A method for extracting selenium from lead-copper-zinc heavy metal smelting acid sludge
By combining wet low-temperature sulfidation slurry preparation and vacuum distillation with adsorbents, high-purity selenium is efficiently extracted from acid sludge in lead, copper, and zinc heavy metal smelting. This method solves the problems of complex processes, high energy consumption, and high costs in existing technologies, and achieves efficient and environmentally friendly selenium recovery.
Patent Information
- Application Number
- CN202411209514.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Existing technologies for extracting selenium from lead, copper, and zinc heavy metal smelting sludge have problems such as complex processes, high energy consumption, generation of hazardous waste, and high costs. In particular, the extraction effect is not good for raw materials with low selenium content.
A wet, low-temperature sulfidation slurry preparation method combined with an adsorbent was adopted. The sulfiding agent was mixed with lead, copper, and zinc heavy metal smelting acid sludge at low temperature, and then distilled under vacuum. The adsorbent was used to adsorb impurities to form non-volatile salts, and high-purity selenium was separated.
It has achieved the extraction of high-purity selenium from lead, copper, and zinc heavy metal smelting sludge with low selenium content, with a selenium purity of over 99.5% and a direct selenium recovery rate of 87.62%, effectively reducing impurity content and production costs.
Abstract
Description
Technical Field
[0001] This invention relates to a method for extracting selenium from acid mud used in the smelting of heavy metals such as lead, copper, and zinc, belonging to the field of rare and dispersed metal extraction technology. Background Technology
[0002] Selenium is a rare and dispersed metallic element of strategic importance, widely used in electronics, chemicals, pharmaceuticals, and healthcare. Industrially, selenium is typically recovered from selenium-containing slags such as copper electrolysis anode mud, acid sludge from sulfuric acid plants, and fumes from lead and zinc smelting. However, existing selenium extraction technologies suffer from disadvantages such as complex processes, the generation of hazardous waste, and high energy consumption, which hinder the extraction, purification, and large-scale application of selenium. Therefore, finding a green and efficient way to extract selenium from recovered selenium-containing acid sludge is of great significance for improving the utilization rate of selenium resources and reducing production costs.
[0003] The occurrence of various elements in the acid sludge from lead, copper, and zinc heavy metal smelting is very complex. It usually contains compounds or elements such as lead sulfate, lead sulfite, lead sulfide, lead selenide, mercury selenide, elemental selenium, elemental mercury, tellurium dioxide, and elemental tellurium. The target element selenium usually exists in the form of selenium compounds. It is difficult to achieve good recovery results by simply distilling and volatilizing. Moreover, different elements or the same element exist in different forms and have different or similar physicochemical properties, which makes it difficult for us to recover valuable elements in acid sludge.
[0004] Chinese patent CN115449637A discloses a method for efficient stepwise separation and extraction of selenium, copper, and tellurium from copper anode mud. The method processes copper anode mud or materials containing copper telluride as raw materials, with the following mass percentages of elements: Cu (5%–40%), Te (0.5%–10%), Se (0.5%–10%), Pb (1%–10%), and Ag (2%–15%). The raw material is then calcined at 600℃ for 3 hours using O2-SO2 to separate selenium, yielding calcined sand and selenium concentrate, with a selenium volatilization rate of 98.46%. This method is a pyrometallurgical extraction of selenium, which is energy-intensive and involves the harmful gas SO2.
[0005] Chinese patent CN116875800A discloses a method for leaching and separating lead, selenium, copper, and mercury from acid sludge. The raw material processed by this method is acid sludge produced during the copper smelting acid production process. Its main components are: Pb (30.61%), Cu (12.58%), Se (15.72%), Hg (4.32%), Zn (1.17%), Sb (0.1%), Bi (1.93%), As (0.93%), Te (0.16%), and Ag (0.11%). The process involves "sulfuric acid + sodium chlorate oxidation synergistic leaching - hydrochloric acid + sodium sulfite reduction precipitation of selenium". Since sulfuric acid and sodium chlorate are strong oxidizing agents, there are problems of equipment corrosion and high reagent costs.
[0006] Chinese patent CN113716532A discloses a method for removing mercury impurities from crude selenium. The raw material used in this method is crude selenium with a selenium content of 90%–97% (Se), 3200 ppm (Hg), and 2%–2.5% (Pb). The method involves adding a sulfiding agent to crude selenium slag crushed to below 200 mesh, mixing and pressing it into a briquette. This briquette is then placed in a sealed furnace and heated for sulfidation under an inert atmosphere. The sulfidated selenium slag is then vacuum distilled, allowing selenium to enter the gas phase and be collected as volatiles. Mercury sulfides and other valuable elements are enriched in the residue. The resulting selenium is then subjected to a second distillation for further mercury removal. This method achieves a selenium recovery rate greater than 98% and a mercury removal rate greater than 99.8%. This is a full-fire selenium extraction method, which is effective for purifying crude selenium but less effective for extracting selenium from raw materials with low selenium content. A single distillation can increase the selenium content from 10.22% to 76.21%. Summary of the Invention
[0007] To extract selenium from lead, copper, and zinc heavy metal smelting sludge with low selenium content, this invention provides a method for extracting selenium from lead, copper, and zinc heavy metal smelting sludge, the specific steps of which are as follows:
[0008] (1) Wet low-temperature sulfidation slurry preparation: Sulfidating agent and adsorbent are added to the acid mud for smelting lead, copper and zinc heavy metals containing water, mixed evenly, and then heated to obtain sulfidation products.
[0009] (2) The sulfide product obtained in step (1) is dried and then vacuum distilled. The condensate on the condenser plate after distillation is the high-purity selenium product.
[0010] Preferably, the lead, copper, and zinc heavy metal smelting acid sludge contains 10%–20% Se, 2%–5% Hg, 30%–40% Pb, and the remainder is other components.
[0011] Preferably, in step (1), the mass ratio of lead, copper, and zinc heavy metal smelting acid mud to sulfiding agent is (5-20):1.
[0012] Preferably, the sulfiding agent in step (1) is elemental sulfur, ferrous disulfide, or sodium sulfide.
[0013] Preferably, in step (1), the mass ratio of lead, copper, and zinc heavy metal smelting acid sludge to adsorbent is (8-15):1.
[0014] Preferably, the adsorbent in step (1) is sodium carbonate or silicon dioxide.
[0015] Preferably, the heating temperature in step (1) is 20-60°C and the heating time is 30-60 min.
[0016] Preferably, the drying temperature in step (2) is 50-80°C and the drying time is 12-24 hours.
[0017] Preferably, the temperature of vacuum distillation in step (2) is 240-350°C, the holding time is 1-2 hours, and the pressure is below 10 Pa.
[0018] Beneficial effects of the present invention
[0019] (1) Add an adsorbent to the raw material to adsorb some of the lead sulfide and mercury sulfide impurities that decompose during the distillation process, so as to avoid the volatilization of impurities affecting the selenium extraction efficiency and the selenium purity of the product.
[0020] (2) Using the method described in this invention, selenium can be extracted from lead, copper and zinc heavy metal smelting acid sludge containing 10.22% selenium and the selenium purity can reach more than 99.5%, with a direct selenium recovery rate of 87.62%. The mercury and lead content in the crude selenium product is reduced from 2.83% and 36.0% in the raw material to 0.139% and 0.111%, respectively, with removal rates of 98.5% and 99.96%.
[0021] (3) The present invention uses wet sulfidation reaction in the sulfidation stage for more complete reaction. In the distillation process, an adsorbent is used to react with residual heavy metal ions such as lead and mercury to form mercury salt and lead salt to further remove heavy metals such as lead and mercury, so that selenium in acid mud is separated out.
[0022] (4) This method is simple, efficient and environmentally friendly. It can be widely used to recover and utilize selenium in acid mud from lead, copper and zinc heavy metal smelting, improve the utilization rate of selenium resources, reduce production costs, and has broad market prospects and application value. Detailed Implementation
[0023] The technical solution of the present invention will be further illustrated below through specific embodiments. However, the following embodiments are merely simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention is determined by the claims.
[0024] The lead, copper, and zinc heavy metal smelting sludge used in all embodiments contained 10.22% Se, 2.83% Hg, and 36.0% Pb by mass, with the remainder being other components.
[0025] Example 1
[0026] A method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting processes includes the following steps:
[0027] (1) Wet low-temperature sulfidation slurry preparation: Take 24.30 g of water-containing lead, copper and zinc heavy metal smelting acid mud, add 2.43 g of sulfur and 3.07 g of adsorbent sodium carbonate according to the mass ratio of lead, copper and zinc heavy metal smelting acid mud raw material to sulfidating agent of 10:1, then mix the slurry evenly, and put the beaker containing the slurry into a 50℃ water bath and heat for 40 min.
[0028] (2) After sulfidation, pour the slurry in the beaker into the drying tray, put the drying tray into the 80℃ drying oven for 12 hours, take out the drying tray after drying, take out the agglomerated material and make it into a block that can be put into the crucible, put the material into the crucible, and then put the crucible containing the material into the vacuum furnace for distillation. Heat the temperature to 300℃ at a heating rate of 10℃ / min, then evacuate to below 10Pa for vacuum distillation, keep it at the temperature for 1 hour, and end the distillation. After the furnace cools down, open the furnace cover to collect the volatiles and residues and weigh and record them. The condensate on the condensing tray is the target crude selenium product. The residue in the crucible can be used as a raw material for rare and precious metal refining.
[0029] The purity of the crude selenium obtained was 99.62%, the direct recovery rate of Se was 93.86%, the removal rate of Hg was over 99%, and the removal rate of Pb was over 99.9%, as determined by ICP-AES and chemical titration.
[0030] Example 2
[0031] A method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting processes includes the following steps:
[0032] (1) Wet low-temperature sulfidation slurry preparation: Take 24.30 g of water-containing lead, copper and zinc heavy metal smelting acid mud, add 4.86 g of ferrous disulfide and 3.50 g of adsorbent silicon dioxide according to the mass ratio of acid mud raw material to sulfiding agent of 5:1, then mix the slurry evenly, and put the beaker containing the slurry into a 50℃ water bath for heating for 40 min.
[0033] (2) After sulfidation, pour the slurry in the beaker into the drying tray, put the drying tray into the 80℃ drying oven for 12 hours, take out the drying tray after drying, take out the agglomerated material and make it into a block that can be put into the crucible, put the material into the crucible, and then put the crucible containing the material into the vacuum furnace for distillation. Heat the temperature to 300℃ at a heating rate of 10℃ / min, then evacuate to below 10Pa for vacuum distillation, keep it at the temperature for 1 hour, and end the distillation. After the furnace cools down, open the furnace cover to collect the volatiles and residues and weigh and record them. The condensate on the condensing tray is the target crude selenium product. The residue in the crucible can be used as a raw material for rare and precious metal refining.
[0034] The purity of the crude selenium obtained was determined by ICP-AES and chemical titration to be over 99.5%, the direct recovery rate of Se was 98.52%, the removal rate of Hg was over 99.5%, and the removal rate of Pb was 99.96%.
[0035] Example 3
[0036] A method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting processes includes the following steps:
[0037] (1) Wet low-temperature sulfidation slurry preparation: Take 24.30 g of water-containing lead, copper and zinc heavy metal smelting acid mud, add sodium sulfide (i.e., 1.62 g of potassium sulfide) according to the mass ratio of acid mud raw material to sulfiding agent of 15:1, add 3.50 g of adsorbent sodium carbonate, then mix the slurry evenly, and put the beaker containing the slurry into a 50℃ water bath for heating for 40 min.
[0038] (2) After sulfidation, pour the slurry from the beaker into a drying tray. Place the drying tray in an 80℃ drying oven for 12 hours. After drying, remove the drying tray and remove the agglomerated material to form blocks that can be placed in a crucible. Place the material into the crucible and then place the crucible containing the material into a vacuum furnace for distillation. Heat the material to 300℃ at a rate of 10℃ / min, then evacuate to below 10Pa for vacuum distillation. Hold the temperature for 1 hour to finish distillation. After the furnace cools down, open the furnace lid to collect the volatiles and residues and weigh and record them. The condensate on the condenser is the target crude selenium product. The residue in the crucible can be used as a raw material for rare and precious metal refining.
[0039] The purity of the crude selenium obtained was determined by ICP-AES and chemical titration to be over 99%, with a direct selenium recovery rate of 87.62%, a Hg removal rate of over 99%, and a Pb removal rate of 99.8%.
[0040] Comparative Example 1
[0041] A method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting processes includes the following steps:
[0042] (1) Take 24.30 grams of water-containing lead, copper and zinc heavy metal smelting acid mud, place it on a drying tray, and put the drying tray into an 80℃ drying oven for 12 hours.
[0043] (2) After drying, remove the drying tray, take out the clumped material and crush it to below 200 mesh. Add 1.62 grams of sulfur to the raw material as a sulfurizing agent according to the mass ratio of raw material to sulfurizing agent of 15:1. Mix evenly and press into blocks to obtain a mixture. Put the material into a crucible and record the total weight of the crucible and the material.
[0044] (3) The crucible is placed in a vacuum furnace and heated to 150°C at a rate of 10°C / min under an inert gas atmosphere for 60 min to obtain the sulfidation product. The sulfidation product is directly subjected to vacuum distillation. After the sulfidation is completed, the furnace temperature is cooled to room temperature, and then heated to 300°C at a rate of 10°C / min. The temperature is then evacuated to below 10 Pa for vacuum distillation, and the temperature is maintained for 1 h to end the distillation. After the furnace has cooled down, the furnace lid is opened to collect the volatiles and residues and the weight is recorded. The condensate on the condenser plate is the target crude selenium product. The residue in the crucible can be used as a raw material for the refining of rare and precious metals.
[0045] The purity of the crude selenium obtained was 76.21%, the direct recovery rate of Se was 84.35%, the removal rate of Hg was 86.91%, and the removal rate of Pb reached 99.97%, as determined by ICP-AES and chemical titration.
[0046] The comparison shows that the method described in this application is more effective in extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting. The wet sulfidation process in the sulfidation stage allows for more thorough contact between impurity elements and the sulfiding agent, resulting in a more complete reaction. Adding an adsorbent to the material allows for adsorption reactions with heavy metal ions such as lead and mercury, forming corresponding, less volatile salts, reducing the volatilization of lead and mercury, and thus lowering the content of volatilized impurities. Therefore, this method achieves better extraction results.
[0047] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, not all embodiments. Other embodiments can be obtained based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting, characterized in that: Specifically, the following steps are included: (1) Wet low-temperature sulfidation slurry preparation: Sulfidating agent and adsorbent are added to the acid sludge containing water-containing lead, copper and zinc heavy metal smelting, mixed evenly, and then heated to obtain sulfidation products; the mass fraction of Se in the acid sludge containing lead, copper and zinc heavy metal smelting is 10% to 20%; the adsorbent is sodium carbonate or silicon dioxide; the heating temperature is 20 to 60°C, and the heating time is 30 to 60 min; (2) The sulfide product obtained in step (1) is dried and then vacuum distilled. The condensate on the condenser after distillation is the high-purity selenium product.
2. The method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting according to claim 1, characterized in that: The lead, copper, and zinc heavy metal smelting acid sludge described in step (1) has a Hg mass fraction of 2% to 5%, a Pb mass fraction of 30% to 40%, and the remainder consists of other components.
3. The method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting according to claim 1, characterized in that: In step (1), the mass ratio of water-containing lead, copper, and zinc heavy metal smelting acid mud to sulfiding agent is (5-20):
1.
4. The method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting according to claim 1, characterized in that: The sulfiding agent mentioned in step (1) is sulfur, ferrous disulfide or potassium sulfide.
5. The method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting according to claim 1, characterized in that: In step (1), the mass ratio of water-containing lead, copper, and zinc heavy metal smelting acid sludge to adsorbent is (8-15):
1.
6. The method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting according to claim 1, characterized in that: The drying temperature in step (2) is 50-80℃ and the drying time is 12-24h.
7. The method for extracting selenium from acid sludge from lead, copper, and zinc heavy metal smelting according to claim 1, characterized in that: In step (2), the temperature of vacuum distillation is 240-350℃, the holding time is 1-2h, and the pressure is below 10Pa.
Citation Information
Patent Citations
Method for efficiently and stepwise separating and extracting selenium, copper and tellurium from copper anode slime
CN115449637A
Method for leaching and stepwise separating and extracting lead, selenium, copper and mercury from acid mud
CN116875800A
Method for producing low-impurity crude selenium from mercury-acid-sludge-containing oxygen pressure alkali leaching liquid
CN106542507A
Method for removing impurity mercury from crude selenium
CN113716532A