A colored release film and a method for manufacturing the same
By coating a transparent polyester film with a colored release agent containing modified pigments, the problem of colorless transparent release films being difficult to distinguish is solved, enabling visualized quality monitoring of colored release films and simplifying the quality control process.
Patent Information
- Application Number
- CN202311649745.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-04
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-12-04
AI Technical Summary
The colorless and transparent release film of the present technology is difficult to identify by visual means as to whether a release film has been applied, and the residual release agent of colored release film is difficult to observe intuitively after removal, requiring complex testing processes for quality control.
A transparent polyester film is used as the substrate layer, and a colored release agent with modified pigments is coated on it. The release agent layer is formed by curing with ultraviolet light. The modified pigments are alkali-resistant inorganic pigments such as iron oxide red, cadmium sulfide or ultramarine. After surface modification treatment, a colored release film is formed, which enables visual observation of the release agent residue and quality.
It enables visual observation of the color of the release film, simplifies quality control, allows real-time monitoring of release agent residue and fogging, avoids complex testing processes, and improves the visibility and controllability of product quality.
Abstract
Description
Technical Field
[0001] This application relates to the field of chemical technology, particularly to the field of thin film materials technology in the chemical industry, and especially to a colored release film and its preparation method. Background Technology
[0002] Release film is a commonly used thin film material in the chemical industry. Also known as peeling film, release film, separation film, etc., it is a type of thin film with a separable surface. When in contact with specific materials under limited conditions, release film exhibits no stickiness or only slight stickiness. Release film is widely used in packaging, printing, screen printing, pad printing, nameplates, membrane switches, flexible circuits, insulating products, circuit boards, laser anti-counterfeiting, lamination, electronics, sealing materials, reflective materials, waterproof materials, pharmaceuticals (plaster paper), sanitary paper, adhesive products, die-cutting and stamping processes, and other industries.
[0003] CN 112375437 B discloses a release film substrate, comprising a polyester film and an activation coating. The activation coating is formed on the surface of the polyester film, and a silicone oil release agent is coated on the surface of the activation coating to form a release agent layer. The components of the activation coating are as follows: 80-100 parts by weight of acrylic resin, 1-2 parts by weight of dimethylsilyl alkyl silicate, 10-15 parts by weight of ethanolamine, 0.5-0.8 parts by weight of polyquaternium salt, 5-10 parts by weight of water-insoluble carbonate, 1-2 parts by weight of melamine, and 80-100 parts by weight of propylene glycol. Through this prior art, a porous hydrophilic activation coating is formed on the surface of the polyester film, significantly improving the surface activity and hydrophilicity of the release film substrate, which is beneficial for tight bonding with silicone oil-based release agents and can prevent the release agent from detaching.
[0004] CN 112661995 B discloses a release film for polarizing films, comprising a release film substrate and a release agent layer coated on the surface of the release film substrate. The release agent layer is made of a UV-curable release agent prepared from the following raw materials in parts by weight: 60-140 parts by weight of polybutadiene polyurethane, 45-85 parts by weight of polyacrylate resin, 10-25 parts by weight of hydroxypropyl methacrylate, 25-55 parts by weight of trifluoroethyl methacrylate reactive monomer diluent, 25-55 parts by weight of octadecyl methacrylate reactive monomer diluent, and 1-5 parts by weight of 2-hydroxy-2-methyl-1-phenyl-1-propanone as an initiator. This prior art UV-curable release agent is a silicone-free UV-curable release agent, requiring no high-temperature baking, and preventing silicone oil seepage, thus eliminating the phenomenon of PAS adhesive being pulled up due to silicone oil transfer.
[0005] The release films of the aforementioned prior art are usually colorless and transparent, making it sometimes difficult to determine whether a release film has been applied to a product.
[0006] CN 219544202 U discloses a blue PE double-sided release film, comprising a nanoscale carbon sponge layer and blue PE films disposed on both sides of the nanoscale carbon sponge layer. A transparent film is disposed on the side of the blue PE films facing away from the nanoscale carbon sponge layer, and a corona layer is disposed on the side of the transparent film facing away from the blue PE films. A release layer is disposed on the corona layer, and the release layer is a UV-curable nano-mixture coated on the corona layer. This prior art release film uses a blue PE film as its substrate, which facilitates identification by color.
[0007] Blue PE film is almost the most common type of film in the film industry. Because PE is easily oxidized and turns blue, to keep PE film colorless, antioxidants need to be added to slow down oxidation. Therefore, colorless PE film is usually more expensive than blue film. In short, the common perception is that blue PE film is of lower quality than colorless film.
[0008] Apart from blue PE film, other types of films are typically colorless. Therefore, to prepare colored release films, pigments are usually added to the base film to give it different colors. For example, commercially available colored release films are usually made from base films of various colors such as yellow, red, green, blue, and gray.
[0009] In the field of electronic product technology, adhesive bonding is becoming increasingly common, and it is also common to adhere different colored release films to the adhesive layer to distinguish different surfaces. For example, CN 116023866 A discloses a highly weather-resistant ultra-thin adhesive film that is easy to apply, comprising a blue release film, AB adhesive, and a transparent release film arranged sequentially from top to bottom, wherein both opposite sides of the AB adhesive are adhesive. The blue release film used in this prior art is easy to remove quickly during later use.
[0010] As mentioned above, existing release films are generally colorless, while colored release films derive their color from dyeing the release film substrate. However, since the release agent on the surface of the release film substrate is generally colorless, it is difficult to determine whether any release agent residue remains after the colored release film is removed.
[0011] For example, CN 113155822 A discloses a method for testing the anti-fogging performance of silicone release agents, including weighing the sample to be tested, covering it with paper, stirring the sample, curing the release agent, dyeing the cover paper, and comparing the dyed sample with a standard sample to obtain the anti-fogging performance result of the test sample. The cover paper used in this prior art is made of plant fiber, and the dyes selected are those that can color fibers, such as Shirlastain A fiber identification agent or malachite green dye. The working principle of this prior art is that under suitable stirring conditions, the silicone release agent forms an aerosol that overflows from the liquid surface and is adsorbed onto the cover paper of the stirring container. The cover paper with the cured release agent is then dyed. Because the silicone release agent and paper fibers show different colors when they come into contact with the dye, the amount of release agent on the cover paper reflects the anti-fogging performance of the measured sample.
[0012] As can be seen from the existing technology, release agents are difficult to observe and distinguish in a visual way. They require additional complex processes and pre-testing. Even if a release agent that meets the quality requirements can be obtained, the residue of the release agent is still difficult to identify in actual use, and quality control can only be achieved through testing. Summary of the Invention
[0013] The technical problem to be solved by this application is to provide a colored release film and a method for preparing the same, so as to reduce or avoid the problems mentioned above.
[0014] To address the aforementioned technical problems, this application proposes a colored release film, comprising a substrate layer and a release agent layer. The substrate layer is made of a single-layer or multi-layer transparent polyester film, and the release agent layer is prepared from a colored release agent containing modified pigments. The colored release agent is prepared from the following components in parts by weight: 100-200 parts by weight of polyurethane acrylate, 60-80 parts by weight of hexaethoxylated trimethylolpropane triacrylate, 20-40 parts by weight of diacetone alcohol, 30-50 parts by weight of tridecylfluorooctyl acrylate, 2.5-4.5 parts by weight of a mixture of solid particles of modified pigments, and 3-5 parts by weight of benzophenone.
[0015] Preferably, the modified pigment is an alkali-resistant inorganic pigment that has undergone surface modification treatment.
[0016] Preferably, the inorganic pigment is one of iron oxide red, cadmium sulfide, ultramarine, or a mixture thereof.
[0017] This application also proposes a method for preparing a colored release film, comprising the following steps: uniformly mixing 100-200 parts by weight of polyurethane acrylate, 60-80 parts by weight of hexaethoxylated trimethylolpropane triacrylate, 20-40 parts by weight of diacetone alcohol, 30-50 parts by weight of tridecylfluorooctyl acrylate, and 2.5-4.5 parts by weight of a solid particle mixture of surface-modified pigments; adding 3-5 parts by weight of benzophenone; magnetically stirring for 120-240 seconds to obtain a release agent; uniformly coating the release agent onto the surface of a substrate layer with a thickness of 12-100 μm; vacuum defoaming for 1-2 hours; curing under N2 conditions with ultraviolet light irradiation for 180-300 seconds to form a release agent layer; and measuring the thickness of the release agent layer to be 0.5-2 μm.
[0018] Preferably, the preparation method further includes a surface modification treatment step for the modified pigment: adding 10-20 parts by weight of inorganic pigment to 100-200 parts by weight of polyvinyl alcohol aqueous solution, stirring continuously for 60-120 minutes to fully disperse; then adding 6-8 parts by weight of sodium tripolyphosphate and stirring for another 60-120 minutes to fully mix and obtain a dispersion mixture; finally, lyophilizing the dispersion mixture to obtain a solid particle mixture of surface-modified pigment.
[0019] The colored release film of this application allows the colored release agent layer to be observed from the outside through the transparent substrate layer, thus enabling visual perception of the color. Furthermore, release agent residue or fogging can be observed with the human eye, allowing for a direct assessment of the release film's quality. Real-time monitoring and timely correction of residual defects are also possible. Detailed Implementation
[0020] To provide a clearer understanding of the technical features, objectives, and effects of this application, the specific implementation methods of this application will be described in detail below.
[0021] In view of the technical problems described in the background art, this application proposes a colored release film, comprising a substrate layer and a release agent layer, wherein the substrate layer is made of a single-layer or multi-layer transparent polyester film, and the release agent layer is prepared by adding a colored release agent with modified pigments.
[0022] Using a transparent substrate layer allows the colored release agent layer to be easily observed from the outside, thus enabling a visual perception of the color. If the substrate layer is opaque, the color cannot be seen, and there is no such thing as a colored release film. Furthermore, using a colored release agent allows for the visual observation of release agent residue or fogging, eliminating the need for complex pre-testing to directly assess the quality of the release film. This enables real-time monitoring and timely correction of residue issues, significantly aiding in real-time product quality control.
[0023] In one specific embodiment of this application, the thickness of the substrate layer is 12-100µm, and the thickness of the release agent layer is 0.5-2µm.
[0024] In another specific embodiment of this application, the colored release agent is prepared from the following components in parts by weight: 100-200 parts by weight of polyurethane acrylate, 60-80 parts by weight of hexaethoxylated trimethylolpropane triacrylate, 20-40 parts by weight of diacetone alcohol, 30-50 parts by weight of tridecylfluorooctyl acrylate, 2.5-4.5 parts by weight of a mixture of solid particles of modified pigment, and 3-5 parts by weight of benzophenone.
[0025] The modified pigment is preferably a surface-modified inorganic pigment, such as one or a mixture of alkali-resistant inorganic pigments like iron oxide red, cadmium sulfide, and ultramarine. Although inorganic pigments are not as vibrant in color as organic pigments, they are inexpensive and readily available. Furthermore, inorganic pigments are easier to disperse and retain their original color after surface modification. Additionally, alkali-resistant inorganic pigments are less prone to discoloration after oxidation, making it easier to identify whether the release film has peeled off or deteriorated.
[0026] Further, the surface modification treatment step of the modified pigment includes: adding 10-20 parts by weight of inorganic pigment to 100-200 parts by weight of polyvinyl alcohol aqueous solution, and stirring continuously for 60-120 minutes to fully disperse; then adding 6-8 parts by weight of sodium tripolyphosphate and stirring for another 60-120 minutes to fully mix and obtain a dispersion mixture; finally, lyophilizing the dispersion mixture to obtain a solid particle mixture of the surface-modified pigment. The polyvinyl alcohol content in the polyvinyl alcohol aqueous solution is 10 wt%-15 wt%.
[0027] Example 1
[0028] 100 parts by weight of polyurethane acrylate, 60 parts by weight of hexaethoxylated trimethylolpropane triacrylate, 20 parts by weight of diacetone alcohol, 30 parts by weight of tridecafluorooctyl acrylate, and 2.5 parts by weight of a surface-modified solid particle mixture (iron oxide red) were uniformly mixed. 3 parts by weight of benzophenone were added, and the mixture was magnetically stirred for 120 seconds to obtain a release agent. The release agent was uniformly coated onto the surface of a 12 μm thick substrate layer, defoamed under vacuum for 1 hour, and cured under N2 conditions with ultraviolet light for 180 seconds to form a release agent layer. The thickness of the release agent layer was measured to be 0.5 μm.
[0029] Comparative Example 1
[0030] The release film was prepared using the same process as in Example 1, except that hexaethoxylated trimethylolpropane triacrylate was removed from the release agent components, and the contents of other components were adjusted. Specifically, the components were: 140 parts by weight of polyurethane acrylate, 20 parts by weight of diacetone alcohol, 50 parts by weight of tridecylfluorooctyl acrylate, 2.5 parts by weight of a modified pigment solid particle mixture (iron oxide red), and 3 parts by weight of benzophenone.
[0031] Example 2
[0032] 150 parts by weight of polyurethane acrylate, 70 parts by weight of hexaethoxylated trimethylolpropane triacrylate, 30 parts by weight of diacetone alcohol, 40 parts by weight of tridecafluorooctyl acrylate, and 3.0 parts by weight of a surface-modified solid particle mixture (cadmium sulfide) were uniformly mixed, and 4 parts by weight of benzophenone were added. The mixture was magnetically stirred for 180 seconds to obtain a release agent. The release agent was uniformly coated onto the surface of a substrate layer with a thickness of 50 μm, defoamed under vacuum for 1.5 hours, and cured under ultraviolet light under N2 conditions for 240 seconds to form a release agent layer. The thickness of the release agent layer was measured to be 1 μm.
[0033] Comparative Example 2
[0034] The release film was prepared using the same process as in Example 2, except that diacetone alcohol was removed from the release agent components, and the contents of other components were adjusted. Specifically, the components were: 170 parts by weight of polyurethane acrylate, 80 parts by weight of hexaethoxylated trimethylolpropane triacrylate, 40 parts by weight of tridecafluorooctyl acrylate, and 3.0 parts by weight of a surface-modified solid particle mixture (cadmium sulfide), all uniformly mixed, with 4 parts by weight of benzophenone added.
[0035] Example 3
[0036] 200 parts by weight of polyurethane acrylate, 80 parts by weight of hexaethoxylated trimethylolpropane triacrylate, 40 parts by weight of diacetone alcohol, 50 parts by weight of tridecafluorooctyl acrylate, and 4.5 parts by weight of a surface-modified solid particle mixture (ultramarine) were uniformly mixed. 5 parts by weight of benzophenone were added, and the mixture was magnetically stirred for 240 seconds to obtain a release agent. The release agent was uniformly coated onto the surface of a 100 μm thick substrate layer, defoamed under vacuum for 2 hours, and cured under N2 conditions with ultraviolet light for 300 seconds to form a release agent layer. The thickness of the release agent layer was measured to be 2 μm.
[0037] Comparative Example 3
[0038] The release film was prepared using the same process as in Example 3, except that tridecylfluorooctyl acrylate was removed from the release agent components, and the contents of other components were adjusted. Specifically, the components were: 230 parts by weight of polyurethane acrylate, 90 parts by weight of hexaethoxylated trimethylolpropane triacrylate, 50 parts by weight of diacetone alcohol, and 4.5 parts by weight of a surface-modified solid particle mixture (ultramarine), all uniformly mixed, with 5 parts by weight of benzophenone added.
[0039] The parameter performance of the above embodiments and comparative examples is shown in the table below.
[0040] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Release force g / 25mm 8.6 7.3 8.1 3.5 2.3 0.5 Adhesion rating 0 1 0 3 3 8 Delamination temperature >350℃ >350℃ >350℃ <160℃ <180℃ <250℃ stable temperature ≤150℃ ≤150℃ ≤150℃ ≤120℃ ≤130℃ ≤160℃ <![CDATA[Stain density count / 10cm 2 > <0.1 <0.1 <0.1 3 5 8
[0041] Examples 4-6 and Comparative Examples 4-6
[0042] The components of the modified pigments in Examples 1-3 were adjusted and their performance was tested. The component weight parts of the modified pigments in Examples 4-6 and Comparative Examples 4-6 are shown in the table below.
[0043] Example 4 Example 5 Example 6 Comparative Example 4 Comparative Example 5 Comparative Example 6 Inorganic pigment solid particle mixture (main component) parts by weight Iron oxide red 10 Cadmium sulfide 15 Ultramarine 20 Iron oxide red 10 Cadmium sulfide 15 Ultramarine 20 Polyvinyl alcohol aqueous solution (concentration) 10010 wt% 15012 wt% 20015 wt% 0 15012 wt% 8010 wt% Sodium tripolyphosphate 6 7 8 6 0 5
[0044] Comparative Example 4 did not use an aqueous solution of polyvinyl alcohol, therefore it could not be prepared by dispersion spraying; instead, iron oxide red and sodium tripolyphosphate were thoroughly mixed into a solid particle mixture. Comparative Example 5 did not add sodium tripolyphosphate, and Comparative Example 6 reduced the amount of polyvinyl alcohol and sodium tripolyphosphate used. The particle size of the inorganic pigment was selected to be 10-15 nm.
[0045] A mixture of solid particles was prepared using the aforementioned modification process and applied to the release films of Examples 1-3, respectively. Specifically, Examples 4 and Comparative Example 4 were used for the release film of Example 1, Examples 5 and Comparative Example 5 were used for the release film of Example 2, and Examples 6 and Comparative Example 6 were used for the release film of Example 3.
[0046] The color distribution uniformity of the release films of Examples 4-6 and Comparative Examples 4-6 were tested respectively, and the index was the average density of color spots per 10 square centimeters (number of spots / 10cm). 2 The values for Examples 4-6 were all less than 0.1, while the values for Comparative Examples 4-6 were 8.6, 5.4, and 2.3, respectively. The pigment dispersion in Comparative Example 4 was poor, with significant agglomeration. The colors of Comparative Examples 5 and 6 were significantly paler than those of Examples 5 and 6, with Comparative Example 5 being almost colorless, the reason for which is unknown.
[0047] Those skilled in the art should understand that although this application is described by way of multiple embodiments, not every embodiment contains only one independent technical solution. This description is merely for clarity, and those skilled in the art should understand the specification as a whole and consider the technical solutions involved in each embodiment as being able to be combined with each other to form different embodiments to understand the scope of protection of this application.
[0048] The above description is merely an illustrative embodiment of this application and is not intended to limit the scope of this application. Any equivalent changes, modifications, and combinations made by those skilled in the art without departing from the concept and principles of this application shall fall within the scope of protection of this application.
Claims
1. A colored release film, comprising a substrate layer and a release agent layer, characterized in that, The substrate layer is made of a single-layer or multi-layer transparent polyester film. The release agent layer is prepared from a colored release agent with modified pigments. The colored release agent is prepared from the following components in parts by weight: 100-200 parts by weight of polyurethane acrylate, 60-80 parts by weight of hexaethoxylated trimethylolpropane triacrylate, 20-40 parts by weight of diacetone alcohol, 30-50 parts by weight of tridecylfluorooctyl acrylate, 2.5-4.5 parts by weight of a mixture of solid particles of modified pigments, and 3-5 parts by weight of benzophenone. The modified pigment is an alkali-resistant inorganic pigment that has undergone surface modification treatment. The inorganic pigment is iron oxide red and sulfurized... The inorganic pigment is one of cadmium, ultramarine, or a mixture thereof, with a particle size of 10-15 nm. The solid particle mixture of the modified pigment is prepared by a surface modification treatment comprising the following steps: adding 10-20 parts by weight of the inorganic pigment to 100-200 parts by weight of a polyvinyl alcohol aqueous solution, wherein the polyvinyl alcohol content in the polyvinyl alcohol aqueous solution is 10-15 wt%, and stirring continuously for 60-120 minutes to fully disperse; then adding 6-8 parts by weight of sodium tripolyphosphate and stirring for another 60-120 minutes to fully mix to obtain a dispersed mixture; finally, the dispersed mixture is subjected to lyophilized spray to obtain a solid particle mixture of the surface-modified pigment.
2. A method for preparing the colored release film as described in claim 1, comprising the following steps: uniformly mixing 100-200 parts by weight of polyurethane acrylate, 60-80 parts by weight of hexaethoxylated trimethylolpropane triacrylate, 20-40 parts by weight of diacetone alcohol, 30-50 parts by weight of tridecylfluorooctyl acrylate, and 2.5-4.5 parts by weight of a surface-modified pigment solid particle mixture; adding 3-5 parts by weight of benzophenone; magnetically stirring for 120-240 seconds to obtain a release agent; uniformly coating the release agent onto the surface of a substrate layer with a thickness of 12-100 μm; vacuum defoaming for 1-2 hours; curing under N2 conditions with ultraviolet light irradiation for 180-300 seconds to form a release agent layer; and measuring the thickness of the release agent layer to be 0.5-2 μm.
Citation Information
Patent Citations
A release film substrate
CN112375437B
A release film for polarizers
CN112661995B
Method for testing anti-fogging performance of organic silicon release agent
CN113155822A
Antibacterial release film with small release force
CN106243371A
Preparation method of color powdered ink
CN109946932A