A graphitized cathode and a preparation method thereof, an aluminum electrolysis cell, and an aluminum electrolysis method
By coating the graphitized cathode substrate with a TiB₂ composite layer and optimizing the structure of the low-temperature aluminum electrolysis cell, the problems of sodium and potassium infiltration damage and low conductivity in the low-temperature electrolysis cell were solved, and stable and efficient production of low-temperature aluminum electrolysis was achieved.
Patent Information
- Application Number
- CN202411239772.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-09-05
AI Technical Summary
In the prior art, when graphitized cathodes are used in low-temperature aluminum electrolysis cells, they are easily damaged by sodium and potassium penetration in the low-temperature electrolyte, leading to problems such as cathode expansion and cracking, layered pulverization and peeling. In addition, the low conductivity of the low-temperature electrolyte system leads to an increase in cell voltage, making it difficult to achieve low-voltage operation.
A TiB₂ composite layer with a carbon content of <20wt.% and a thickness of 5mm-50mm is used to cover the surface of a graphitized cathode substrate. Combined with a forced heat dissipation device and optimized low-temperature electrolyte composition and superheat, the electrolytic cell structure is improved to enhance its anti-permeation performance and electrolysis efficiency.
It effectively resists the sodium and potassium permeation and expansion of the low-temperature electrolyte, improves the hardness and wettability of the cathode, reduces the cell voltage, and achieves stable operation and efficient production of low-temperature aluminum electrolysis.
Smart Images

Figure CN119080533B_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present application relates to the technical field of aluminum smelting, and in particular to a graphitized cathode and a preparation method thereof, an aluminum electrolysis cell, and an aluminum electrolysis method. BACKGROUND
[0002] The graphitized cathode is a cathode carbon block made of petroleum coke, pitch coke and the like as main raw materials, through forming, baking, impregnation and high-temperature graphitization treatment above 2300 DEG C. In this process, carbon elements in the raw materials are rearranged at high temperature to form a crystal structure similar to graphite, thereby giving the carbon block excellent electrical conductivity, thermal conductivity and corrosion resistance. The graphitized cathode is mainly used as a cathode material for an aluminum electrolysis cell. In the aluminum electrolysis production process, it plays a key role in improving current efficiency, reducing energy consumption, prolonging the service life of the electrolysis cell and the like as an important part of the electrically conductive and lining of the electrolysis cell.
[0003] However, when low-temperature aluminum electrolysis production is carried out on the current industrialized pre-baked carbon anode aluminum electrolysis cell, the low-temperature electrolyte system usually contains a high potassium, and the penetration and damage to the carbonaceous cathode are strong. In particular, when the aluminum electrolysis cell uses ordinary carbon blocks, semi-graphitic, graphitic cathode materials, the cathode is prone to swelling and cracking after being eroded by potassium. The graphitized cathode has a slightly smaller risk of swelling and cracking due to potassium, but the soft graphite is weak against potassium penetration, and there is a problem of layered pulverization and peeling due to potassium erosion during long-term operation. Therefore, it is urgent to develop a method that can solve the problem of sodium and potassium penetration and damage of the low-temperature electrolyte to the cathode. SUMMARY
[0004] The present application provides a graphitized cathode and a preparation method thereof, an aluminum electrolysis cell, and an aluminum electrolysis method, to solve the technical problem of how to resist the sodium and potassium penetration and damage of the low-temperature electrolyte to the graphitized cathode.
[0005] In a first aspect, the present application provides a graphitized cathode, which comprises: a graphitized cathode base; and a TiB2 composite layer covering at least part of the surface of the graphitized cathode base, the carbon content of the TiB2 composite layer being < 20 wt.%, and the thickness of the TiB2 composite layer being 5-50 mm.
[0006] In a second aspect, the present application provides a preparation method of the graphitized cathode of the first aspect, which comprises: obtaining a TiB2 composite paste-like material and / or a TiB2 composite powder-like material; laying the TiB2 composite paste-like material on the surface of the graphitized cathode paste to obtain a mixed material; or laying the TiB2 composite powder-like material on the surface of the graphitized cathode paste to obtain a mixed material; or TiB2 composite paste is laid on the surface of the graphitized cathode paste, and TiB2 composite powder is laid on the upper surface of the TiB2 composite paste to obtain a mixture; The mixture is integrally pressed and sintered to obtain a graphitized cathode.
[0007] Optionally, the components of the TiB2 composite paste are as follows: 12wt.%-15wt.% of pitch, 0.1wt.%-1wt.% of graphite fiber, and the balance of TiB2 powder.
[0008] Optionally, the components of the TiB2 composite powder are as follows: 2wt.%-10wt.% of TiN powder, 1wt.%-5wt.% of CoB powder, 1wt.%-3wt.% of ZrB2 powder, 1wt.%-3wt.% of metal powder, 1wt.%-2wt.% of polyvinyl alcohol binder, and the balance of TiB2 powder.
[0009] In a third aspect, the application provides a low-temperature aluminum electrolysis cell, which comprises the graphitized cathode of the first aspect.
[0010] Optionally, the aluminum electrolysis cell is provided with a forced heat dissipation device on the sidewall shell; The distance between the sidewall lining of the aluminum electrolysis cell and the carbon anode is greater than or equal to 320mm; After the graphitized cathode is connected with the cathode current collector rod, the vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode current collector rod is greater than or equal to 300mm.
[0011] Optionally, the distance between the sidewall lining of the aluminum electrolysis cell and the carbon anode is 320mm-380mm; The vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode current collector rod is 300mm-340mm.
[0012] Optionally, the forced heat dissipation device comprises one or more of vertical heat dissipation fins, air-cooled heat exchangers, and heat-conducting oil cooling heat exchangers; The connection between the graphitized cathode and the cathode current collector rod is made by phosphorus cast iron, and the cathode current collector rod is made of one of high-conductivity steel rods and copper-plated steel rods.
[0013] In a fourth aspect, the application provides a low-temperature aluminum electrolysis method, which uses the low-temperature aluminum electrolysis cell of any one of the third aspect, and the method comprises the following parameters: the initial crystallization temperature of the low-temperature electrolyte is 820℃-850℃, the electrolysis temperature is 845℃-900℃, and the superheat is 20℃-50℃.
[0014] Optionally, the composition of the cryogenic electrolyte is: KF: 12wt.%-15wt.%, LiF: 1wt.%-2wt.%, CaF2: 0-5wt.%, MgF2: 0-2wt.%, Al2O3: 2wt.%-4wt.%, NaF: 26wt.%-33wt.%, with the balance being AlF3.
[0015] The technical solutions provided in this application have the following advantages compared with the prior art: This application provides a graphitized cathode comprising: a graphitized cathode substrate; and a TiB2 composite layer, wherein the TiB2 composite layer covers at least a portion of the surface of the graphitized cathode substrate, the carbon content of the TiB2 composite layer is <20 wt.%, and the thickness of the TiB2 composite layer is 5 mm-50 mm. First, in the harsh environment of an electrolytic cell, the TiB2 composite material exhibits excellent resistance to sodium and potassium permeation in the low-temperature electrolyte. Second, when the carbon content in the TiB2 composite material is less than 20 wt.%, the prepared cathode has good wettability with molten aluminum, high hardness, and can effectively resist sodium and potassium permeation expansion in the low-temperature electrolyte. Third, limiting the thickness of the composite layer to 5 mm-50 mm satisfies the resistance to permeation expansion between the cathode and molten aluminum. Furthermore, when the thickness of the composite layer exceeds 50 mm, the difference in sintering shrinkage between the TiB2 composite material and the graphitized cathode may cause microcracks in the composite layer, thereby reducing its resistance to permeation. This resists the sodium-potassium permeation damage to the graphitized cathode by the low-temperature electrolyte. Attached Figure Description
[0016] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.
[0017] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0018] Figure 1 A schematic diagram of a graphitized cathode provided in an embodiment of this application; Figure 2 A flowchart illustrating a method for preparing a graphitized cathode, as provided in this application embodiment; Figure 3 A schematic diagram of a low-temperature aluminum electrolysis cell provided in an embodiment of this application; Attached image description: 1-Anode guide rod; 2-Gas collection hood and tank cover plate; 3-Anode steel claw; 4-Anode; 5-Furnace side crust; 6-Forced heat dissipation device; 7-TiB2 composite layer; 8-Graphitized cathode substrate; 9-Insulation material; 10-Cathode current collector (copper steel rod inserted); 11-Aluminum liquid; 13-Side wall lining; 14-Electrolyte melt; 15-Heat exchange medium outlet. Detailed Implementation
[0019] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0020] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.
[0021] Furthermore, in the description of this application, the terms "comprising," "including," etc., mean "including but not limited to." In this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this document, "and / or" describes the relationship between related objects, indicating that three relationships can exist; for example, A and / or B can represent: A alone, A and B simultaneously, or B alone. A and B can be singular or plural. In this document, "at least one" means one or more, and "more than" means two or more. "At least one," "at least one of the following," or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c" or "at least one of a, b, and c" can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be a single or multiple.
[0022] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0023] The inventive concept of this application is as follows: Low-temperature aluminum electrolysis offers advantages such as reduced heat dissipation from the electrolytic cell, lower energy consumption, and improved current efficiency, and is considered an important direction for energy conservation in the aluminum electrolysis industry. Furthermore, low-temperature aluminum electrolysis is also a crucial approach to improving the corrosion resistance of inert anodes; therefore, it has been extensively studied in the aluminum smelting field.
[0024] However, there are still many difficulties in carrying out low-temperature aluminum electrolysis production on the current industrialized prebaked carbon anode aluminum electrolysis cells, mainly: (1) The solubility and dissolution rate of alumina are low under low-temperature electrolysis conditions. If the alumina added to the electrolysis cell cannot dissolve and diffuse in time, it will precipitate to the bottom of the electrolysis cell. In addition, Na +The directional migration and enrichment effect towards the cathode causes the molecular ratio and primary crystal temperature of the melt in the cathode region to rise. Under low-temperature electrolysis conditions, the high molecular ratio melt in the cathode region and the alumina precipitate are very likely to form a crust, which affects the normal operation of the electrolytic cell. (2) If the problem of precipitation crust is solved by simply using the method of high superheat, it will bring the problem of the difficulty in forming furnace wall crust to protect the side material of the electrolytic cell, and will also affect the current efficiency and aggravate the volatilization of electrolyte. (3) Low-temperature electrolyte systems usually contain high potassium, which has a strong penetrating and destructive effect on carbon cathodes. In particular, when aluminum electrolytic cells use ordinary carbon blocks, semi-graphite, or graphite cathode materials, the cathode is prone to expansion and cracking after being corroded by potassium. The risk of potassium expansion and cracking in graphitized cathodes is slightly lower, but graphite is soft and has weak resistance to potassium penetration. Long-term operation also has the problem of layered pulverization and peeling due to potassium erosion; (4) Compared with conventional electrolyte systems, the conductivity of low-temperature electrolyte systems is usually lower, which will lead to an increase in cell voltage. If the cell voltage is directly reduced, the electrode spacing will be compressed. Due to the fluctuation of aluminum liquid, the compression of electrode spacing will increase the oxidation loss of aluminum liquid and reduce the current efficiency. Therefore, before there are better current stabilization (reducing aluminum liquid fluctuation) measures, it is not easy to achieve low-voltage operation in low-temperature aluminum electrolysis, thus limiting the energy-saving effect of low-temperature aluminum electrolysis.
[0025] Currently, there is some research on low-temperature aluminum electrolysis. Patents CN201610868647.5, CN201210417817.X, and CN200910312193.3 provide low-temperature aluminum electrolytes for temperatures above 880℃ or 850℃, focusing on solving the problems of low conductivity, low alumina solubility, and low dissolution rate. Patents CN201010207080.X and CN201010587618.4 provide a highly conductive titanium boride cathode material and its preparation method that can highly wet with molten aluminum, resist electrolyte penetration and erosion by molten aluminum, and has a lower cost than hot-pressed cathodes. However, from the perspective of the preparation process, achieving large-scale application and use in existing prebaked anode aluminum electrolysis cells still requires further research and development. Patents CN200710119898.4 and CN200710119908.4 describe a production method for preparing graphitized wettable cathode carbon blocks containing TiB2 composite layers by vibration molding. However, the carbon content is still too high, even reaching about 80 wt.%.
[0026] The patented technologies mentioned above address individual technical problems in low-temperature aluminum electrolysis from a single perspective, and simple integration is insufficient to achieve true low-temperature aluminum electrolysis. To solve the technical challenges of industrializing low-temperature aluminum electrolysis, in addition to considering the cathode and low-temperature electrolyte system, comprehensive improvements are needed in aspects such as the electrolytic cell structure, furnace wall formation, and low-voltage operation to truly realize low-temperature aluminum electrolysis. Selecting a suitable low-temperature electrolyte system, maintaining matching process control parameters, and improving alumina dissolution performance are crucial. Furthermore, it is necessary to effectively address the sodium and potassium erosion of the carbonaceous cathode by the electrolyte melt in industrial electrolytic cells, resolve the furnace wall formation problem under high superheat conditions in the low-temperature electrolyte system, and solve the problems of aluminum liquid stability and high current efficiency under low-voltage conditions.
[0027] In summary, there is still a lack of complete low-temperature aluminum electrolysis technologies in this field to realize the industrial production of low-temperature aluminum electrolysis.
[0028] Figure 1 This is a schematic diagram of a graphitized cathode provided in an embodiment of this application.
[0029] To address the aforementioned technical issues to some extent, please refer to [link / reference]. Figure 1 This application provides a graphitized cathode, the graphitized cathode comprising: Graphitized cathode substrate; and A TiB2 composite layer is formed, which covers at least a portion of the surface of the graphitized cathode substrate. The carbon content of the TiB2 composite layer is <20 wt.%, and the thickness of the TiB2 composite layer is 5 mm to 50 mm.
[0030] First, TiB2 composite materials exhibit excellent performance in the harsh environment of electrolytic cells due to their high hardness, high melting point, wear resistance, and corrosion resistance. In particular, TiB2 composite materials demonstrate superior resistance to sodium and potassium permeation in low-temperature electrolytes. Second, laboratory-scale electrolysis tests show that when the carbon content in the TiB2 composite material is less than 20 wt.%, the prepared cathode exhibits good wettability with molten aluminum, high hardness, and effective resistance to sodium and potassium permeation expansion in low-temperature electrolytes. This finding provides important reference for industrial production. Third, laboratory studies have found that the penetration depth of sodium and potassium permeation expansion is less than 5 mm. Therefore, limiting the composite layer thickness to 5 mm-50 mm satisfies the requirements for wettability, resistance to permeation expansion, and wear resistance of the cathode with molten aluminum. Thinner composite layers may not provide sufficient protection, while excessively thick composite layers increase cost and weight. Furthermore, when the composite layer thickness exceeds 50 mm, the difference in sintering shrinkage between the TiB2 composite material and the graphitized cathode may lead to microcracks in the composite layer, thereby reducing its resistance to permeation. For example, the carbon content of the TiB2 composite layer can be 0, 2 wt.%, 4 wt.%, 6 wt.%, 10 wt.%, 12 wt.%, 15 wt.%, 19 wt.%, etc., and the thickness of the TiB2 composite layer can be 5 mm, 10 mm, 15 mm, 20 mm, 30 mm, 40 mm, 50 mm, etc.
[0031] Figure 2 This is a schematic flowchart illustrating a method for preparing a graphitized cathode according to an embodiment of this application.
[0032] Please see Figure 2 This application provides a method for preparing the graphitized cathode described above, the method comprising: S1. Obtain TiB2 composite paste and / or TiB2 composite powder; S2a. A mixture is obtained by spreading TiB2 composite paste on the surface of graphitized cathode paste; or S2b, TiB2 composite powder is spread on the surface of graphitized cathode paste to obtain a mixture; or S2c. Lay TiB2 composite paste on the surface of graphitized cathode paste, and lay TiB2 composite powder on the upper surface of TiB2 composite paste to obtain a mixture. S3. The mixture is integrally pressed, molded, and sintered to obtain a graphitized cathode.
[0033] This application employs an integrated molding and sintering technology to directly form a TiB2 composite material layer on the surface of a graphitized cathode. This technology not only ensures a tight bond between the composite layer and the graphitized cathode substrate but also avoids the peeling problem that may occur with traditional coatings. Furthermore, the raw materials used to form the TiB2 composite layer can be TiB2 composite paste, TiB2 composite powder, or a combination of both. When the raw materials for the TiB2 composite layer are a combination of TiB2 composite paste and TiB2 composite powder, a transition from low-carbon to carbon-free TiB2 composite materials can be achieved, increasing the thickness of the TiB2 composite material layer.
[0034] In some embodiments, the TiB2 composite paste is prepared by hot kneading.
[0035] In some embodiments, the TiB2 composite paste comprises: 12wt.%-15wt.% asphalt, 0.1wt.%-1wt.% graphite fiber, and the balance being TiB2 powder.
[0036] Before being molded together with the graphitized cathode paste, the TiB2 composite material exists in the form of a paste. This paste has good flowability and plasticity, facilitating coating and molding on the surface of the graphitized cathode. Through specific pressing methods (such as molding and extrusion), the paste can be uniformly coated onto the cathode surface and sintered at high temperatures to form a dense composite layer. Asphalt is used as a binder. Asphalt can melt at high temperatures and firmly bind the other components together to form a dense and stable composite layer. Simultaneously, asphalt also has a certain degree of corrosion resistance, which can protect the matrix from electrolyte erosion to some extent. The addition of graphite fibers enhances the strength and toughness of the composite material, improving its wear resistance and impermeability during electrolysis. Furthermore, graphite fibers have good electrical conductivity, helping to maintain the normal operation of the electrolytic cell. TiB2 powder is the main component of the composite material, accounting for the remainder. Due to the high hardness and high melting point of TiB2, this composite material performs excellently in the harsh environment of the electrolytic cell. Meanwhile, by controlling the amount of TiB2 powder, the carbon content of the composite material can be ensured to be less than 20 wt.%, thus meeting specific performance requirements. For example, the content of bitumen can be 12 wt.%, 12.5 wt.%, 13 wt.%, 13.5 wt.%, 14 wt.%, 15 wt.%, etc., and the content of graphite fiber can be 0.1 wt.%, 0.3 wt.%, 0.5 wt.%, 0.7 wt.%, 0.9 wt.%, 1 wt.%, etc.
[0037] In some embodiments, the TiB2 composite powder is prepared by wet ball milling and spray granulation.
[0038] In some embodiments, the TiB2 composite powder comprises: 2wt.%-10wt.% TiN powder, 1wt.%-5wt.% CoB powder, 1wt.%-3wt.% ZrB2 powder, 1wt.%-3wt.% metal powder, 1wt.%-2wt.% polyvinyl alcohol binder, with the balance being TiB2 powder.
[0039] Before being molded together with the graphitized cathode paste, the TiB2 composite material exists in powder form. This powder form facilitates mixing and uniform dispersion of various components, and also facilitates subsequent molding and processing. Through specific pressing processes (such as molding and extrusion), the powder can be uniformly coated on the cathode surface, and a dense composite layer is formed after high-temperature sintering. TiN (titanium nitride) is a material with high hardness, high wear resistance, and good chemical stability. Its addition can enhance the hardness and wear resistance of the TiB2 composite material, thereby improving the service life of the electrolytic cell cathode. CoB powder can improve the strength and conductivity of the composite material. ZrB2 (zirconium diboride) is a material with high melting point, high hardness, and good corrosion resistance. Its addition can further improve the high-temperature resistance and corrosion resistance of the composite material. The addition of metal powder can improve the conductivity and mechanical properties of the composite material, and can also aid sintering. Common metal powders include one or more alloys of nickel, iron, and copper. Polyvinyl alcohol, as a binder, can form a strong bond between powder particles, enabling the composite material to maintain a stable shape and structure during molding. For example, the content of TiN powder can be 2wt.%, 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 9wt.%, 10wt.%, etc.; the content of CoB powder can be 1wt.%, 2wt.%, 3wt.%, 4wt.%, 5wt.%, etc.; the content of ZrB2 powder can be 1wt.%, 1.5wt.%, 2wt.%, 2.5wt.%, 3wt.%, etc.; the content of metal powder can be 1wt.%, 1.5wt.%, 2wt.%, 2.5wt.%, 3wt.%, etc.; and the content of polyvinyl alcohol binder can be 1wt.%, 1.2wt.%, 1.4wt.%, 1.6wt.%, 1.8wt.%, 2wt.%, etc.
[0040] The product prepared by the method of preparing the graphitized cathode is the graphitized cathode described above. The chemical composition and microstructure of the graphitized cathode prepared by the method of preparing the graphitized cathode can be referred to the above embodiments. Since the method of preparing the graphitized cathode adopts some or all of the technical solutions of the graphitized cathode embodiments, it has at least all the beneficial effects brought about by the technical solutions of the graphitized cathode embodiments, which will not be elaborated here.
[0041] Figure 3This is a schematic diagram of a low-temperature aluminum electrolysis cell provided in an embodiment of this application.
[0042] Please see Figure 3 Based on a general inventive concept, this application provides a low-temperature aluminum electrolysis cell, which includes the graphitized cathode described above.
[0043] In some embodiments, a forced heat dissipation device is provided on the side wall shell of the aluminum electrolysis cell; The distance between the inner lining of the side wall of the aluminum electrolytic cell and the carbon anode is ≥320mm; After the graphitized cathode is connected to the cathode current collector, the vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode current collector is ≥300mm.
[0044] In some embodiments, the distance between the sidewall lining of the aluminum electrolytic cell and the carbon anode is 320mm-380mm; The vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode current collector is 300mm-340mm.
[0045] In some embodiments, the forced heat dissipation device includes one or more of the following: vertical heat sinks, air-cooled heat exchangers, and heat transfer oil-cooled heat exchangers; The connection between the graphitized cathode and the cathode current collector is made by casting with phosphorus pig iron, and the cathode current collector is made of either a high-conductivity steel rod or a copper-inserted steel rod.
[0046] This application addresses the problem of low-temperature electrolytes failing to form a protective crust on the sidewall lining by adding a forced heat dissipation device to the sidewall of the electrolytic cell and designing a wide distance between the side lining and the carbon anode. The forced heat dissipation device facilitates the formation of a crust on the sidewall lining by the electrolyte melt inside the electrolytic cell. The 320mm-380mm wide distance between the side lining and the carbon anode allows for dynamic adjustment of the crust thickness. Furthermore, the forced heat dissipation device can also serve as a heat balance regulation method, enabling the electrolytic cell to perform current enhancement or variable load production. For example, the distance between the sidewall lining and the carbon anode of an aluminum electrolytic cell can be 320mm, 330mm, 340mm, 350mm, 360mm, 370mm, 380mm, etc.
[0047] This application reduces the horizontal current in the molten aluminum in an aluminum electrolysis cell and improves the stability of the molten aluminum by controlling the high-conductivity current collector / copper-inserted current collector and the vertical distance between the upper surface of the current collector and the upper surface of the graphitized cathode, thereby achieving low electrode spacing, low voltage, and high efficiency operation. The stability of the molten aluminum in the electrolysis cell is affected by the Lorentz force generated by the combined action of the vertical magnetic field and the horizontal current. The vertical magnetic field is determined by the cathode bus system of the electrolysis cell and is difficult to change; therefore, reducing the horizontal current becomes the main means to improve the stability of the molten aluminum. Research results show that when using a graphitized cathode, a vertical distance greater than 300 mm between the upper surface of the high-conductivity cathode current collector and the upper surface of the graphitized cathode can significantly reduce the horizontal current in the molten aluminum. A larger vertical distance yields better results, but considering the actual height range of the cathode and the cross-sectional area of the current collector, a vertical distance of 300 mm to 340 mm is more reasonable. For example, the vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode current collector can be 300 mm, 310 mm, 320 mm, 330 mm, 340 mm, etc.
[0048] This application provides a low-temperature aluminum electrolysis method, wherein the method uses the low-temperature aluminum electrolysis cell described in any one of the above-mentioned methods, and the method includes the following parameters: the initial crystallization temperature of the low-temperature electrolyte is 820℃-850℃, the electrolysis temperature is 845℃-900℃, and the superheat is 20℃-50℃.
[0049] In some embodiments, the composition of the cryogenic electrolyte is: KF: 12wt.%-15wt.%, LiF: 1wt.%-2wt.%, CaF2: 0-5wt.%, MgF2: 0-2wt.%, Al2O3: 2wt.%-4wt.%, NaF: 26wt.%-33wt.%, with the balance being AlF3.
[0050] First, this invention employs a low-temperature electrolyte with an initial crystallization temperature in the range of 820-850℃. This temperature range is set based on optimization of the electrolysis process and considerations for cathodic protection. Simultaneously, this electrolyte system exhibits relatively high conductivity and alumina saturation concentration, which helps improve electrolysis efficiency and reduce alumina precipitation. To further enhance the electrolyte's performance, this invention adds two additives, LiF and KF. However, the amounts of these two additives need to be strictly controlled to balance their different effects on electrolyte performance. The addition of LiF significantly improves the electrolyte's conductivity, but also significantly reduces the saturation solubility of alumina. Experimental studies show that when the LiF content exceeds 3 wt.%, its effect on the saturation solubility of alumina becomes significant. Therefore, to maintain the saturation solubility of alumina at a certain level, this invention controls the LiF content to within 2 wt.%. The addition of KF can improve the saturation solubility of alumina, but at the same time, it increases the penetration damage to the carbon cathode. Experimental studies have found that when the KF content is below 15 wt.%, the potassium expansion effect on the graphitized cathode is relatively small. Therefore, this invention controls the KF content to a level close to but not exceeding 15 wt.% to ensure the stability and safety of the cathode. After determining the addition amounts of LiF and KF, this invention further adjusts the electrolyte composition by keeping the KF / (KF+NaF) ratio constant and reducing the molecular ratio (i.e., increasing the AlF3 content). This allows for obtaining an optimal electrolyte composition with relatively high conductivity and alumina saturation solubility while maintaining a constant primary crystallization temperature range. Finally, this invention also verifies the effectiveness of this low-temperature electrolyte system at superheats of 20-50℃ through laboratory-scale electrolysis experiments. The experimental results show that no crust formation occurs on the cathode within this superheat range. Therefore, this invention controls the superheat between 20-50℃ to ensure the smooth progress of the electrolysis process and the stable operation of the cathode. In summary, this invention successfully solves the problem of alumina precipitation and crust formation by optimizing the electrolyte composition and controlling the superheat, providing new ideas and solutions for the development of the aluminum electrolysis industry. The initial crystallization temperatures of the low-temperature electrolyte are 820℃, 825℃, 830℃, 835℃, 840℃, 845℃, 850℃, etc., and the electrolysis temperatures can be 845℃, 855℃, 865℃, 875℃, 885℃, 895℃, 900℃, etc., and the superheat can be 20℃, 25℃, 30℃, 35℃, 40℃, 45℃, 50℃, etc.
[0051] The present application is further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the application. Experimental methods in the following embodiments that do not specify specific conditions are generally determined according to industry standards. If there is no corresponding industry standard, then common international standards, conventional conditions, or conditions recommended by the manufacturer are followed.
[0052] Example 1 In a certain aluminum electrolysis enterprise, a 300kA prebaked carbon anode aluminum electrolysis cell was overhauled and transformed into a low-temperature aluminum electrolysis cell for low-temperature aluminum electrolysis production.
[0053] The average thickness of the low-carbon TiB2 composite layer on the surface of the graphitized cathode substrate is approximately 50 mm, and the measured carbon content of the TiB2 composite layer is 7.96%. This low-carbon TiB2 composite material consists of 12 wt.% pitch, 1 wt.% graphite fiber, and 87 wt.% TiB2 powder. It is prepared into a paste through hot kneading, uniformly spread on the surface of the graphitized cathode paste, and then integrally pressed and sintered with the graphitized cathode paste to obtain the graphitized cathode. A high-conductivity steel rod (room temperature resistivity 11 × 10⁻⁶) is used. -8 Ω·m), cast iron with phosphorus, the vertical distance h from the upper surface of the steel rod to the upper surface of the graphitized cathode is 340mm; the forced heat dissipation device on the side wall shell of the electrolytic cell is a vertical heat sink, and heat dissipation holes are opened on the horizontal edge plate of the electrolytic cell to better achieve convective heat dissipation; the inner lining of the side wall is made of silicon carbide combined with silicon nitride material with a thickness of 60mm, and the distance b from the inner lining to the carbon anode is 320mm.
[0054] The design composition of the cryogenic electrolyte, by mass percentage, is: KF 14wt.%; LiF 2wt.%; CaF2 4wt.%; MgF2 0.5wt.%; Al2O3 3.2wt.%; NaF 32wt.%; AlF3 44.3wt.%; with a molecular ratio CR = 1.44. During electrolysis, electrolyte samples were taken from different locations in the electrolytic cell, and the initial crystallization temperature was measured, with an average value of 846℃. The electrolysis temperature ranged from 895 to 900℃, with a superheat of approximately 50℃. The anolyte current density was 0.762 A / cm³. 2 The effect coefficient is less than 0.06 times / cell day, the furnace wall thickness is 183.6 mm, the electrolytic cell operating voltage is 3.774 V, the current efficiency is 93.95 wt.%, and the DC power consumption is 11971 kWh / t-Al. During the operating cycle of the electrolytic cell in this embodiment, the graphitized cathode with low-carbon TiB2 composite material on the electrolytic cell remained undamaged, and no alumina crust was found on the bottom of the cell.
[0055] Example 2 In a certain aluminum electrolysis enterprise, a 300kA prebaked carbon anode aluminum electrolysis cell was overhauled and transformed into a low-temperature aluminum electrolysis cell for low-temperature aluminum electrolysis production.
[0056] The average thickness of the low-carbon TiB2 composite layer on the surface of the graphitized cathode substrate is approximately 30 mm, and the measured carbon content of the TiB2 composite layer is 8.3%. This low-carbon TiB2 composite material consists of 15 wt.% pitch, 0.1 wt.% graphite fiber, and 84.9 wt.% TiB2 powder. These components are prepared into a paste through hot kneading, uniformly spread on the surface of the graphitized cathode paste, and then integrally pressed and sintered with the graphitized cathode paste to obtain the graphitized cathode. A copper-inserted cathode steel rod (with a room temperature resistivity of 7.8 × 10⁻⁶) is used. -8 Ω·m), cast iron with phosphorus, the vertical distance h from the upper surface of the steel rod to the upper surface of the graphitized cathode is 300mm; the forced heat dissipation device on the side wall shell of the electrolytic cell is a vertical heat sink, and heat dissipation holes are opened on the horizontal edge plate of the electrolytic cell to better achieve convective heat dissipation; the inner lining of the side wall is made of silicon carbide combined with silicon nitride material with a thickness of 60mm, and the distance b from the inner lining to the carbon anode is 320mm.
[0057] The design composition of the low-temperature electrolyte, by mass percentage, is: KF 15wt.%; LiF 2wt.%; CaF2 2.5wt.%; MgF2 2wt.%; Al2O3 3.2wt.%; NaF 31wt.%; AlF3 44.3wt.%; with a molecular ratio CR = 1.40. During electrolysis, electrolyte samples were taken from different locations in the electrolytic cell, and the initial crystallization temperature was measured, with an average value of 838℃. The electrolysis temperature was 870-875℃, with a superheat of approximately 35℃; the anolyte current density was 0.762 A / cm³. 2 The effect coefficient is less than 0.07 times / cell day, the furnace wall thickness is 196.4 mm, the electrolytic cell operating voltage is 3.768 V, the current efficiency is 93.88 wt.%, and the DC power consumption is 11961 kWh / t-Al. During the operating cycle of the electrolytic cell in this embodiment, the graphitized cathode with low-carbon TiB2 composite material on the electrolytic cell remained undamaged, and no alumina crust was found on the bottom of the cell.
[0058] Example 3 In a certain aluminum electrolysis enterprise, a 300kA prebaked carbon anode aluminum electrolysis cell was overhauled and transformed into a low-temperature aluminum electrolysis cell for low-temperature aluminum electrolysis production.
[0059] The average thickness of the low-carbon TiB2 composite layer on the surface of the graphitized cathode substrate is approximately 5 mm, and the measured carbon content of the TiB2 composite layer is less than 0.01%. This low-carbon TiB2 composite material consists of 10 wt.% TiN powder, 1 wt.% CoB powder, 1 wt.% ZrB2 powder, 3 wt.% nickel-iron alloy powder (nickel: 40 wt.%, iron: 60 wt.%), 2 wt.% polyvinyl alcohol binder (CAS No.: 9002-89-5), and 83 wt.% TiB2 powder. It was prepared into a powder by wet ball milling and spray granulation. This powder was uniformly spread on the surface of the graphitized cathode paste, and then integrally pressed and sintered with the graphitized cathode paste to obtain the graphitized cathode. A copper-inserted cathode steel rod (room temperature resistivity 7.8 × 10⁻⁶) was used. -8 Ω·m), cast iron with phosphorus, the vertical distance h from the upper surface of the steel rod to the upper surface of the graphitized cathode is 300mm; the forced heat dissipation device on the side wall shell of the electrolytic cell is a vertical heat sink, and heat dissipation holes are opened on the horizontal edge plate of the electrolytic cell to better achieve convective heat dissipation; the inner lining of the side wall is made of silicon carbide combined with silicon nitride material with a thickness of 60mm, and the distance b from the inner lining to the carbon anode is 320mm.
[0060] The design composition of the low-temperature electrolyte, by mass percentage, is: KF 12; LiF 1wt.%; Al2O3 3.2wt.%; CaF2 0wt.%; MgF2 2wt.%; NaF 33wt.%; AlF3 48.8wt.%; molecular ratio CR = 1.35. During electrolysis, electrolyte samples were taken from different locations in the electrolytic cell to test the initial crystallization temperature, which had an average value of 832℃. The electrolysis temperature was 870-875℃, with a superheat of approximately 40℃; the anolyte current density was 0.762 A / cm³. 2 The effect coefficient is less than 0.07 times / cell day, the furnace wall thickness is 190.6 mm, the electrolytic cell operating voltage is 3.776 V, the current efficiency is 94.05 wt.%, and the DC power consumption is 11964 kWh / t-Al. During the operating cycle of the electrolytic cell in this embodiment, the graphitized cathode with low-carbon TiB2 composite material on the electrolytic cell remained undamaged, and no alumina crust was found on the bottom of the cell.
[0061] Example 4 In a certain aluminum electrolysis enterprise, a 300kA prebaked carbon anode aluminum electrolysis cell was overhauled and transformed into a low-temperature aluminum electrolysis cell for low-temperature aluminum electrolysis production.
[0062] The average thickness of the low-carbon TiB2 composite layer on the surface of the graphitized cathode substrate is approximately 50 mm. The measured carbon content of the TiB2 composite layer is less than 0.01% on the surface and 8.12% on the inner layer. This low-carbon TiB2 composite material uses both paste and powder forms. The paste consists of 12 wt.% pitch, 2 wt.% graphite fiber, and 86 wt.% TiB2 powder, which are prepared by hot kneading and uniformly spread on the surface of the graphitized cathode paste, followed by uniformly spreading the powder form. The powdered material consists of 2 wt.% TiN powder, 5 wt.% CoB powder, 3 wt.% ZrB2 powder, 1 wt.% nickel-iron alloy powder (nickel: 40 wt.%, iron: 60 wt.%), 1 wt.% polyvinyl alcohol binder, and 88 wt.% TiB2 powder. It is prepared into a powdered material through wet ball milling and spray granulation, and then integrated with graphitized cathode paste through pressing and sintering to obtain a graphitized cathode. A copper-inserted cathode steel rod (room temperature resistivity 7.8 × 10⁻⁶) is used. -8 Ω·m), cast iron with phosphorus, the vertical distance h from the upper surface of the steel rod to the upper surface of the graphitized cathode is 300mm; the forced heat dissipation device on the side wall shell of the electrolytic cell is an air-cooled heat exchanger, and the heat exchange medium 15 is air; the side wall lining is made of silicon carbide combined with silicon nitride material with a thickness of 60mm, and the distance b from the lining to the carbon anode is 320mm.
[0063] The design composition of the low-temperature electrolyte, by mass percentage, is: KF 14%; LiF 2 wt.%; CaF 25 wt.%; MgF 20 wt.%; Al₂O₃ 3.2 wt.%; NaF 30 wt.%; AlF 345.8 wt.%; molecular ratio CR = 1.31. During electrolysis, electrolyte samples were taken from different locations in the electrolytic cell to test the initial crystallization temperature, which had an average value of 823℃. The electrolysis temperature was 850-855℃, with a superheat of approximately 30℃; the anolyte current density was 0.762 A / cm². 2 The effect coefficient is less than 0.07 times / cell day, the furnace wall thickness is 195.7 mm, the electrolytic cell operating voltage is 3.759 V, the current efficiency is 93.81 wt.%, and the DC power consumption is 11941 kWh / t-Al. During the operating cycle of the electrolytic cell in this embodiment, the graphitized cathode with low-carbon TiB2 composite material on the electrolytic cell was undamaged, and no alumina crust was found on the bottom of the cell.
[0064] Example 5 In a certain aluminum electrolysis enterprise, a 400kA prebaked carbon anode aluminum electrolysis cell was overhauled and transformed into a low-temperature aluminum electrolysis cell for low-temperature aluminum electrolysis production.
[0065] The average thickness of the low-carbon TiB2 composite layer on the surface of the graphitized cathode substrate is approximately 50 mm. The measured carbon content of the TiB2 composite layer is less than 0.01% on the surface and 8.23% on the inner layer. This low-carbon TiB2 composite material utilizes both paste and powder formulations. The paste consists of 12 wt.% bitumen, 2 wt.% graphite fiber, and 86 wt.% TiB2 powder, prepared by hot kneading and uniformly spread on the surface of the graphitized cathode paste, followed by a uniform spread of the powder. The powder consists of 5 wt.% TiN powder, 5 wt.% CoB powder, 1 wt.% ZrB2 powder, 1 wt.% nickel-iron alloy powder (nickel: 40 wt.%, iron: 60 wt.%), 1 wt.% polyvinyl alcohol binder, and 87 wt.% TiB2 powder, prepared by wet ball milling and spray granulation. Finally, the graphitized cathode paste is integrally pressed, molded, and sintered to obtain the graphitized cathode; a copper-inserted cathode steel rod (room temperature resistivity 8.05 × 10⁻⁶) is used. -8 Ω·m), cast iron with phosphorus, the vertical distance h from the upper surface of the steel rod to the upper surface of the graphitized cathode is 320mm; the forced heat dissipation device on the side wall shell of the electrolytic cell is a heat transfer oil heat exchanger, the heat exchange medium 15 is heat transfer oil; the side wall lining is made of silicon carbide combined with silicon nitride material, with a thickness of 60mm, and the distance b from the lining to the carbon anode is 380mm.
[0066] The design composition of the low-temperature electrolyte, by mass percentage, is: KF 14%; LiF 2 wt.%; CaF2 4 wt.%; MgF2 0.5 wt.%; Al2O3 2.8 wt.%; NaF 30.5 wt.%; AlF3 46.2 wt.%; molecular ratio CR = 1.32. During electrolysis, electrolyte samples were taken from different locations in the electrolytic cell to test the initial crystallization temperature, which had an average value of 826℃. The electrolysis temperature was 845-850℃, with a superheat of approximately 20℃. The anolyte current density was 0.802 A / cm³. 2 The effect coefficient is less than 0.08 times / cell day, the furnace wall thickness is 205.7 mm, the electrolytic cell operating voltage is 3.772 V, the current efficiency is 93.88 wt.%, and the DC power consumption is 11973 kWh / t-Al. During the operating cycle of the electrolytic cell in this embodiment, the graphitized cathode with low-carbon TiB2 composite material on the electrolytic cell remained undamaged, and no alumina crust was found on the bottom of the cell.
[0067] Furthermore, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages: In this embodiment of the invention, a synergistic solution and optimal parameters were determined through systematic research to address the key issues faced in the industrial production of low-temperature aluminum electrolysis, forming a complete set of low-temperature aluminum electrolysis technologies. This technology can realize industrial-scale low-temperature aluminum electrolysis production, has significant practical value, and has broad application prospects.
[0068] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A graphitized cathode, characterized in that, The graphitized cathode comprises: Graphitized cathode substrate; and A TiB2 composite layer is formed, which covers at least a portion of the surface of the graphitized cathode substrate. The carbon content of the TiB2 composite layer is <20 wt.%, and the thickness of the TiB2 composite layer is 5 mm to 50 mm. The graphitized cathode is prepared by a method comprising the following steps: TiB2 composite paste and TiB2 composite powder were obtained; TiB2 composite paste is laid on the surface of graphitized cathode paste, and TiB2 composite powder is laid on the upper surface of TiB2 composite paste to obtain a mixture. The mixture is integrally pressed and sintered to obtain a graphitized cathode; The TiB2 composite paste is composed of: 12wt.%-15wt.% asphalt, 0.1wt.%-1wt.% graphite fiber, and the balance being TiB2 powder. The composition of the TiB2 composite powder is as follows: 2wt.%-10wt.% TiN powder, 1wt.%-5wt.% CoB powder, 1wt.%-3wt.% ZrB2 powder, 1wt.%-3wt.% metal powder, 1wt.%-2wt.% polyvinyl alcohol binder, and the balance is TiB2 powder.
2. A low-temperature aluminum electrolysis cell, characterized in that, The aluminum electrolytic cell includes the graphitized cathode as described in claim 1.
3. The low-temperature aluminum electrolytic cell according to claim 2, characterized in that, A forced heat dissipation device is provided on the side wall shell of the aluminum electrolysis cell. The distance between the inner lining of the side wall of the aluminum electrolytic cell and the carbon anode is ≥320mm; After the graphitized cathode is connected to the cathode current collector, the vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode current collector is ≥300mm.
4. The low-temperature aluminum electrolytic cell according to claim 3, characterized in that, The distance between the inner lining of the side wall of the aluminum electrolytic cell and the carbon anode is 320mm-380mm; The vertical distance between the upper surface of the graphitized cathode and the upper surface of the cathode current collector is 300mm-340mm.
5. The low-temperature aluminum electrolysis cell according to claim 3, characterized in that, The forced heat dissipation device includes one or more of the following: vertical heat sink, air-cooled heat exchanger, and heat transfer oil cooling heat exchanger; The connection between the graphitized cathode and the cathode current collector is made by casting with phosphorus pig iron, and the cathode current collector is made of either a high-conductivity steel rod or a copper-inserted steel rod.
6. A low-temperature aluminum electrolysis method, characterized in that, The method employs the low-temperature aluminum electrolytic cell described in any one of claims 2 to 5, and the method includes the following parameters: the initial crystallization temperature of the low-temperature electrolyte is 820℃-850℃, the electrolysis temperature is 845℃-900℃, and the superheat is 20℃-50℃.
7. The method according to claim 6, characterized in that, The composition of the cryogenic electrolyte is as follows: KF: 12wt.%-15wt.%, LiF: 1wt.%-2wt.%, CaF2: 0-5wt.%, MgF2: 0-2wt.%, Al2O3: 2wt.%-4wt.%, NaF: 26wt.%-33wt.%, with the balance being AlF3.
Citation Information
Patent Citations
Production method of graphitized wetable cathode carbon block for aluminium electrolysis bath
CN101158047A
Graphitized wetable cathode carbon block for aluminium electrolysis bath and production method thereof
CN101158048A
Low-temperature aluminum electrolysis process and electrolyte
CN101713082B
Titanium boride cathode material for aluminium electrolysis and preparation method thereof
CN101876079B
Titanium boride composite material for aluminum electrolysis and preparation method thereof
CN102010206A