed oxide in the mixed oxide support is selected from the group consisting of TiO2 / ZrO2, CeO2 / MgO, WO3 / ZrO2, WO3 / Al2O3, WO3 / TiO2, WO3 / SiO2, Al2O3 / La2O3, TiO2 / Al2O3, V2O5 / TiO2-Al2O3, Nb2O5 / SiO2, ZnO / Al2O3, SiO2 / TiO2, SiO2 / Al2O3, Mn / TiO2 / Al2O3 and perovskite.

6. The H2-SCR catalyst composition according to claim 4 or 5, wherein the mixed oxide is selected from TiO2 / ZrO2, WO3 / Al2O3, WO3 / TiO2, WO3 / SiO2, WO3 / ZrO2, SiO2 / TiO2, and SiO2 / Al2O3. 7 . The H 2 -SCR catalyst composition of claim 1 , further comprising an acidic oxide modifier on the oxide support.

8. The H2-SCR catalyst composition of claim 1, wherein the zeolite is an acidic zeolite.

9. The H2-SCR catalyst composition of claim 1, wherein the zeolite is a metal-promoted zeolite.

10. The H2-SCR catalyst composition of claim 1, wherein the zeolite comprises more than one structure type. 11 . The H 2 -SCR catalyst composition according to claim 1 , wherein the first component and the second component are added in a mass ratio ranging from 95:5 to 10:

90.

12. The H2-SCR catalyst composition of claim 1, wherein the first component and the second component are combined into a composite material by: (1) physically mixing the first component and the second component; (2) dispersing the first component and the second component in water to form a slurry; (3) co-grinding the first component and the second component; or (4) a combination thereof.

13. A method for effectively catalyzing the reduction of nitrogen oxides (NO x ) is a selective catalytic reduction (SCR) product for reducing H2-SCR, the SCR product comprising a substrate on which the H2-SCR catalyst composition according to claim 1 is disposed.

14. A method for selectively reducing NO from an exhaust gas stream x An emission treatment system for a compound, the system comprising the SCR article according to claim 13.

15. A method for treating NO x A method for treating an exhaust gas stream containing a plurality of compounds, the method comprising passing the exhaust gas stream through the emissions treatment system of claim 14.

Citation Information

Patent Citations

  • Catalysts for NOX reduction employing h2 and a method of reducing NOX

    EP2313196A2

  • 4-way hybrid binary catalysts, methods and uses thereof

    EP3409359A2

  • Wireless Communication Techniques

    US20120178380A1

  • Hydrogen-assisted integrated emission control system

    US20210102486A1

  • Mixed metal large crystal molecular sieve catalyst compositions, catalytic articles, systems and method