A polycrystalline silicon high-boiling impurity removing agent, a preparation method thereof and a removing method

By using recycled salt prepared from polysilicon production waste as a purification agent, combined with distillation, the problem of removing aluminum and titanium impurities from high-boiling polysilicon was solved, achieving efficient, low-cost, and recyclable purification.

CN119080007BActive Publication Date: 2026-11-24XINJIANG DAQO NEW ENERGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411196780.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2026-11-24
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Existing high-boiling-point impurity removal processes for polycrystalline silicon suffer from problems such as complex impurity removal agents, inability to simultaneously remove aluminum and titanium impurities, unsatisfactory impurity removal effect, complex process, high cost, inability to recycle impurity removal agents, and easy introduction of new impurities.

Method used

Waste generated during polysilicon production is used as recycled salt. Through hydrolysis, pressure filtration, silicon removal, and impurity removal, an impurity removal agent is prepared. This agent is then mixed with high-boiling polysilicon and distilled to remove aluminum and titanium impurities. The solid material after distillation can be recycled.

Benefits of technology

It achieves efficient removal of aluminum and titanium impurities, reduces the cost of impurity removal, does not introduce new impurities, and the impurity removal agent can be reused, making it economical and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080007B_ABST
    Figure CN119080007B_ABST
Patent Text Reader

Abstract

This invention relates to a decontaminant for high-boiling-point polycrystalline silicon and its preparation and decontamination methods. The preparation method of the decontaminant for high-boiling-point polycrystalline silicon includes the following steps: (1) hydrolyzing waste gas containing chlorosilanes, adjusting the pH of the hydrolysate to neutral to obtain neutral wastewater; (2) filtering the neutral wastewater under pressure, then sequentially performing silicon removal and decontamination treatments, evaporating and crystallizing, and drying to obtain recovered salt, i.e., the decontaminant. The decontaminant for high-boiling-point polycrystalline silicon and its preparation and decontamination methods of this invention utilize recovered salt obtained from waste gas treatment in polycrystalline silicon to remove impurities from high-boiling-point polycrystalline silicon. This method can simultaneously remove aluminum and titanium impurities, and has the advantages of high decontamination efficiency, low cost, and reusability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of impurity removal from high-boiling-point polycrystalline silicon, specifically relating to an impurity remover for high-boiling-point polycrystalline silicon, its preparation method, and the impurity removal method. Background Technology

[0002] Polysilicon is a fundamental raw material for the photovoltaic industry, and its production process generates some byproducts. A portion of these byproducts consists of high-boiling-point compounds (commonly known as "high-boiling substances") with boiling points exceeding 70°C, accounting for 7.0-8.0% of the crude monomer. These high-boiling-point compounds are highly complex, primarily including oxysilanes such as hexachloroethoxysilane and pentachloroethoxysilane, and polychlorosilanes such as hexachlorodisilane and pentachlorodisilane. The boiling points of these components are relatively close, making them difficult to separate using common methods, thus hindering their effective utilization. In actual production, the main method for handling high-boiling-point compounds is concentration and separation. After recovering some low-boiling-point compounds such as silicon tetrachloride, the remaining high-boiling-point compounds are hydrolyzed along with metal chlorides and other solid impurities carried over during polysilicon processing. While this method is simple and effective, it consumes a large amount of valuable Si and Cl elements, hindering the sustainable development of polysilicon production. Furthermore, improper handling of these high-boiling-point compounds can increase production costs and cause safety and environmental problems.

[0003] To address the aforementioned issues, methods have been developed that use organic amines as catalysts to catalyze the cracking of polychlorosilanes into monosilicon compounds. Specifically, tri-n-octylamine, N,N-diethylbutylamine, and other catalysts are used to crack high-boiling-point substances into chlorosilanes for recycling. However, these high-boiling-point substances contain metallic impurities, with aluminum trichloride and titanium tetrachloride being the most representative, reaching concentrations of hundreds to thousands of ppm by mass. These metallic impurities can complex with the organic amines in the catalyst, causing significant catalyst loss during the cracking process. To maintain catalytic efficiency, the lost catalyst needs to be continuously replenished, increasing operating costs and severely impacting the stability of the production process. Furthermore, these metallic impurities also enter the subsequent distillation system along with the cracked monosilicon compounds, increasing the pressure required for purification. Under normal pressure, titanium tetrachloride has a boiling point of 135-136℃, and aluminum trichloride has a boiling point of 182.7℃, but both sublimate at 177.8℃. These temperatures are very close to the boiling range of high-boiling substances (120-180°C), making it difficult to separate these two metal chlorides from other components in high-boiling substances using common methods such as distillation.

[0004] Current impurity removal processes for high-boiling-point polycrystalline silicon involve adding a decontaminant to the high-boiling-point material to form a non-volatile compound mixture with the metallic impurities. The remaining components in the high-boiling-point material are then separated from this mixture by distillation, thus removing aluminum chloride impurities. Alternatively, cooling and sedimentation crystallization allows aluminum trichloride to exist in a stable solid form, which is then removed by filtration. However, these methods suffer from several drawbacks, including complex decontaminant agents, inability to simultaneously remove impurities such as aluminum and titanium, unsatisfactory removal efficiency, complex processes, high costs, inability to recover the decontaminant, and the potential introduction of new impurities.

[0005] In view of this, the present invention proposes a new impurity remover for high-boiling polycrystalline silicon and its preparation and removal methods. The method uses recovered salt obtained from waste gas treatment in polycrystalline silicon to remove impurities from high-boiling polycrystalline silicon, which can remove aluminum and titanium impurities at the same time. It has the advantages of high impurity removal effect, low cost and reusability. Summary of the Invention

[0006] The purpose of this invention is to provide a simple method for preparing a depurifying agent for high-boiling polycrystalline silicon.

[0007] To achieve the above objectives, the technical solution adopted is as follows:

[0008] A method for preparing a depurifying agent for high-boiling polycrystalline silicon, characterized by comprising the following steps:

[0009] (1) After hydrolyzing the waste gas and waste liquid containing chlorosilane, the pH of the hydrolysis solution is adjusted to neutral to obtain neutral wastewater.

[0010] (2) After the neutral wastewater is filtered, it is subjected to silicon removal and impurity removal treatment in sequence, evaporated and crystallized, and then dried to obtain the recovered salt, which is the impurity removal agent.

[0011] Furthermore, in step (1), sodium hydroxide solution is used to adjust the hydrolysis solution to neutral.

[0012] Furthermore, in step (2), the silicon removal process involves adding calcium hydroxide.

[0013] Furthermore, in step (2), the impurity removal process involves adding carbonate ions to remove Mg. 2+ Ca 2+ Ba 2+ 、Sr 2+ .

[0014] Another objective of this invention is to provide a decontaminant for high-boiling-point polycrystalline silicon, prepared using the above-described method. This decontaminant uses solid waste generated during polycrystalline silicon production as a treatment agent, resulting in low cost.

[0015] Another objective of this invention is to provide a method for removing impurities from high-boiling polycrystalline silicon. This method can simultaneously remove aluminum and titanium impurities, and has the advantages of significant impurity removal effect, low cost, and no introduction of new impurities.

[0016] To achieve the above objectives, the technical solution adopted is as follows:

[0017] A method for removing impurities from high-boiling polycrystalline silicon, characterized in that the method comprises: mixing an impurity remover with the high-boiling polycrystalline silicon and then performing distillation to obtain the impurity-removed high-boiling polycrystalline silicon;

[0018] The impurity removal agent is the one described above.

[0019] Furthermore, the mass ratio of the impurity remover to the high-boiling polycrystalline silicon is 0.8-1.8:100.

[0020] Furthermore, the mass ratio of the impurity remover to the high-boiling polycrystalline silicon is 0.8-1.05:100.

[0021] Furthermore, the distillation process is carried out at a temperature greater than 150°C.

[0022] Furthermore, the pressure of the distillation process is 20-100 kPa.

[0023] Furthermore, after the distillation process, the solution that was not distilled off is subjected to hydrolysis, neutralization, pressure filtration, silicon removal, impurity removal, evaporation crystallization, and drying. The resulting solid substance can be used as an impurity remover for further impurity removal of polycrystalline silicon high-boiling-point substances.

[0024] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0025] 1. In the technical solution of the present invention, solid waste (recycled salt) generated in polysilicon production is used as a purification agent, which requires no additional cost, turns waste into treasure, creates benefits, and is economical and environmentally friendly.

[0026] 2. In the technical solution of the present invention, recycled salt is used as a decontamination agent, which can not only efficiently remove aluminum from high boiling points, but also has a certain effect on removing titanium.

[0027] 3. In the technical solution of the present invention, the solid waste generated in the production of polycrystalline silicon mainly consists of various inorganic salts and trace amounts of organic matter in the original system. It will not introduce new impurities into the system. Moreover, these trace amounts of organic matter are recycled in the system as impurity removal agents along with this solid waste, which will not cause subsequent environmental problems. At the same time, the impurity removal cost is low.

[0028] 4. In the technical solution of the present invention, after the impurity removal agent complexes with impurities such as aluminum and titanium, it can be recycled and reused as an impurity removal agent after post-treatment such as hydrolysis, thereby further reducing the cost of impurity removal. Attached Figure Description

[0029] Figure 1 This is a flowchart of Example 1. Detailed Implementation

[0030] To further illustrate the present invention's impurity remover for high-boiling polycrystalline silicon, its preparation method, and the impurity removal method, and to achieve the intended objectives of the invention, the following, in conjunction with preferred embodiments, details the specific implementation methods, structures, features, and effects of the impurity remover for high-boiling polycrystalline silicon proposed by the present invention. In the following description, different "embodiments" or "embodiments" do not necessarily refer to the same embodiment. Furthermore, specific features, structures, or characteristics in one or more embodiments can be combined in any suitable manner.

[0031] Before detailing the impurity removal agent for high-boiling polycrystalline silicon and its preparation and removal methods according to the present invention, it is necessary to further explain the relevant background mentioned in the present invention in order to achieve better results.

[0032] Current technologies offer methods for separating metallic impurities and preventing their depletion of catalysts. For example:

[0033] Patent CN108658082A discloses a method for removing aluminum chloride by pretreating high-boiling-point substances. This method involves sending the high-boiling-point substances to a cooling and stirring tank, stirring them at a low temperature for 1-5 hours, then sending them to a settling tank, and finally allowing the high-boiling-point substances to settle in a nitrogen atmosphere for 1-20 hours, thereby separating a slurry containing solid impurities and metal halides. However, this method has a long processing time and the effect of removing aluminum chloride is not ideal.

[0034] Patent CN113149017A discloses a complexing agent for removing aluminum from high-boiling polycrystalline silicon and its application. The complexing agent has a complex structure and is difficult to apply on a large scale in actual production.

[0035] Patent CN105271246A discloses a method for removing aluminum chloride from high-boiling substances. This method first adds an auxiliary agent to the high-boiling substances to form a mixed system containing non-volatile aluminum compounds with aluminum impurities. Then, the remaining components in the high-boiling substances are separated from the mixed system by distillation, thereby removing aluminum chloride impurities. However, the auxiliary agent used in this method is prepared by mixing "deferoxamine", "deferoxone" and "ferricidine" in a certain proportion. It has a high iron removal effect, but the aluminum removal effect is not ideal, and the cost is also high.

[0036] Patent CN116216724A discloses a compound alkali metal chloride and aminocarboxylate as a reagent for removing aluminum and titanium impurities from high-boiling polycrystalline silicon. This impurity remover can raise the boiling point or sublimation temperature of metal impurities in high-boiling polycrystalline silicon, which helps to separate high-boiling polycrystalline silicon from metal impurities during distillation and reduces the loss of organic amine catalysts by metal impurities during catalytic cracking. However, the impurity remover cannot be recovered.

[0037] Patent CN117342563A discloses a method for removing aluminum from high-boiling polycrystalline silicon. The method involves the cations in a pyrrolidine-based or piperidine-based ionic liquid combining with aluminum trichloride in the high-boiling polycrystalline silicon to form a chloroaluminate ionic liquid. This chloroaluminate ionic liquid can further be used as a catalyst for the catalytic cracking reaction of the high-boiling polycrystalline silicon. However, the impurity removal agent cannot be recovered, and the cost is high.

[0038] CN104402004A discloses an extraction method for treating chlorosilane slurry, which involves mixing a certain alkane as an extractant with a high-boiling polycrystalline silicon material, followed by drying in a dryer, evaporation in an evaporator, and then dry distillation in a distillation tower to separate aluminum trichloride.

[0039] CN115893424A discloses a treatment agent for removing aluminum from high-boiling polycrystalline silicon and its application. The treatment agent is obtained by compounding alkali metal chloride, alkaline earth metal chloride, transition metal element chloride and alkaline earth metal sulfate. The metal salt in the treatment agent is mixed with high-boiling polycrystalline silicon to form a multi-element molten salt system, which is then separated by distillation.

[0040] Therefore, existing impurity removal technologies have the following problems:

[0041] (1) Existing aluminum treatment agents include organic and inorganic types. Organic types include pyrrolidine ionic liquids, piperidine ionic liquids, or C12-C16 alkanes, which are expensive and add additional treatment agent recovery processes and costs. If the recovery is incomplete, organic matter will be introduced into the water body during subsequent hydrolysis treatment, which is not easy to remove and does not meet the environmental protection requirements for external drainage. Inorganic types are obtained by compounding four salts: alkali metal chlorides, alkaline earth metal chlorides, transition metal element chlorides, and alkaline earth metal sulfates, which have complex compositions.

[0042] (2) Existing high-boiling-point aluminum treatment agents have a single function, only removing aluminum and not removing titanium.

[0043] (3) Existing complexing impurity removers cannot be recycled and reused.

[0044] Having understood the relevant background mentioned in this invention, the following will provide a more detailed description of a high-boiling-point impurity remover for polycrystalline silicon, its preparation method, and the impurity removal method, in conjunction with specific embodiments:

[0045] The technical solution of this invention is as follows:

[0046] A method for preparing a decontaminant for high-boiling polycrystalline silicon includes the following steps:

[0047] (1) After hydrolyzing the waste gas and waste liquid containing chlorosilane (reacting with water), the pH of the hydrolysis solution is adjusted to neutral to obtain neutral wastewater.

[0048] (2) After the neutral wastewater is filtered by pressure, it is subjected to silicon removal and impurity removal treatment in sequence, then evaporated and crystallized and dried to obtain the recovered salt, which is the impurity removal agent.

[0049] Preferably, in step (1), sodium hydroxide solution is used to adjust the hydrolysis solution to neutral.

[0050] Preferably, in step (2), the silicon removal process involves adding calcium hydroxide;

[0051] Preferably, in step (2), the impurity removal process is as follows: adding carbonate ions to remove Mg. 2+ Ca 2+ Ba 2+ 、Sr 2+ .

[0052] A method for removing impurities from high-boiling polycrystalline silicon involves mixing an impurity remover with the high-boiling polycrystalline silicon and then performing distillation to obtain the impurity-removed high-boiling polycrystalline silicon.

[0053] The impurity removal agent is the one described above.

[0054] In the above technical solution, the recovered salt can complex metallic impurities such as aluminum, titanium, iron, calcium, magnesium, copper, nickel, and zinc in high-boiling substances, transforming them into substances with even higher boiling points, which are then retained at the bottom of the purification vessel.

[0055] Preferably, the mass ratio of the impurity remover to the high-boiling polycrystalline silicon is 0.8-1.8:100.

[0056] More preferably, the mass ratio of the impurity remover to the high-boiling polycrystalline silicon is 0.8-1.05:100. Preferably, the distillation treatment temperature is greater than 150°C.

[0057] Preferably, the pressure of the distillation process is 20-100 kPa.

[0058] Preferably, after the distillation process, the solution that is not distilled off is subjected to hydrolysis, neutralization, pressure filtration, silicon removal, impurity removal, evaporation crystallization, and drying. The resulting solid substance, i.e., the recovered salt, can be used as an impurity removal agent for further impurity removal of polycrystalline silicon high-boiling-point substances.

[0059] In the above technical solution, the neutralization, pressure filtration, silicon removal, impurity removal, and evaporation crystallization treatments are the same as the preparation methods of the above-mentioned impurity removal agent.

[0060] Example 1.

[0061] The specific steps are as follows:

[0062] A. Preparation of recycled salt

[0063] (1) Polysilicon production generates some waste gas and waste liquid containing chlorosilanes. The waste liquid also contains some esters and aniline organic compounds, which cannot be discharged and need to be hydrolyzed. Chlorosilanes react with water to produce HCl, which needs to be neutralized with NaOH solution to form neutral wastewater.

[0064] (2) Neutral wastewater contains silica, silicon powder, etc., which enter the filter press system, forming a filter cake. After removing silica and silicon powder, the neutral wastewater undergoes silica removal and Mg removal. 2+ Ca 2+ Ba 2+ 、Sr 2+ After removing impurities, the salt is evaporated and crystallized to produce recovered salt. At this time, the moisture content of the recovered salt is about 10%, and it needs to be dried to a dew point of ≤-50℃ using a single cone dryer before use.

[0065] The silicon removal process involves adding calcium hydroxide to the neutral wastewater after removing silicon dioxide and silicon powder, stirring, and then allowing the Ca hydroxide to dissolve. 2+ The calcium silicate precipitate is formed by the reaction with silicate ions. It settles naturally in an inclined plate settler, is initially filtered by a quartz sand filter to remove large solid particles, and then PAC coagulant is added. The CaSiO3 precipitate is further removed by a first-stage self-cleaning filter, and then solid particles ≥0.02um are intercepted by a first-stage ultrafiltration membrane.

[0066] Except Mg 2+ Ca 2+ Ba 2+ 、Sr 2+ Impurities: Added sodium carbonate, carbonate ions react with Mg 2+ Ca 2+ Ba 2+ 、Sr 2+ Impurities form precipitates, thereby removing Mg. 2+ Ca 2+ Ba 2+ 、Sr 2+ Impurities.

[0067] The recovered salt after the above treatment mainly consists of inorganic sodium chloride, and also contains trace amounts of sodium silicate and other inorganic chloride salts. A small amount of calcium silicate, produced during the silicon removal process, remains. Calcium silicate can help prevent sodium chloride from caking in the impurity removal agent, so this trace amount can act as an anti-caking agent. It also contains trace amounts of aniline-based organic compounds and trace amounts of organic sodium salts formed by the hydrolysis of esters under alkaline conditions. This combination of organic and inorganic substances not only efficiently removes aluminum from high-boiling-point environments but also has a certain effect on titanium removal.

[0068] B. High-boiling-point impurity removal from polycrystalline silicon: combined with Figure 1

[0069] The recovered salt and high-boiling-point substances are mixed and heated for distillation in a purification vessel at a certain ratio. The distillation temperature is greater than 150℃ and the pressure is 20-100kPa. The purification vessel is stirred to ensure that the recovered salt and polycrystalline silicon high-boiling-point substances are fully mixed. The substances vaporized in the reaction vessel are condensed through a condenser and collected in a container connected to the condenser.

[0070] Preferably, the mass ratio of the impurity remover, i.e., the recovered salt, to the high-boiling polycrystalline silicon is 0.8-1.8:100.

[0071] The condensed liquid is a high-boiling-point substance that has had metallic impurities such as aluminum removed, and can enter the subsequent titanium removal system and pyrolysis conversion system.

[0072] The recovered salt can complex metallic impurities such as aluminum, titanium, iron, calcium, magnesium, copper, nickel, and zinc in high-boiling-point substances, transforming them into substances with even higher boiling points. These substances remain at the bottom of the purification vessel and can be hydrolyzed together with the unvaporized high-boiling-point substances. After pH adjustment, the hydrolysis products enter the filter press system. The neutral wastewater after filter press undergoes silica and magnesium removal processes. 2+ Ca 2+ Ba 2+ 、Sr 2+ After a series of processes including evaporation, crystallization, and drying (these processes are the same as those in step A), the recovered salt can be obtained again for recycling.

[0073] The definitions of aluminum removal rate and titanium removal rate in the embodiments are as follows:

[0074] Aluminum removal rate = (1 - Al content of condensed and collected distillate / Al content in high-boiling polycrystalline silicon to be treated) × 100%.

[0075] Titanium removal rate = (1 - Ti content of condensed and collected distillate / Ti content in high-boiling polycrystalline silicon to be treated) × 100%.

[0076] Example 2.

[0077] The operation steps of Example 2 are the same as those of Example 1, except that:

[0078] The high-boiling point to be treated (Al content of 480.576 ppm and Ti content of 403.018 ppm) and 0.8% by mass of the recovered salt (the recovered salt prepared in step A of Example 1) were added to the reactor, stirred and distilled at 155 °C and 100 kPa.

[0079] The vapor phase condensate was sampled, and the Al content was measured to be 56.977 ppm and the Ti content was 130.002 ppm. Calculations show that the aluminum removal rate in this embodiment is 88.14% and the titanium removal rate is 67.74%.

[0080] Example 3.

[0081] The operation steps of Example 3 are the same as those of Example 2, except that:

[0082] The high-boiling point to be treated (Al content of 480.576 ppm and Ti content of 403.018 ppm) and 0.9% of the recovered salt by mass were added to the reactor, stirred and distilled at 155 °C and 100 kPa.

[0083] The gas-phase condensate was sampled and the Al content was measured to be 32.563 ppm and the Ti content was 91.462 ppm. Calculations show that the aluminum removal rate in this embodiment is 93.22% and the titanium removal rate is 77.31%.

[0084] Example 4.

[0085] The operation steps of Example 4 are the same as those of Example 2, except that:

[0086] The high-boiling point to be treated (Al content of 480.576ppm and Ti content of 403.018ppm) and 1.0% of the recovered salt by mass were added to the reactor, stirred and distilled at 155℃ and 100kPa.

[0087] The gas-phase condensate was sampled and the Al content was measured to be 11.045 ppm and the Ti content was 62.323 ppm. Calculations show that the aluminum removal rate in this embodiment is 97.70% and the titanium removal rate is 84.54%.

[0088] Example 5

[0089] The operation steps of Example 5 are the same as those of Example 1, except that:

[0090] The high-boiling point to be treated (Al content of 480.576 ppm and Ti content of 403.018 ppm) and 1.05% of the recovered salt by mass were added to the reactor, stirred and distilled at 155 °C and 100 kPa.

[0091] The gas-phase condensate was sampled and the Al content was found to be 0 ppm, and the Ti content was 60.002 ppm. Calculations show that the aluminum removal rate in this embodiment is 100%, and the titanium removal rate is 85.11%.

[0092] Example 6.

[0093] The operation steps of Example 6 are the same as those of Example 2, except that:

[0094] The high-boiling point to be treated (Al content of 480.576 ppm and Ti content of 403.018 ppm) and 1.05% of the recovered salt by mass were added to the reactor, stirred and distilled at 158 ​​°C and 100 kPa.

[0095] The gas-phase condensate was sampled and the Al content was 0 ppm and the Ti content was 61.032 ppm. Calculations show that the aluminum removal rate in this embodiment is 100% and the titanium removal rate is 84.86%.

[0096] Example 7.

[0097] During stirred distillation, the recovered salt complexes with metallic impurities such as aluminum, titanium, iron, calcium, magnesium, copper, nickel, and zinc in the high-boiling-point substances in the purification vessel, transforming them into substances with even higher boiling points. These substances remain at the bottom of the purification vessel and are hydrolyzed together with the unvaporized high-boiling-point substances. After the pH of the hydrolysis products is adjusted to meet the requirements, they enter the pressure filtration system. The neutral wastewater after pressure filtration undergoes silicon and magnesium removal processes. 2+ Ca 2+ Ba 2+ 、Sr 2+ After a series of processes including evaporation, crystallization, and drying (these processes are the same as those in step A), the recovered salt is obtained again. This secondary recovered salt is then used again to remove impurities from high-boiling substances.

[0098] The high-boiling point to be treated (Al content of 480.576 ppm and Ti content of 403.018 ppm) and 1.05% by mass of secondary recovered salt were added to the reactor, stirred and distilled at 155℃ and 100 kPa.

[0099] The gas-phase condensate was sampled and the Al content was found to be 0 ppm, and the Ti content was 63.942 ppm. Calculations show that the aluminum removal rate in this embodiment is 100%, and the titanium removal rate is 84.13%.

[0100] Example 8.

[0101] The operation steps of Example 8 are the same as those of Example 2, except that:

[0102] The high-boiling point to be treated (Al content of 344.119 ppm and Ti content of 528.414 ppm) and 1.05% of the recovered salt by mass were added to the reactor, stirred and distilled at 155 °C and 100 kPa.

[0103] The gas-phase condensate was sampled and the Al content was found to be 0 ppm, and the Ti content was 52.3287 ppm. Calculations show that the aluminum removal rate in this embodiment is 100%, and the titanium removal rate is 90.10%.

[0104] Example 9.

[0105] The operation steps of Example 9 are the same as those of Example 2, except that:

[0106] (1) The high-boiling point to be treated (Al content of 228.825ppm and Ti content of 1193.067ppm) and 1.05% of the recovered salt by mass were added to the reactor, stirred and distilled at 155℃ and 100kPa.

[0107] The gas-phase condensate was sampled and the Al content was measured to be 2.212 ppm and the Ti content was 483.355 ppm. Calculations show that the aluminum removal rate in this embodiment is 99.03% and the titanium removal rate is 59.49%.

[0108] The high Ti content in the high-boiling point sample meant that the amount of impurity remover needed was insufficient to achieve the desired titanium removal effect.

[0109] (2) The high-boiling-point salt to be treated (Al content of 228.825ppm and Ti content of 1193.067ppm) was added to the reactor and stirred and distilled at 155℃ and 100kPa.

[0110] The mass ratios of recovered salt to high-boiling-point substances were 1.3:100, 1.5:100, and 1.8:100, respectively.

[0111] The impurity removal effect was measured by sampling the gas phase condensate. The aluminum removal rate and titanium removal rate both increased with the increase of the amount of recovered salt. When the mass ratio of recovered salt to high boiling point was 1.5:100, the aluminum removal rate was 100%. When the mass ratio of recovered salt to high boiling point was 1.8:100, the titanium removal rate was 88.25%.

[0112] Example 10.

[0113] The operation steps of Example 10 are the same as those of Example 2, except that:

[0114] The high-boiling point to be treated (Al content of 344.119 ppm and Ti content of 528.414 ppm) and 1.05% of the recovered salt by mass were added to the reactor, stirred and distilled at 155 °C and 20 kPa.

[0115] The gas-phase condensate was sampled and the Al content was 0 ppm and the Ti content was 48.254 ppm. Calculations show that the aluminum removal rate in this embodiment is 100% and the titanium removal rate is 90.87%.

[0116] Example 11.

[0117] The operation steps of Example 11 are the same as those of Example 2, except that:

[0118] The high-boiling point to be treated (Al content of 344.119 ppm and Ti content of 528.414 ppm) and 1.05% of the recovered salt by mass were added to the reactor, stirred and distilled at 155 °C and 80 kPa.

[0119] The gas-phase condensate was sampled and the Al content was found to be 0 ppm, and the Ti content was 50.148 ppm. Calculations show that the aluminum removal rate in this embodiment is 100%, and the titanium removal rate is 90.51%.

[0120] Comparative Example 1.

[0121] The high-boiling point to be treated (Al content of 480.576 ppm and Ti content of 403.018 ppm) and 1.05% of the recovered salt by mass were added to the reactor, stirred and distilled at 145 °C and 100 kPa.

[0122] The gas-phase condensate was sampled and the Al content was measured to be 59.937 ppm and the Ti content was 226.584 ppm. Calculations show that the aluminum removal rate in this embodiment is 87.53% and the titanium removal rate is 43.78%.

[0123] Comparing Comparative Example 1 with Example 2, it can be seen that the distillation temperature has a significant effect on the impurity removal effect.

[0124] Comparative Example 2.

[0125] According to patent CN115893424A, 960 parts NaCl, 2 parts KCl, 3 parts CaCl2, 1 part FeCl3 and 2 parts CaSO4 were added to a ball mill and ball-milled for 3 hours. Then the mixture was placed in a vibrating screen and sieved through a 120-mesh stainless steel screen to prepare the polycrystalline silicon high-boiling-point aluminum removal agent of this comparative example.

[0126] 50g of the high-boiling-point substance to be treated (Al content of 480.576ppm and Ti content of 403.018ppm) and 1g of the polycrystalline silicon high-boiling-point substance aluminum removal agent of this comparative example were added to the reactor, stirred and distilled at 155℃, and the operating pressure was controlled at 0.2MPa.

[0127] The gas-phase condensate was sampled and the Al content was measured to be 7.655 ppm and the Ti content was 392.569 ppm. Calculations showed that the aluminum removal rate of this comparative example was 98.41% and the titanium removal rate was 2.59%.

[0128] Comparing Comparative Example 2 with Examples 2-9 reveals that Comparative Example 2 does not exhibit titanium removal effectiveness (the 2.59% titanium removal rate here is primarily due to the titanium removal effect of the distillation process itself), and it requires a large amount of impurity removal agent. Therefore, compared to Comparative Example 2, the technical solution of this invention not only efficiently removes aluminum from high-boiling-point environments but also achieves a certain degree of titanium removal.

[0129] Comparative Example 3.

[0130] The operating steps of Comparative Example 3 are the same as those of Example 2, except that the impurity removal agent is sodium chloride.

[0131] The vapor phase condensate was sampled, and the Al content was measured to be 91.437 ppm and the Ti content to be 398.584 ppm. Calculations show that the aluminum removal rate in this embodiment is 80.97% and the titanium removal rate is 1.10%.

[0132] As can be seen from Comparative Example 3, the aluminum removal effect of a single chloride salt is poor, and it does not have the effect of removing titanium (here, the titanium removal rate of 1.10% is the titanium removal effect of the distillation process itself).

[0133] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention shall still fall within the scope of the technical solution of the present invention.

Claims

1. A method for removing impurities from high-boiling-point polycrystalline silicon, characterized in that, The impurity removal method is as follows: after mixing the impurity removal agent with the high-boiling polycrystalline silicon, the mixture is distilled at a temperature greater than 150°C to obtain the impurity-removed high-boiling polycrystalline silicon. The method for preparing the impurity remover includes the following steps: (1) After hydrolyzing the waste gas and waste liquid containing chlorosilane, the pH of the hydrolysate is adjusted to neutral by sodium hydroxide solution to obtain neutral wastewater; (2) After the neutral wastewater is filtered by pressure, it is subjected to silicon removal and impurity removal treatment in sequence, evaporated and crystallized, and then dried to obtain the recovered salt, which is the impurity removal agent. The silicon removal process involves adding calcium hydroxide. The impurity removal process involves adding carbonate ions to remove Mg. 2+ Ca 2+ Ba 2+ 、Sr 2+ .

2. The impurity removal method according to claim 1, characterized in that, The mass ratio of the impurity remover to the high-boiling polycrystalline silicon is 0.8-1.8:

100.

3. The impurity removal method according to claim 2, characterized in that, The mass ratio of the impurity remover to the high-boiling polycrystalline silicon is 0.8-1.05:

100.

4. The impurity removal method according to claim 1, characterized in that, The pressure of the distillation process is 20-100 kPa.

5. The impurity removal method according to claim 1, characterized in that, After the distillation process, the undistilled solution is subjected to hydrolysis, neutralization, pressure filtration, silicon removal, impurity removal, evaporation crystallization, and drying. The resulting solid substance can be used as an impurity remover for further impurity removal of polycrystalline silicon high-boiling-point materials.

Citation Information

Patent Citations

  • Preparation method for production of white carbon black by industrial sodium silicate parallel flow carbon decomposition

    CN104402004A

  • Method for preparing chlorinated disilane by utilization of polysilicon byproducts

    CN105271246A

  • High-boiling product cracking technology in polycrystalline silicon production

    CN108658082A

  • Complexing agent for removing aluminum from polycrystalline silicon high-boiling residues and application method of complexing agent

    CN113149017A

  • Treating agent for removing aluminum from polycrystalline silicon high-boiling residues and application of treating agent